Solder, laser welding joint and manufacturing method thereof

By adding Fe, Mn, and Ni solder to the molten pool during the welding process, the problem of joint performance degradation caused by aluminum plating entering the weld is solved, a high-strength, high-toughness laser welded joint is achieved, and the cost of welding materials and process complexity to ensure the stability and reliability of weld performance.

CN118357579BActive Publication Date: 2024-10-22SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410790034.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

When manufacturing laser welded blanks with surfaces coated with aluminum or aluminum alloys, the aluminum coating enters the weld, resulting in a decrease in joint performance. Existing technology is difficult to effectively suppress the formation of ferrite, resulting in a weakened load-bearing capacity of the welded joint and an increased risk of failure. , and the commonly used welding wire alloy element ratios are complex and costly.

Method used

By transitionally adding solder composed of Fe, Mn, and Ni into the molten pool during the welding process, it is ensured that the volume fraction of martensite in the weld is not less than 90%, the Mn element content is not less than 3.2%, and the Al element content is not less than 1.4%. The C element content is lower than that of the steel plate base material. Welding wire with high Mn and low Ni is used to suppress the formation of ferrite and carbides and improve the mechanical properties and stability of the welded joint.

Benefits of technology

It achieves high performance and stability of welded joints, reduces the cost of welding materials and process complexity, ensures that welds have high reliability and excellent fracture strength and elongation under different assembly gaps, and avoids ferrite and carbonization adverse effects of things.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118357579B_ABST
    Figure CN118357579B_ABST
Patent Text Reader

Abstract

The present invention provides a solder, a laser welding joint and a manufacturing method thereof, which can ensure that the aluminum-coated steel plate has excellent joint strength and toughness after hot forming and quenching of butt welding. A laser welding joint, when two steel plate base materials are butt-welded for laser welding, laser welding solder is added to the molten pool to form an initial weld, and the initial weld is formed after quenching to form the laser welding joint, wherein at least one steel plate is a steel plate with an aluminum coating or an aluminum alloy coating, characterized in that the internal lath martensite volume fraction of the laser welding joint is not less than 90%, the average mass fraction of the Mn element is not less than 3.2%, the average mass fraction of the Al element is not higher than 1.4%, and the average mass fraction of the C element is lower than the C content of the steel plate base material, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint do not exceed 0.4mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the manufacture of high-strength steel coated plate welding parts, in particular to a solder, a laser welding joint and a manufacturing method thereof. Background Art

[0002] In some fields, especially in the manufacture of automobile and aerospace parts, the use of materials requires high corrosion resistance, so more and more materials with coatings on the surface are used. Since the steel with aluminum or aluminum alloy coated on the surface manufactured by cold rolling or hot rolling not only has good corrosion resistance, but also has high high temperature resistance, which is conducive to the manufacture of certain parts by hot processing, the steel plate with aluminum alloy coated on the surface is especially used in the manufacture of automobile bodies, and is used in automobile structural parts, such as door reinforcements, B-pillar structural parts, roof reinforcements and other parts, especially in the application of ultra-high strength hot stamping plates, so as to achieve high corrosion resistance, reduce the weight of the automobile body, and improve collision absorption energy.

[0003] In the automotive manufacturing industry, in order to reduce vehicle weight and achieve lightweight goals, more and more materials of equal thickness, unequal thickness, homogeneous and heterogeneous quality are first welded, and then the welded parts are hot stamped to achieve better weight reduction and cost reduction. The laser welding method is the preferred method of this approach, with higher quality, higher efficiency and better flexibility, and is called "laser welded blanks". High-strength fully martensitic steel structural parts are often obtained by first laser butt welding the flat workpiece and then hot stamping and quenching the workpiece with the weld. When hot stamping, the weld structure is first heated to a temperature exceeding the AC3 temperature of the steel workpiece for complete austenitization. Due to the high temperature, the bare plate will inevitably oxidize and decarburize the surface, resulting in a decrease in the final structural performance; so it is also necessary to coat the surface, and aluminum or aluminum alloy coatings are widely used in this process; documents represented by patent CN101583486B describe this type of material in detail.

[0004] However, there are great difficulties in manufacturing laser welded plates with aluminum or aluminum alloy coating on the surface. When the welding surface is coated with aluminum or aluminum alloy, the coating on the surface will enter the melting area, especially the melting area of ​​the weld, which will cause the formation of high-temperature ferrite structure during cooling. Even after cooling and high-temperature austenitization, it will remain in the final weld and cause the joint formation to decrease. Under the action of subsequent mechanical loads, these large amounts of ferrite will become the initial position of failure cracks, seriously weakening the bearing capacity of the welded joint and directly breaking in the weld when loaded. Therefore, it is very necessary to suppress the degradation of joint performance caused by aluminum entering the weld.

[0005] Patents CN101426612B, 106334875A, etc. use mechanical methods, laser methods or other methods to remove the surface coating in advance to prevent it from entering the weld, but this method has problems such as high cost and complex process.

[0006] Patent CN106392328B discloses a method for welding aluminum-silicon coated hot-formed steel under protective gas conditions. This patent uses oxidizing gas to combine with the aluminum element in the coating during the welding process to produce aluminum oxide, which has no effect on the toughness of the weld. However, in this solution, the time for the metal to melt to form a molten pool and then solidify into a weld is very short during the welding process. The reaction time of the oxidizing gas and the aluminum element is limited. Once the aluminum element that has not reacted with the oxidizing gas enters the molten pool, aluminum accumulation will be generated inside the molten pool, reducing the toughness and strength of the weld, and there is a risk of cracking of the hot stamping parts.

[0007] Patent CN 106488824 B discloses a method for joining two blanks by welding with a filler wire, the welding wire being made of a stainless steel alloy comprising the following weight percentages: 0%-0.3% carbon, 0%-1.3% silicon, 0.5%-7% manganese, 5%-22% chromium, 6%-20% nickel, 0%-0.4% molybdenum, 0%-0.7% niobium and the remainder of iron and unavoidable impurities. In this method, when laser and arc welding are mixed, the heat input increases, the probability of thermal deformation of the plate increases, and it is not conducive to the splicing of thin plates. Moreover, the welding speed of laser and arc welding mixed welding is limited, which reduces production efficiency.

[0008] CN 111432975 A discloses a welding wire filled with the following weight percentages: 0.03% carbon, 0.5% silicon, 1.8% manganese, 20.5% chromium, 25% nickel, 4.7% molybdenum, less than 0.05% sulfur, less than 0.05% phosphorus, and 1.6% copper. When the welding wire is used as a filling material, a high content of Cr will lead to the risk of ferrite formation in the weld zone of the tailor-welded blank after hot stamping, resulting in a decrease in the mechanical properties of the welded joint, the inability to guarantee the quality of the product, and a high risk of failure of the welded joint. CN 112368105 A discloses a method for laser welding a coated steel blank using a filler wire, wherein the welding wire includes nickel, chromium, and carbon elements, which are 1.68-10.48%, 0-2.70%, and 0.91-2.00% by weight, respectively. The high carbon content of the welding wire will lead to an excessively high carbon content in the tailored weld zone, which will reduce the plasticity and impact properties. The excessively high carbon content will make the weld prone to cracking, and will also reduce the corrosion resistance of the weld and the service life of the tailored weld. In addition, the welding wire has a high content of C element, which is very difficult to produce during the drawing process of the welding wire, and is very easy to be hardened and break the welding wire.

[0009] CN 108025400 A discloses a laser welding method for semi-finished plates of hardenable steel with aluminum-based or aluminum-silicon-based coatings. The method uses a filler electrode to heat the electrode with another heat source before the base material melts and then transfers it to the molten weld to achieve the regulation of weld performance. The second heat source is required in the whole process. At the same time, the weld width needs to be controlled to be at least 0.15 mm, and the amount of electrode melted needs to be controlled to account for more than 20% of the material. A large amount of solder is required, and multiple control processes are relatively complicated. The external heat source also makes the entire process cost high. In this method, a filler containing a weight percentage of 0.5 to 2.0 of the sum of Cr and Mo and a weight percentage of 1 to 4 of Ni is filled. The addition of Mo and Cr easily leads to the precipitation of carbides in the weld and increases the brittleness of the joint, making the performance unstable.

[0010] CN 104994989 A discloses a welding wire filled with the following weight percentages: 0.05-0.15% carbon, 0.5-2.0% silicon, 1.0-2.5% manganese, 0.5-2.0 chromium and molybdenum, 1.0-4.0% nickel, and the balance of iron and inevitable impurities. The welding wire contains relatively low chromium and molybdenum elements, and the hardenability and corrosion resistance of the welded joint obtained by using the welding wire as a filler wire are poor, and it is impossible to ensure that the influence of ferrite is completely suppressed during high-temperature heat treatment, which increases the failure risk of the welded joint in the weld and heat-affected zone.

[0011] CN104023899B discloses a laser welding method for filling welding wires for plates of unequal thickness or unequal strength, wherein no ferrite structure is produced at 900-950°C, wherein the filling welding wire is mainly composed of carbon or manganese, wherein the carbon content of the filling welding wire is 0.1wt% to 0.8wt% higher than the carbon content of the base material of the coated steel plate, and the manganese content of the filling welding wire is 1.5wt% to 7.0wt% higher than the manganese content of the base material of the coated steel plate. People in the field are aware that the Mn content of hot-formed steel is between 1.0-2.5, that is, the Mn content of the welding wire is between 2.5% and 9.5%; relying solely on carbon or manganese elements to achieve austenitization of the weld is very likely to cause Mn segregation or high C content and brittleness. At the same time, the density of the C element is low, and a large volume of welding wire needs to be added to achieve an improvement in the quality of the C element in the final weld compared to the base material; and the Mn element has poor austenitization ability compared to the Ni element, so a large amount of welding wire needs to be added, which will lead to a decrease in welding speed and an increase in wire feeding speed; welding efficiency and welding material consumption are increased, and manufacturing costs are increased.

[0012] CN 112548395 A discloses a welding wire for laser wire-filling welding, a preparation method and a tailor-welded plate process. This method fills a welding wire with a high carbon content. The carbon content in the welding wire is about 2.5 to 10 times that of the welding base material, resulting in an excessively high carbon content in the tailor-welded area, which reduces the plasticity and impact properties. In addition, an excessively high carbon content will make the weld prone to cracks, and will also reduce the corrosion resistance of the weld and the service life of the tailor-welded plate.

[0013] A welding method for coated steel plates is disclosed in US 20210008665 A1. The weight percentage of the carbon content of the welding wire is 0.80 to 2.28 times the carbon content of the base material. Excessive carbon content will make the weld prone to cracking and hardening and brittleness, and will also reduce the corrosion resistance of the weld and the service life of the welded plate, resulting in poor mechanical properties of the welded joint, reducing product quality, and is not suitable for mass production.

[0014] At present, the welding wire for laser welding of coated steel blanks usually needs to be matched with special laser processes or equipment to improve the welding quality of steel plates. In addition, the types of welding wires added are mainly composed of various alloy elements, including C, Cr, Ni, Mo, Mn, Si and other alloy elements. On the one hand, this type of welding wire is difficult to fully ensure that the weldment has stable and excellent mechanical properties and corrosion properties after welding. At the same time, due to the addition of various alloy elements, it is very easy to produce work hardening during the drawing and forming stage of the welding wire, which makes the welding wire yield low and the manufacturing difficulty is relatively large; at the same time, the complex ratio of various alloy elements is difficult to effectively control during the process, which is very likely to cause the final weld performance to be unqualified. The more expensive Mo element also makes the manufacturing cost higher. In addition, another study by the applicant uses the Ni element to expand the austenite interval of the weld to inhibit the formation of ferrite, but the Ni element is an expensive strategic metal with a high cost of use. Therefore, a relatively low-cost way is needed to achieve high-efficiency laser welding of surface coated plates while ensuring high-strength and high-toughness laser welded joints. Summary of the invention

[0015] The present invention provides a solder, a high-performance laser welding joint and a manufacturing method. Without removing the aluminum coating on the surface, a solder composed of Fe, Mn and Ni is added to the molten pool during the welding process to finally obtain a high-performance laser welding joint. The volume fraction of the internal lath martensite of the laser welding joint is not less than 90%, the average mass fraction of the Mn element is not less than 3.2%, the average mass fraction of the Al element is not higher than 1.4%, and the average mass fraction of the C element is lower than the C content of the steel plate base material. The final weld front side excess h1 and the final weld back side excess h2 formed by the laser welding joint do not exceed 0.4 mm, which greatly improves the mechanical properties and stability of the weldment. This method can greatly reduce the addition of other alloying elements by adding welding materials mainly composed of Fe, Mn and Ni to the molten pool during the welding process; in the manufacture of welding materials, since Mn can infinitely dissolve in austenite to replace Ni elements, the austenitization interval is expanded, the formation of high-temperature ferrite is inhibited, and the welding joint has excellent performance, so on the one hand, the cost of welding materials can be reduced; in addition, the saving of other alloying elements also reduces the complexity of the proportion of welding materials and the difficulty of process control in the manufacturing process. The present invention mainly adds Fe, Mn and Ni elements, without additional large amounts of alloying elements, which can reduce the formation of coarse carbides in the final weld, and the carbon-manganese compounds formed can be greatly dissolved in the subsequent austenitization process, reducing the adverse effects of Mn segregation, and finally improving the mechanical properties of the joint; at the same time, the addition of welding materials with high Mn content can ensure the removal of ferrite in the final weld, retaining the weld structure with more than 90% of martensite, and ensuring the performance of the weld. However, in the actual welding process, there is often an uncertain assembly gap. When adding solders with other alloy elements, it is often easy to cause incomplete matching and poor solder adaptability. The solder and method of the present invention can ensure that a highly reliable and stable weld is formed under different assembly gaps, and has excellent fracture strength and elongation. A significant reduction in manufacturing costs is achieved by replacing Ni with Mn. The overall idea is to use high-Mn, low-Ni welding wire to rely on the preferential solubility of Mn and Ni to suppress the formation of brittle phases (including ferrite and highly brittle carbides) in the weld, and to synergistically improve the strength and toughness of the joint through solid solution strengthening of Mn and Ni, so as to achieve a significant improvement in the performance of the entire joint.

[0016] The following solutions are provided:

[0017] In a first aspect, the present invention provides a laser welding solder for forming a laser welding joint, wherein the solder is composed of Fe, Mn, Ni, trace alloying elements and other inevitable elements, wherein, in weight percentage, the following conditions are satisfied: Mn ≥ 15%, 1.5% ≤ Ni ≤ 5%, trace alloying elements 0 ~ 0.36%, and other inevitable elements ≤ 2%; the trace alloying elements are at least one of Nb, V, and Ti elements, and the contents of Nb, V, and Ti elements do not exceed 0.12%.

[0018] In the second aspect, the present invention provides a laser welded joint, when two steel plate base materials are butt-jointed for laser welding, the laser welding solder described in the first aspect is added to the molten pool to form an initial weld, and the initial weld is quenched to form the laser welded joint, wherein at least one steel plate is a steel plate with an aluminum coating or an aluminum alloy coating, the internal lath martensite volume fraction of the laser welded joint is not less than 90%, the average mass fraction of the Mn element is not less than 3.2%, the average mass fraction of the Al element is not higher than 1.4%, and the average mass fraction of the C element is lower than the C content of the steel plate base material, and the final weld front side reinforcement h1 and the final weld back side reinforcement h2 formed by the laser welded joint do not exceed 0.4mm. Preferably, the average mass fraction of the Mn element is 3.2% to 5.2%.

[0019] Preferably, the volume fraction of lath martensite is not less than 92%.

[0020] Furthermore, the specific steps of quenching are: keeping the initial weld at 880-980°C for 90-500s, and then achieving rapid cooling through a mold with rapid cooling or a liquid medium, with a cooling rate of ≥25°C / s.

[0021] Furthermore, the rapid cooling method is flat die stamping cooling, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint meet , where t1 is the thickness of the first steel plate and t2 is the thickness of the second steel plate.

[0022] Furthermore, the rapid cooling method is water-cooling quenching, and the initial weld front side excess height h10 and the initial weld back side excess height h11 meet , where t1 is the thickness of the first steel plate, t2 is the thickness of the second steel plate, B10 is the initial weld upper surface width, and B11 is the initial weld lower surface width.

[0023] In a third aspect, the present invention provides a method for manufacturing a laser welded joint, the method comprising the following steps:

[0024] Step 1: provide two steel plate base materials, at least one of which is a steel plate with an aluminum coating or an aluminum alloy coating, and butt the two steel plates;

[0025] Step 2: laser welding the butt-jointed steel plates, wherein the solder described in the first aspect is added to the molten pool during the welding process to form an initial weld;

[0026] Step 3: quenching and cooling the initial weld to obtain the laser welded joint described in the second aspect;

[0027] Step 2 During the laser welding process, the melting volume of the two steel plates is V1, and the volume of the solder in the molten pool is V2. V1 and V2 satisfy .

[0028] In a fourth aspect, the present invention provides a high-strength steel workpiece, which is composed of two steel plate mother materials and a laser welding joint for connecting the mother materials; when the high-strength steel workpiece is subjected to a tensile test, it breaks and fails in the mother material area.

[0029] In a fifth aspect, the present invention provides a component containing the above-mentioned laser welded joint, which is used in a structural component or a safety component of a mechanized land vehicle. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 Shown is a schematic diagram of a cross section of a typical laser welded joint of the present invention;

[0032] Figure 2 Shown is a cross-sectional schematic diagram of the steel plate base material involved in the present invention;

[0033] Figure 3 Shown is a schematic diagram of the main steps of the laser welding joint manufacturing process involved in the present invention;

[0034] Figure 4 It is a schematic diagram of the steel plates involved in the present invention when they are butt-jointed;

[0035] Figure 5 Shown is a schematic diagram of the laser welding process involved in the present invention;

[0036] Figure 6 Shown is a schematic top view of the laser welding process involved in the present invention;

[0037] Figure 7Shown is a cross-sectional schematic diagram of the initial weld obtained in the present invention;

[0038] Figure 8 Another schematic cross-sectional view of the initial weld obtained in the present invention is shown;

[0039] Fig. 9 Shown is another cross-sectional schematic diagram of the initial weld obtained in the present invention;

[0040] Fig.10 Shown is another cross-sectional schematic diagram of the initial weld obtained in the present invention;

[0041] Fig.11 The figure shows the metallographic cross section of the initial weld obtained in a specific embodiment involved in the present invention;

[0042] Fig.12 The present invention is shown as follows Fig.11 A cross-sectional view of the final weld after quenching and cooling of the initial weld in the embodiment.

[0043] Fig.13 The present invention is shown as follows Fig.12 The state of the welded joint obtained in the embodiment after tensile failure;

[0044] Fig.14 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;

[0045] Fig.15 The present invention is shown as follows Fig.14 The state of the welded joint obtained in the embodiment after tensile failure;

[0046] Fig.16 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;

[0047] Fig.17 The present invention is shown as follows Fig.16 The state of the welded joint obtained in the embodiment after tensile failure;

[0048] Fig.18 The figure shows the metallographic cross section of the final weld obtained in a specific embodiment involved in the present invention;

[0049] Fig.19 The present invention is shown as follows Fig.18 The state of the welded joint obtained in the embodiment after tensile failure. DETAILED DESCRIPTION

[0050] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, the accompanying drawings are schematic diagrams, so the device and equipment of the present invention are not limited by the size or ratio of the schematic diagrams.

[0051] It should be noted that in the claims and description of this patent, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "including one" do not exclude the existence of other identical elements in the process, method, article or device including the elements. The final weld in the present invention refers to the laser welded joint. The present invention provides a solder for laser welding of steel plates with aluminum coating or aluminum alloy coating, wherein the solder is composed of Fe, Mn, Ni, trace alloying elements and inevitable impurities, wherein, by weight percentage, the following conditions are satisfied: Mn ≥ 15%, 1.5% ≤ Ni ≤ 5%, trace alloying elements 0-0.36%, and inevitable impurities ≤ 2%; the trace alloying elements are at least one of Nb, V, and Ti elements, and the contents of Nb, V, and Ti elements are all less than 0.12%. Except for Fe, Mn, and Ni, other elements in the solder are not necessary. A higher total Mn content can ensure that the joint has a minimum ferrite content after welding, thereby ensuring the joint performance. The solder can be in various forms such as filaments, powders, or sheets; for example, solid welding wire or flux-cored welding wire, when in the form of welding wire, the diameter is generally 0.6-2.0 mm, preferably 0.8-1.2 mm.

[0052] Reference now Figure 1The figure shows a laser welded joint 2 involved in the present invention, which is formed by butting two steel plate base materials (first steel plate 11, second steel plate 12) and performing laser welding. At least one of the first steel plate 11 and the second steel plate 12 has an aluminum coating on one surface. The joint has the following characteristics when observed along the cross section of the weld: the joint 2 is composed of lath martensite 21 with a volume fraction of not less than 90%, and the austenite structure 22 contained does not exceed 10%; preferably, the lath martensite accounts for not less than 92%; in a preferred example, the martensite content in the weld exceeds 95%, and the more extreme one can be composed of all lath martensite. In addition, trace carbide components other than lath martensite and austenite may also exist in the final weld. The distribution and size of the residual austenite in the weld can have various forms, and the presence of a trace amount of austenite structure in the weld can ensure that the TRIP effect occurs during the load-bearing process of the weld to transform the austenite into the martensite structure, so that the weld provides additional plasticity and ensures sufficient strength. The average mass fraction of the Mn element inside the joint 2 is not less than 3.2%; the Mn and Ni elements are mainly present in the weld in the form of solid solution. And the average mass fraction of the Al element is not higher than 1.4%; the average mass fraction of the C element is lower than the C content of the original steel plate parent material. The weld may also contain elements such as Si, Cr, and Mo derived from the steel plate parent material, and the average mass fraction of the Si element is 0.2-1.0%. It is worth mentioning that the weld can also contain trace amounts of Nb, V, and Ti alloy elements, which play a role in precipitation strengthening and fine grain strengthening. The content of each of them is generally less than 0.12%, which can be derived from the steel plate parent material or the solder, further improving the tensile properties of the joint. The steel plate parent material mentioned above generally has a coating on at least one side, such as Figure 2The first steel plate 11 shown has a first surface coating 111 and a second surface coating 112. Generally, the coating is composed of aluminum and silicon, wherein the aluminum content is not less than 85%, and preferably the aluminum content exceeds 90%. The total coating thickness is generally 10-50 μm. The coating of the coated steel plate is generally composed of a metal alloy layer and an intermetallic compound alloy layer. The steel plate base material is generally composed of ferrite and pearlite, wherein the carbon content is not less than 0.15%, and has a boron content of about 0.002-0.006 to meet the hardenability of the subsequent quenching process, and can form a full martensitic structure after quenching, with high strength, and the typical boron steel tensile strength is not less than 1000Mpa. The typical steel plate base material grade 22MnB5 mainly contains the following elements by mass: 0.15%≤C≤0.45%; 0.5%≤Mn≤2.5%; 0.08%≤Si≤0.4%; Al≤0.45%; 0.01%≤Cr≤0.5%; Ti≤0.1%; Nb≤0.1%; V≤0.1%; S≤0.05%; P≤0.05%; 0.002%≤B≤0.006%; the rest is Fe and unavoidable impurities. The steel plate base material involved in the present invention is various steel grades with different carbon content or alloy elements, such as hot stamping steel, boron steel, martensitic steel, etc., which are well known in the art, but they are raw materials before quenching (stamping), and their thickness is generally 1.0-3.0 mm, which is well known in the art and will not be repeated here. In addition, the welding joint can be formed by laser welding a first steel plate 11 and a second steel plate 12 with different thicknesses or different coating states, and their strength levels can also be different, that is, a combination of different thicknesses or different strengths. For example, the tensile strength of the steel plate base material after hot stamping can exceed 2000Mpa.

[0053] The manufacturing method of the laser welded joint 2 described above mainly includes three steps: steel plate butt joint, laser welding and quenching treatment. Figure 3 shown.

[0054] In step 1, a set of first steel plates 11 and second steel plates 12 with aluminum coating to be welded are first provided, and then the first steel plates 11 and the second steel plates 12 are butt-welded, and there may be a gap or no gap between the first steel plates 11 and the second steel plates 12. Figure 4 As shown, the assembly gap width B is generally between 0-0.5 mm.

[0055] In step 2, laser welding is performed on the assembled steel plates, such as Figure 5As shown. A laser beam 3 and solder 4 are provided and transported to the butt joint position and travel along the welding path at a certain welding speed. The laser beam melts the first steel plate 11, the second steel plate 12 and the solder to form an initial weld 6 on the travel path. During the laser welding process, the melting volume of the two steel plates is V1, and the volume of the solder in the molten pool is V2. V1 and V2 satisfy , solder 4 is the laser welding solder of the present invention. The relative position between the solder and the laser beam can include various types, including coaxial delivery or off-axis delivery, which is well known in the art. In the process of laser welding, the laser beam is generally emitted by a laser, wherein the laser can include various types, such as a solid-state laser beam or a gas laser beam, specifically including a fiber laser, a disk laser, a semiconductor diode laser, and a Nd:YAG-type solid-state laser, or a CO2 gas laser. Of course, other types can also be included, as long as they can generate a laser beam and generate a keyhole and a molten weld pool. Figure 6 The figure shows a schematic top view of the welding process, 5 is a welding pool formed by the first steel plate 11, the second steel plate 12 and the solder 4 under the action of the laser beam, and 6 is an initial weld formed after cooling and solidification. In the welding process, the laser beam can also be composed of one or more light spots, and the beam energy distribution can be in various forms such as Gaussian distribution, average distribution or point ring distribution. In the welding process, the laser beam can also be fixed or synchronously move at high speed in various forms such as swinging when traveling along the welding direction. At this time, the swing shape can include various shapes such as circle, broken line, 8-shaped, ∞-shaped, etc. The swing frequency is generally 50-500HZ, and the swing amplitude is between 0.2-1.5mm. In the process of welding, multiple single or mixed protective gases can also be added, such as Ar gas, He gas, etc., or it can be carried out without protective gas.

[0056] The addition of solder during the welding process can include a variety of forms, including powder or wire delivery. When delivered by wire, it is laser wire welding, which is well known in the art. The wire feeding device can be, for example, MAG (metal active gas), MIG (metal inert gas), TIG (tungsten inert gas) as a feeding device. The welding wire can be a solid wire or a flux-cored wire. If added in the form of flux-cored wire or powder, it will be easier to achieve component ratio control, which is also well known in the art. The addition of solder can also be a composite of two different devices, for example, through two filler devices, different solders are delivered respectively, one delivering solder containing a certain component, and the other delivering solder of another component, and the combination of the two solders is realized to achieve the solder with the required proportion of components finally delivered into the molten pool. In addition, the solder 4 can also be added by synthesis through multiple steps or multiple parts; for example, the solder 4 is composed of 3 independent welding wires, and the average mass composition ratio of the final 3 solder combinations meets the content described in the present invention; and the 3 solders can be one mainly composed of Fe elements, one mainly composed of Ni elements, and one mainly composed of Mn elements, which are added at the same time. In addition, the addition of solder can be a multi-step method, for example, through a front-and-back method, so that the structure in the final welded joint meets more than 90% of the lath martensite composition. The combination of multiple welding wires will be more conducive to the manufacturing and production of welding wires and reduce the difficulty of welding wire production.

[0057] In the present invention, the regulation of different melting amounts is achieved by matching the laser welding speed with the welding wire feeding speed and controlling the welding wire composition. In the present invention, the welding speed and the wire feeding speed of the welding wire are controlled so that the initial weld front side height h10 and the initial weld back side height h11 on both sides of the initial weld obtained by welding are not lower than the final weld front side height h1 and the final weld back side height h2, which can be estimated based on the welding wire diameter, welding speed and wire feeding speed. Generally, the welding speed S1 is not less than 3m / min, and the welding wire diameter is d, which is generally 0.6-1.6mm, more commonly 1.0-1.2mm, which is generally more than twice the assembly gap width B. In the present invention, assuming that the average width of the upper and lower surfaces of the formed weld is B1, the wire feeding speed of the welding wire is S0, and the average thickness of the two steel plates is t, it must satisfy 0.05≤ ≤0.4; generally S0 is 0.5-4.0m / min; thus ensuring that the initial weld front height h10 and the initial weld back height h11 after welding do not exceed 0.4mm. Generally speaking, the heights on both sides of the initial weld section are of an overall dome-shaped morphology that is higher than the base surface of the steel plate. The volume of the melted solder during the entire process is V2, including the case with or without gaps; and the total volume melted by the steel plate base material is V1; it satisfies 0.02≤V2 / V1≤0.8, and more narrowly 0.02≤V2 / V1≤0.5, and the entire weld volume is composed of V1 and V2. The average width B1 of the upper and lower surfaces of the weld is generally between 0.5mm and 4.0mm, B10 is the width of the upper surface of the initial weld, and B11 is the width of the lower surface of the initial weld. Such as Figure 7 The figure shows a schematic cross-sectional view of the initial weld obtained after laser welding. The cross-sectional morphology of the initial weld formed can include various types; Figure 7 The overall shape is shown as X; it can also include a Y-shaped or U-shaped shape; Figure 8 , 9 The following are schematic diagrams of Y-shaped and U-shaped welds, respectively. Their specific shapes can be adjusted by matching the process parameters of the laser welding process. Fig.10 The figure shows a schematic diagram when the thickness of the first steel plate t1 and the thickness of the second steel plate t2 are different. Generally, the internal structure of the initial weld obtained is mainly martensite and residual austenite, and the martensite content is higher. Since the complete austenitization temperature of the initial weld must be different from that of the parent material after adding the solder containing Ni into the weld, it is ensured that the austenitization temperature Ac31 of the initial weld joint (weld) finally obtained deviates from the austenitization temperature Ac30 of the steel plate parent material by no more than 100°; and the martensite transformation start temperature Ms1 deviates from the martensite transformation start temperature Ms0 of the steel plate parent material by no more than 100°. To ensure that the Mn content in the weld after hot stamping and quenching is not less than 2.0%, and not more than 8%, and the volume fraction of the residual austenite content in the weld does not exceed 10%, and more narrowly not more than 5%. The retention of some residual austenite can produce a TRIP effect in the subsequent stress process to improve the joint performance.

[0058] When performing the hot stamping (quenching) process, it is ensured that the initial weld can achieve full austenitization under the heating temperature and heat preservation. Generally, the temperature is 880-980℃ and the heat preservation time is 90-500s. After heat preservation, rapid cooling is performed. This process can be achieved by a mold with rapid cooling or a liquid medium. The cooling rate is generally not less than 25℃ / s. When the mold is used for stamping cooling, various formed parts including flat plates and parts shapes can be formed, that is, a flat mold or a forming mold is used. When a flat mold is used for stamping cooling, the excess height morphology of the initial weld will become flat under the action of pressure. At this time, the final weld front excess height h1 and the final weld back excess height h2 will be smaller than the initial weld front excess height h10 and the initial weld back excess height h11. At this time, the surface excess height is approximately equivalent to a rectangular section, and the following mathematical formula is satisfied: 0.03≤(h1+h2) / (t1+t2)≤0.2. When water-cooling quenching is used, the initial weld surface reinforcement does not change much in shape compared to the final weld reinforcement, and the following is also satisfied: The inventive method, solder and weld joint can be used to manufacture components including hot stamped steel applications, such as various vehicles.

[0059] The technical solution of the present invention will be described in detail and completely through specific implementation methods below.

[0060] Example 1

[0061] like Fig.11 Shown is a cross-sectional view of an initial weld obtained after laser welding using the method of the present invention. Fig.12 The figure shows the cross-sectional view of the final weld after quenching and cooling. The original material for welding is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30μm thickness on both the upper and lower surfaces, and a strength of more than 1500Mpa after quenching, and its thickness is 1.5mm. The final weld is X-shaped as a whole, with a lath martensite content of about 96% in the weld, a mass fraction of Mn element in the weld of about 4.0%, an average mass fraction of aluminum element of about 1.4%, a Ni element content of about 0.6%, and a carbon element content lower than that of the original material; the widths of the final weld on both sides are about 2.3mm and 2.5mm, respectively, which are obtained by stamping with a flat die during quenching; the final weld front and back excess heights are about 0.08mm and 0.14mm, respectively; in the welding wire added during the welding process, Mn accounts for 22% of the welding wire mass fraction, and the Ni content is 3.2%. The diameter of the welding wire used is 1.2 mm, and the laser wire-filling welding method is used to manufacture the tailor-welded blanks; the assembly gap width B is 0 mm, the welding speed S1 is 5.0 m / min, the wire feeding speed S0 is 2.5 m / min, and the average melting volume V1 of the two steel plates per minute is about 18000 mm 3According to the wire feeding speed, the average melting volume V2 of the solder in the molten pool is about 2827mm per minute. 3 , V2 / V1≈0.157, satisfying 0.02≤V2 / V1≤0.8. After welding, the initial weld is placed in a heating furnace, heated to 930°C, and kept warm for about 300s. Then, hot stamping is performed under a flat die at a cooling rate of about 40°C / s and cooled to obtain a laser welded joint. Fig.13 The figure shows the mechanical properties test results of the laser welded joints after standard tensile specimen preparation. The results show that all three specimens failed in the parent material area, and the elongation at break reached 8.62%.

[0062] Example 2

[0063] like Fig.14 The figure shows another cross-sectional view of the final weld obtained by the method of the present invention. The welded raw material is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30 μm thickness on both the upper and lower surfaces, and a strength of more than 1500 MPa after quenching, and its thickness is 2.0 mm. The final weld is X-shaped as a whole, with a lath martensite content of about 96% in the weld, a mass fraction of Mn element in the weld of about 3.85%, an average mass fraction of aluminum element of about 1.3%, a Ni element content of about 0.50%, and a carbon element content lower than that of the original material; the widths of the final weld on both sides are about 1.6 mm and 1.8 mm, respectively, which are obtained by stamping with a flat die during quenching; the final weld front excess height and the final weld back excess height are about 0.1 mm and 0.07 mm, respectively; in the welding wire added during the welding process, Mn accounts for 15% of the welding wire mass fraction, and the Ni content is 3.2%. The diameter of the welding wire used is 1.2mm. The laser wire-filling welding method is used to manufacture the tailor-welded blanks. The assembly gap width B is 0.1mm, the welding speed S1 is 5.0m / min, the wire feeding speed S0 is 2.8m / min, and the average melting volume V1 of the two steel plates per minute is about 17000mm 3 According to the wire feeding speed, the average melting volume V2 of the solder in the molten pool is about 3167mm per minute. 3 , V2 / V1≈0.186, satisfying 0.02≤V2 / V1≤0.8. After welding, the initial weld is placed in a heating furnace, heated to 930°C, and kept warm for about 300s. Then, hot stamping is performed under a flat die at a cooling rate of about 40°C / s and cooled to obtain a laser welded joint. Fig.15 The figure shows the mechanical properties test results of the laser welded joints obtained. The results show that all three specimens failed in the parent material area, with a fracture elongation of about 8.52%.

[0064] Example 3

[0065] like Fig.16 The figure shows a cross-sectional view of a final weld obtained by the method of the present invention. The original materials for welding are respectively aluminum-silicon coatings with a coating thickness of about 30 μm on the surface, and the strengths of the quenched hot-formed steels are about 1500Mpa and 2000Mpa respectively, and the thickness is 1.4mm. The final weld is X-shaped as a whole, the martensite content of the lath in the weld is about 92%, the mass fraction of the Mn element in the weld is about 4.5%, the average mass fraction of the aluminum element is about 1.2%, the Ni element content is about 0.45%, and the carbon content is lower than that of the original material; the widths of the final weld on both sides are about 1.8mm and 1.6mm respectively, which are obtained by water quenching during quenching; the front and back excess heights of the final weld are about 0.18mm and 0.24mm respectively; in the welding wire added during the welding process, Mn accounts for 30% of the welding wire mass fraction, and the Ni content is 2.5%. The diameter of the welding wire used is 1.2 mm. The laser wire-filling welding method is used to manufacture the tailor-welded plates. The assembly gap width B is about 0.2 mm. The welding speed S1 is 5.0 m / min. The wire feeding speed S0 of the welding wire is 2.0 m / min. The average melting volume V1 of the two steel plates per minute is about 11900 mm3. The average melting volume V2 of the solder in the molten pool is estimated to be about 2262 mm3 per minute according to the wire feeding speed. 3 , V2 / V1≈0.084, satisfying 0.02≤V2 / V1≤0.8. After welding, the initial weld is placed in a heating furnace, heated to 930°C, and kept warm for about 300s. Then, hot stamping is performed under a flat die at a cooling rate of about 40°C / s and cooled to obtain a laser welded joint. Fig.17 The figure shows the mechanical properties test results of the laser welded joint after standard tensile specimen preparation. The results show that all three specimens broke and failed in the base material area with lower strength, and the elongation after fracture was about 8.17%.

[0066] Example 4

[0067] like Fig.18The figure shows a cross-sectional view of a final weld obtained by the method of the present invention. The original materials for welding are respectively aluminum-silicon coating with a coating thickness of about 20 μm on the surface and iso-strength hot-formed steel with a strength of about 1500 MPa after quenching, and the thicknesses are 1.4 mm and 1.6 mm respectively. The final weld is X-shaped as a whole, the martensite content of the lath in the weld reaches more than 97%, the mass fraction of Mn element in the weld is about 4.8%, the average mass fraction of aluminum element is about 1.0%, the content of Ni element is about 0.68%, and the carbon content is lower than that of the original material. The initial weld upper surface width B10 and the initial weld lower surface width B11 are approximately 1.4mm and 1.7mm respectively, which are obtained by water quenching during quenching; the initial weld front side height h10 and the initial weld back side height h11 are approximately 0.2mm and 0.3mm respectively; the final weld front side height h1 and the final weld back side height h2 are approximately 0.2mm and 0.3mm respectively; in the welding wire added during the welding process, Mn accounts for 22% of the welding wire mass fraction, and the Ni content is 3.2%. The diameter of the welding wire used is 1.2mm, and the laser wire filling welding method is used to manufacture the tailored welded plate. The assembly gap width B is approximately 0mm, the welding speed S1 is 5.0m / min, the wire feeding speed S0 is 2.0m / min, and the average melting volume V1 of the two steel plates per minute is approximately 11625mm 3 According to the wire feeding speed, the average melting volume V2 of the solder in the molten pool is about 2262mm per minute. 3 , V2 / V1≈0.19, satisfying 0.02≤V2 / V1≤0.8. After welding, the initial weld is placed in a heating furnace at a heating temperature of 930°C for a holding time of about 300s. Subsequently, water cooling is performed at a cooling rate exceeding 40°C / s to obtain a laser welded joint. Fig.19 The figure shows the mechanical properties test results of the laser welded joints after standard tensile specimen preparation. The results show that all three specimens failed in the base metal area of ​​the thin plate side, and the elongation after fracture reached 7.83%.

[0068] Example 5

[0069] The original material for welding is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30μm thickness on both the upper and lower surfaces, and a strength of more than 1500Mpa after quenching, and its thickness is 1.5mm. The final weld is X-shaped as a whole, with a lath martensite content of about 94% in the weld, a mass fraction of Mn elements in the weld of about 5.2%, an average mass fraction of aluminum elements of about 1.3%, and a Ni content of about 0.4%. The carbon content is lower than that of the original material; the widths of the final weld on both sides are about 2.4mm and 2.5mm respectively, which are obtained by stamping with a flat die during quenching; the final weld front and back excess heights are about 0.09mm and 0.16mm respectively; in the welding wire added during the welding process, Mn accounts for 30% of the welding wire mass fraction, and the Ni content is 1.5%. The diameter of the welding wire used is 1.2 mm, and the laser wire-filling welding method is used to manufacture the tailor-welded blanks; the assembly gap width B is 0 mm, the welding speed S1 is 5.0 m / min, the wire feeding speed S0 is 2.8 m / min, and the average melting volume V1 of the two steel plates per minute is about 18375 mm 3 According to the wire feeding speed, the average melting volume V2 of the solder in the molten pool is about 3167mm per minute. 3 , V2 / V1≈0.172, satisfying 0.02≤V2 / V1≤0.8. After welding, the initial weld was placed in a heating furnace, heated to 930°C, and kept warm for about 300s. Subsequently, the laser welded joint was obtained by hot stamping and cooling at a cooling rate of about 40°C / s under a flat die. All three joint specimens broke and failed in the parent material area, and the elongation at break reached 7.88%.

[0070] Example 6

[0071] The original material for welding is a hot-formed steel 22MnB5 with an aluminum-silicon coating of about 30μm thickness on both the upper and lower surfaces, and a strength of more than 1500Mpa after quenching, and its thickness is 1.5mm. The final weld is X-shaped as a whole, with a lath martensite content of about 94% in the weld, a mass fraction of Mn elements in the weld of about 3.2%, an average mass fraction of aluminum elements of about 1.3%, and a Ni content of about 0.8%. The carbon content is lower than that of the original material; the widths of the final weld on both sides are about 2.4mm and 2.5mm respectively, which are obtained by stamping with a flat die during quenching; the final weld front and back excess heights are about 0.09mm and 0.16mm respectively; in the welding wire added during the welding process, Mn accounts for 15% of the welding wire mass fraction, and the Ni content is 5.0%. The diameter of the welding wire used is 1.2 mm, and the laser wire-filling welding method is used to manufacture the tailor-welded blanks; the assembly gap width B is 0 mm, the welding speed S1 is 5.0 m / min, the wire feeding speed S0 is 2.4 m / min, and the average melting volume V1 of the two steel plates per minute is about 16875 mm 3According to the wire feeding speed, the average melting volume V2 of the solder in the molten pool is about 2714mm per minute. 3 , V2 / V1≈0.161, satisfying 0.02≤V2 / V1≤0.8. After welding, the initial weld was placed in a heating furnace, heated to 930°C, and kept warm for about 300s. Subsequently, the laser welded joint was obtained by hot stamping and cooling at a cooling rate of about 40°C / s under a flat die. All three joint specimens broke and failed in the parent material area, and the elongation at break reached 8.05%.

[0072] Table 1 lists the welding joint performance and related result data obtained in the above examples.

[0073]

[0074] All samples of the laser welded joints of Examples 1 to 6 broke and failed in the base material area, with a fracture strength greater than 1560 MPa and an elongation greater than 7.5. They have very high mechanical properties and can meet the production and manufacturing of related parts.

[0075] Comparative Example

[0076] When the same welding raw materials as in Example 1 are used, welding is performed without filler wire, and different surface treatments are performed, all the welded joints of the comparative example are broken and failed at the weld position, and the relevant mechanical properties are as follows:

[0077]

[0078] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A laser welded joint, wherein when two steel plates are butt-jointed for laser welding, laser welding solder is added to the molten pool to form an initial weld, and the initial weld is quenched to form the laser welded joint, wherein at least one of the steel plates is a steel plate with an aluminum coating or an aluminum alloy coating, characterized in that: The volume fraction of the internal lath martensite of the laser welded joint is not less than 90%, the average mass fraction of the Mn element is 3.2% to 5.2%, the average mass fraction of the Al element is not higher than 1.4%, and the average mass fraction of the C element is lower than the C content of the steel plate base material. The final weld front side reinforcement h1 and the final weld back side reinforcement h2 formed by the laser welded joint do not exceed 0.4 mm; The solder is composed of Fe, Mn, Ni, trace alloying elements and other inevitable elements, wherein, by weight percentage, the following conditions are met: Mn ≥ 15%, 1.5% ≤ Ni ≤ 5%, trace alloying elements 0-0.36%, and other inevitable elements ≤ 2%; the trace alloying element is at least one of Nb, V, and Ti, and the contents of Nb, V, and Ti do not exceed 0.12%; The solder is a welding wire, and the welding speed S1 and the wire feeding speed S0 of the welding wire during the welding process satisfy the following relationship: 0.05≤ ≤0.4, where d is the diameter of the welding wire, d is in the range of 0.6-1.6mm and is more than twice the width of the assembly gap B, B is in the range of 0-0.5mm, S1 is not less than 3m / min, B1 is the average width of the upper and lower surfaces of the weld formed, S0 is in the range of 0.5-4.0m / min, and t is the average thickness of the two steel plates; The specific steps of quenching are: keeping the initial weld at 880-980°C for 90-500s, and then cooling it rapidly through a mold with rapid cooling or a liquid medium, with a cooling rate of ≥25°C / s; The rapid cooling method is flat die stamping cooling, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint meet , where t1 is the thickness of the first steel plate, and t2 is the thickness of the second steel plate; Or the rapid cooling method is water-cooling quenching, the initial weld front side height h10 and the initial weld back side height h11 meet 0.03≤ ≤0.3, where t1 is the thickness of the first steel plate, t2 is the thickness of the second steel plate, B10 is the initial weld upper surface width, and B11 is the initial weld lower surface width.

2. The laser welded joint according to claim 1, characterized in that: The volume fraction of the lath martensite is not less than 92%.

3. A method for manufacturing a laser welded joint, characterized in that: The method comprises the following steps: Step 1: provide two steel plate base materials, at least one of which is a steel plate with an aluminum coating or an aluminum alloy coating, and butt the two steel plates; Step 2: Laser welding the steel plates together, wherein solder is added to the molten pool during the welding process to form an initial weld; Step 3: quenching and cooling the initial weld to obtain the laser welded joint according to any one of claims 1 to 2; Step 2 During the laser welding process, the melting volume of the two steel plates is V1, and the volume of the solder in the molten pool is V2. V1 and V2 satisfy ; In step 2, the solder is a welding wire, and the solder is composed of Fe, Mn, Ni, trace alloying elements and other inevitable elements, wherein, by weight percentage, the following conditions are met: Mn ≥ 15%, 1.5% ≤ Ni ≤ 5%, trace alloying elements 0-0.36%, and other inevitable elements ≤ 2%; the trace alloying elements are at least one of Nb, V, and Ti, and the contents of Nb, V, and Ti do not exceed 0.12%; during welding, the welding speed S1 and the wire feeding speed S0 of the welding wire meet the following relationship: 0.05 ≤ ≤0.4, where d is the diameter of the welding wire, d is in the range of 0.6-1.6mm and is more than twice the width of the assembly gap B, B is in the range of 0-0.5mm, S1 is not less than 3m / min, B1 is the average width of the upper and lower surfaces of the weld formed, S0 is in the range of 0.5-4.0m / min, and t is the average thickness of the two steel plates; The specific steps of quenching are: keeping the initial weld at 880-980°C for 90-500s, and then cooling it rapidly through a mold with rapid cooling or a liquid medium, with a cooling rate of ≥25°C / s; The rapid cooling method is flat die stamping cooling, and the final weld front side excess height h1 and the final weld back side excess height h2 formed by the laser welding joint meet , where t1 is the thickness of the first steel plate, and t2 is the thickness of the second steel plate; Or the rapid cooling method is water-cooling quenching, the initial weld front side height h10 and the initial weld back side height h11 meet 0.03≤ ≤0.3, where t1 is the thickness of the first steel plate, t2 is the thickness of the second steel plate, B10 is the initial weld upper surface width, and B11 is the initial weld lower surface width.

4. A high-strength steel workpiece, characterized in that: The high-strength steel workpiece is composed of two steel plate mother materials and a laser welding joint as described in any one of claims 1-2 for connecting the mother materials; when the high-strength steel workpiece is subjected to a tensile test, it breaks and fails in the mother material area, and the elongation at break is not less than 5%.