A defect-rich carbon carrier for proton exchange membrane fuel cell and preparation method thereof

By preparing defect-rich carbon support, the problems of fuel cell catalyst falling off and transition metal dissolution under high potential are solved, the stability and electrocatalytic activity of the catalyst are improved, and the cost reduction and easy production expansion effect is achieved.

CN118367161BActive Publication Date: 2024-11-29NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410790493.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-29
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Existing fuel cell catalysts are prone to catalyst particles falling off and transition metal dissolution under high potentials, and fail to effectively regulate the surface defects of the carbon support, affecting the electrocatalytic activity and stability of the catalyst.

Method used

Defective-rich carbon support is prepared by hydrochloric acid polymerization, hydrothermal reaction, carbonization, ball milling and pickling steps, to regulate the surface micromorphology and defect sites of the carbon support, and improve the deposition stability and electrocatalysis of catalyst particles. active.

Benefits of technology

The deposition stability of the catalyst and the electrocatalytic oxygen reduction reaction activity are improved, the cost is reduced, and the preparation method is simple and easy to expand production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118367161B_ABST
    Figure CN118367161B_ABST
Patent Text Reader

Abstract

The invention discloses a defect-rich carbon carrier for a proton exchange membrane fuel cell and a preparation method thereof, the preparation method comprising the following steps: S1, dissolving a biomass-based carbon source in an organic solvent, stirring and then adding hydrochloric acid for polymerization; S2, dissolving the substance obtained in step S1 in a mixed aqueous solution of a non-precious metal salt hydrate and urea, placing the mixed solution in a reactor for hydrothermal reaction, and obtaining a polymer containing non-precious metal particles; S3, placing the polymer obtained in step S2 in a tubular furnace for heat preservation and heat treatment to achieve polymer carbonization; S4, ball milling the carbonized material obtained in step S3; S5, dissolving the powder obtained in step S4 in a hydrochloric acid solution, stirring evenly, rotary evaporating, and drying to obtain a defect-rich carbon carrier. The present invention prepares a carbon carrier material containing surface micromorphology and rich defects, and these defect sites are conducive to the anchoring of the subsequently deposited catalyst particles, thereby improving the electrocatalytic oxygen reduction reaction activity and stability of the catalyst layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cell catalysts, and in particular to a defect-rich carbon carrier of a proton exchange membrane fuel cell and a preparation method thereof. Background Art

[0002] A fuel cell is a device that directly converts chemical energy into electrical energy. It generates electricity and water through a redox reaction between fuels such as hydrogen and methanol and oxygen under the action of a catalyst. Fuel cells have the advantages of high efficiency, low pollution, and no noise, and are widely used in transportation, aerospace, household electricity, and other fields. Among them, the catalyst is an important component of the fuel cell, which improves the efficiency of the battery through electrocatalytic reactions. Commonly used fuel cell catalysts include precious metals such as platinum and palladium. They have good catalytic activity and stability, but their high cost limits the commercial application of fuel cells. In order to reduce costs and improve the performance of catalysts, researchers began to explore the use of carbon carriers as alternative materials for catalysts. Carbon carriers have good conductivity, chemical stability, and rich surface functional groups, which can improve the activity and stability of catalysts. By regulating the structure and surface functional groups of carbon carriers, efficient redox reactions can be achieved, promoting the development of fuel cell technology and providing new possibilities for the commercial application of fuel cells.

[0003] The electrocatalytic reaction in the fuel cell is a surface reaction, so researchers often use porous carbon as a carrier to increase the exposure area of ​​the catalyst, thereby increasing the electrochemical active sites of the catalyst. For example, patent document CN117497787A discloses a method for preparing intermetallic compound catalyst nanoparticles by step-by-step evaporation of solvents. This method can reduce the amount of precious metals used and avoid the agglomeration problem of transition metal single atoms during the preparation process, but does not consider the adsorption stability of catalyst particles on the carrier surface, especially the problem of catalyst particles falling off under long-term circulation, and the transition metal dissolution that is easy to occur in alloy catalysts under high potential. Patent document CN117023572A discloses a graphitized nitrogen-doped mesoporous carbon material and its preparation method and application, using phenolic resin generated by the reaction of dopamine and formaldehyde as a carbon source and a nitrogen source, in-situ preparing N-doped porous carbon, and then immersing it in iron salt, using the catalytic properties of the metal iron salt to achieve carbon graphitization under low temperature conditions, and finally using acid washing to remove iron to obtain a graphitized nitrogen-doped carbon material. This technology uses iron salts to catalyze graphitization conversion and is loaded on the surface of nitrogen-doped carbon. However, this method does not take into account the regulatory effect of metal salts on the surface defects of carbon materials, which will have a crucial impact on the subsequent loading of precious metals and electrocatalytic activity. Summary of the invention

[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide a process for preparing a carbon carrier with a high degree of graphitization and rich surface defects.

[0005] To achieve the above object, the first aspect of the present invention provides a method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell, comprising the following steps:

[0006] S1, dissolving a biomass-based carbon source in an organic solvent, adding hydrochloric acid to polymerize after stirring, and removing the hydrochloric acid and remaining monomers by rotary evaporation after polymerization;

[0007] S2, dissolving the substance obtained in step S1 in a mixed aqueous solution of non-precious metal salt hydrate and urea, placing the mixed solution in a reactor for hydrothermal reaction, collecting the reaction product by centrifugation, and drying to obtain a polymer containing non-precious metal particles;

[0008] S3, placing the polymer obtained in step S2 in a tubular furnace for heat treatment to achieve carbonization of the polymer;

[0009] S4, ball-milling the carbonized material obtained in step S3;

[0010] S5. Dissolve the powder obtained in step S4 in a hydrochloric acid solution, stir evenly, and obtain a defect-rich carbon carrier after rotary evaporation and drying.

[0011] The present invention provides a novel method for preparing a carbon carrier. Non-precious metal particles are deposited on a biomass-based carbon source after polymerization, and then carbonization, ball milling, and acid washing steps are performed to obtain a carbon carrier material containing surface micromorphology and rich defects. These defect sites are conducive to the anchoring of subsequently deposited catalyst particles, thereby improving the electrocatalytic oxygen reduction reaction activity and stability of the catalytic layer.

[0012] Furthermore, in step S1, the biomass-based carbon source is selected from one or more of D-glucose, lactic acid, ethylene glycol, furfuryl alcohol, and 5-hydroxymethylfurfural, and the organic solvent is selected from one or more of methanol, n-propanol, and isopropanol.

[0013] Furthermore, in step S1, the hydrochloric acid concentration is 1 to 6 mol / L, and the stirring time is 0.5 to 12 hours. The pore size acidity and alkalinity of the material are adjusted by hydrochloric acid, thereby having a positive effect on the catalyst activity.

[0014] Furthermore, in step S2, the non-precious metal salt hydrate is selected from one or more of NiCl2·6H2O, CoCl2·6H2O, FeCl3·6H2O, ZnCl2·4H2O, MnCl2·4H2O, and CuCl2·2H2O. The introduction of chlorine into the mixed solution is conducive to uniform dispersion of the non-metallic particles.

[0015] Furthermore, in step S2, the concentration of the non-precious metal salt in the mixed aqueous solution of the non-precious metal salt hydrate and urea is 0.1 to 1 mmol / L, and the concentration of urea is 0.1 to 20 mmol / L. Urea is used to neutralize acidity and alkalinity and adjust the hydrophilicity and hydrophobicity of the carrier surface, thereby adjusting the agglomerated particle size of the carrier.

[0016] Furthermore, in step S2, the hydrothermal reaction temperature is 100-120° C., and the reaction time is 10-12 hours. Controlling the polymerization reaction process conditions can effectively regulate the deposition effect of non-precious metal particles on the material surface, thereby controlling the surface morphology of the carbon carrier.

[0017] Furthermore, in step S3, the heat treatment temperature is 800-1000° C. and the holding time is 0.5-5 hours. The presence of non-precious metal particles catalyzes carbonization, thereby reducing the temperature required for carbonization and saving process costs.

[0018] Furthermore, in step S4, the ball milling speed is 300-900 rpm and the time is 0.5-3 hours. The material is ground into powder, thereby achieving micromorphology control of the carbon carrier.

[0019] Furthermore, in step S5, the pH of the hydrochloric acid solution is 1 to 3. Acid washing can remove non-precious metal particles deposited on the surface of the material, thereby obtaining a micro-morphology and defect-rich carbon carrier.

[0020] A second aspect of the present invention provides a defect-rich carbon carrier for a proton exchange membrane fuel cell, which is prepared by the above-mentioned preparation method.

[0021] In summary, compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention uses biomass-based carbon sources as raw materials and achieves micro-morphology and defect-rich preparation of carbon carriers through non-precious metal polymerization, carbonization, ball milling, and acid washing steps.

[0023] (2) The surface of the carbon support prepared by the present invention is rich in defects, which can improve the subsequent deposition stability of catalyst particles. The carbon support has a high specific surface area, which helps to increase the exposure sites of the catalyst, thereby improving the catalytic performance.

[0024] (3) The preparation method of the present invention is simple, low-cost, and easy to scale up production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the process of preparing a defect-rich carbon carrier in a specific embodiment of the present invention.

[0026] Figure 2This is a transmission electron microscope image of the platinum-carbon catalyst prepared in Example 1 of the present invention.

[0027] Figure 3 This is a graph showing the change in the initial potential of the membrane electrode prepared in Example 1 of the present invention as a function of the number of cycle tests.

[0028] Figure 4 This is a graph showing the change in the ECSA adsorption peak of the membrane electrode prepared in Example 1 of the present invention as a function of the number of cycle tests.

[0029] Figure 5 This is a transmission electron microscope image of the platinum-carbon catalyst prepared in Example 2 of the present invention.

[0030] Figure 6 This is a graph showing the change in the initial potential of the membrane electrode prepared in Example 2 of the present invention as a function of the number of cycle tests.

[0031] Figure 7 This is a graph showing the change in the ECSA adsorption peak of the membrane electrode prepared in Example 2 of the present invention as a function of the number of cycle tests.

[0032] Figure 8 This is a graph showing the change in the ECSA desorption peak of the membrane electrode prepared in Example 2 of the present invention as a function of the number of cycle tests.

[0033] Fig. 9 This is a transmission electron micrograph of the platinum-carbon catalyst prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0035] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0036] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention's description will be apparent to those skilled in the art.

[0037] The specific embodiment of the present invention provides a method for preparing a defect-rich carbon carrier, combining Figure 1 As shown, the following steps are included:

[0038] (1) Aggregation

[0039] The biomass-based carbon source is dissolved in an organic solvent, and hydrochloric acid is added after stirring for polymerization, preferably the concentration of hydrochloric acid is 1 to 6 mol / L, and the stirring time is 0.5 to 12 hours. After polymerization, the hydrochloric acid and the remaining monomers are removed by rotary evaporation. In a specific embodiment, the optional biomass-based carbon source includes: D-glucose, lactic acid, ethylene glycol, furfuryl alcohol, 5-hydroxymethylfurfural, etc., and the organic solvent includes: methanol, n-propanol, isopropanol, etc.

[0040] (2) Hydrothermal

[0041] The polymerized substance is dissolved in a mixed aqueous solution of non-precious metal salt hydrate and urea. In a specific embodiment, the optional non-precious metal salt hydrate includes: NiCl2·6H2O, CoCl2·6H2O, FeCl3·6H2O, ZnCl2·4H2O, MnCl2·4H2O, CuC12·2H2O, etc.; the preferred concentration of non-precious metal salt in the mixed aqueous solution of non-precious metal salt hydrate and urea is 0.1 ~ 1 mmol / L, and the preferred concentration of urea is 0.1 ~ 20 mmol / L. The mixed solution is placed in a reactor for hydrothermal reaction to deposit non-precious metal particles on the surface of the material. The hydrothermal reaction temperature is 100~120℃, and the reaction time is 10~12 hours. The reaction product is collected by centrifugation and dried to obtain a polymer containing non-precious metal particles.

[0042] (3) Carbonization

[0043] The polymer with non-precious metal particles is placed in a tube furnace for heat treatment to achieve carbonization of the polymer. In a specific embodiment, the heat treatment temperature is 800-1000° C. and the heat treatment time is 0.5-5 hours.

[0044] (4) Ball milling

[0045] The carbonized material is ball-milled to achieve micro-morphology control of the carbon carrier. In a specific embodiment, the ball-milling speed is 300-900 rpm and the time is 0.5-3 hours.

[0046] (5) Pickling

[0047] The ball-milled powder is dissolved in a hydrochloric acid solution with a pH of 1 to 3 and stirred evenly. After rotary evaporation and drying, a micro-morphology and defect-rich carbon carrier is obtained.

[0048] The carbon carrier prepared by the above method can be used as a carrier of proton exchange membrane fuel cell catalyst. The surface of the carbon carrier is rich in defects. These defect sites are conducive to the anchoring of subsequently deposited Pt, PtCo, Ru and other catalyst particles, thereby improving the activity and stability of electrocatalytic oxygen reduction (ORR).

[0049] The technical solutions and effects of the present invention are illustrated below in conjunction with specific embodiments. Example 1

[0050] Dissolve 10 g of furfuryl alcohol in 100 ml of methanol, stir vigorously for 2 hours, add 1 mol / L hydrochloric acid for polymerization, and remove hydrochloric acid and residual monomers at 60 °C after polymerization. Place the obtained black substance in a mixed solution of 0.1 mmol / L NiCl2·6H2O and 1 mmol / L urea. Place the mixed solution in a polytetrafluoroethylene reactor at 120 °C for 12 hours, centrifuge to obtain the lower layer, and place it in a vacuum drying oven at 80 °C to obtain a metal-containing polymer. Place the polymer in a tubular furnace with N2, and heat it from 25 °C to 1000 °C at 5 °C / min, and maintain the temperature for heat treatment for 2 hours. The carbonized material is ball milled at 600 rpm for 2 hours. Dissolve the ball-milled powder in a hydrochloric acid solution with a pH of 1 and stir evenly. After rotary evaporation at 60 °C, place it in a vacuum drying oven at 80 °C for 8 hours to obtain a defect-rich carbon carrier material.

[0051] The carbon support prepared in the above example was dispersed in water, and then H2PtCl6 and formic acid were added, stirred for 5 hours, filtered, washed, and dried to obtain a platinum-carbon catalyst, the morphology of which is as follows: Figure 2 As shown in Figure 2, the average particle size is 4.12 nm and D50 is 4 nm. The specific surface area of ​​the carbon support calculated by BET is 1200 m 2 / g, the specific surface area of ​​the platinum-carbon catalyst is 606 m 2 / g. The Pt loading of the platinum-carbon catalyst tested by RED was 50%, and the half-cell ECSA was 54.40 m 2 / gPt, and the mass activity is 0.18 A / mgPt.

[0052] The above platinum-carbon catalyst was coated on the proton exchange membrane to prepare a membrane electrode, and the membrane electrode loading was 0.2 Pt, mg / cm 2 , the durability of the membrane electrode was tested under the following conditions: 90°C, 30,000 cycles; 100% RH; H2 / N2; 0.6-0.95 V, 3 s square wave cycle each; fixture: 50 cm 2 , serpentine flow channel (groove width: 0.5 mm depth: 0.5 mm). The test results are as follows Figure 3 and Figure 4 As shown, after 30,000 cycles of cycling, the onset potential ORR decreased by 13 mV and the ECSA adsorption peak increased by 2.76%, showing good stability. Example 2

[0053] Dissolve 10 g of 5-hydroxymethylfurfural in 100 ml of methanol, stir vigorously for 1 hour, add 3 mol / L hydrochloric acid for polymerization, and remove hydrochloric acid and residual monomers by rotary evaporation at 60°C after polymerization. Place the obtained black substance in a mixed solution of 1 mmol / L FeCl3·6H2O and 10 mmol / L urea. Place the mixed solution in a polytetrafluoroethylene reactor at 120°C for 10 hours, centrifuge to obtain the lower layer, and place it in a vacuum drying oven at 80°C to obtain a metal-containing polymer. Place the polymer in a tubular furnace with N2, and heat it from 25°C to 950°C at 5°C / min, and maintain the temperature for heat treatment for 2.5 hours. The carbonized material is ball milled at 500 rpm for 2 hours. The ball-milled powder is dissolved in a hydrochloric acid solution with a pH of 3 and stirred evenly. After rotary evaporation at 60°C, place it in a vacuum drying oven at 80°C for 8 hours to obtain a defect-rich carbon carrier material.

[0054] The same method as in Example 1 was used to load Pt catalyst particles to obtain a platinum-carbon catalyst having the following morphology: Figure 5 As shown in Figure 2, the average particle size is 3.32 nm and D50 is 3.19 nm. The specific surface area of ​​the carbon support calculated by BET is 1289 m 2 / g, and the specific surface area of ​​the platinum-carbon catalyst is 590 m 2 / g. The Pt loading of the platinum-carbon catalyst tested by RED was 49.6%, and the half-cell ECSA was 51.62m 2 / gPt, and the mass activity is 0.15 A / mgPt.

[0055] The above platinum-carbon catalyst was coated on the proton exchange membrane to prepare a membrane electrode, and the membrane electrode loading was 0.3 Pt, mg / cm 2 The durability of the membrane electrode was tested under the following conditions: 85°C, 90,000 cycles; 95°C, 10,000 cycles; 100% RH; H2 / N2; 0.6-0.95 V, 3 s square wave cycles each; fixture: 50 cm 2 , serpentine flow channel (groove width: 0.5mm depth: 0.5mm). The test results are as follows Figure 6 , Figure 7 and Figure 8 As shown, after 100,000 cycles of endurance test, the onset potential ORR decreased by 20 mV, the ECSA adsorption peak drop ratio was 0.57%, and the desorption peak drop ratio was 10.57%, showing good stability. Example 3

[0056] Dissolve 10 g of lactic acid in 100 ml of methanol, stir vigorously for 6 hours, add 2 mol / L hydrochloric acid for polymerization, and remove hydrochloric acid and residual monomers by rotary evaporation at 60°C after polymerization. Place the obtained black substance in a mixed solution of 0.5 mmol / L CoCl2·6H2O and 5 mmol / L urea. Place the mixed solution in a polytetrafluoroethylene reactor at 110°C for 12 hours, centrifuge to obtain the lower layer, and place it in a vacuum drying oven at 80°C to obtain a metal-containing polymer. Place the polymer in a tubular furnace with N2, and heat it from 25°C to 900°C at 5°C / min, and keep the temperature for heat treatment for 3 hours. The carbonized material is ball-milled at 900 rpm for 1 hour using a ball mill. Dissolve the ball-milled powder in a hydrochloric acid solution with a pH of 2 and stir evenly. After rotary evaporation at 60°C, place it in a vacuum drying oven at 80°C and dry it for 8 hours to obtain a defect-rich carbon carrier material.

[0057] The same method as in Example 1 was used to load Pt catalyst particles to obtain a platinum-carbon catalyst having the following morphology: Fig. 9 As shown in Figure 2, the average particle size is 3.45 nm and D50 is 3.35 nm. The specific surface area of ​​the carbon support calculated by BET is 939 m 2 / g, the specific surface area of ​​the platinum-carbon catalyst is 523 m 2 / g. The Pt loading of the platinum-carbon catalyst tested by RED was 44%, and the half-cell ECSA was 54.33 m 2 / gPt, and the mass activity is 0.11 A / mgPt.

[0058] The above platinum-carbon catalyst was coated on the proton exchange membrane to prepare a membrane electrode, and the membrane electrode loading was 0.2 Pt, mg / cm 2 The durability of the membrane electrode was tested under the following conditions: 85°C, 90,000 cycles; 95°C, 10,000 cycles; 100% RH; H2 / N2; 0.6-0.95 V, 3 s square wave cycles each; fixture: 50 cm 2 , serpentine flow channel (groove width: 0.5 mm depth: 0.5 mm). After 100,000 cycles of endurance test, the onset potential ORR decreased by 1 mV, the ECSA adsorption peak drop ratio was 9.48%, and the desorption peak drop ratio was 13.96%, showing good stability. Example 4

[0059] Dissolve 10 g of D-glucose in 100 ml of n-propanol, stir vigorously for 2 hours, add 6 mol / L hydrochloric acid for polymerization, and remove hydrochloric acid and residual monomers by rotary evaporation at 60°C after polymerization. Place the obtained black substance in a mixed solution of 0.2 mmol / L ZnCl2·4H2O and 15 mmol / L urea. Place the mixed solution in a polytetrafluoroethylene reactor at 120°C for 10 hours, centrifuge to obtain the lower layer, and place it in a vacuum drying oven at 80°C to obtain a metal-containing polymer. Place the polymer in a tubular furnace with N2, and heat it from 25°C to 1000°C at 5°C / min, and maintain the temperature for heat treatment for 4 hours. The carbonized material is ball milled at 300 rpm for 3 hours. Dissolve the ball-milled powder in a hydrochloric acid solution with a pH of 1 and stir evenly. After rotary evaporation at 60°C, place it in a vacuum drying oven at 80°C for 8 hours to obtain a defect-rich carbon carrier material.

[0060] The Pt catalyst particles were loaded in the same manner as in Example 1 to obtain a platinum-carbon catalyst with an average particle size of 2.85 nm and a D50 of 2.84 nm. The Pt loading of the platinum-carbon catalyst in the RED test was 60%, and the half-cell ECSA was 65.5 m 2 / gPt, and the mass activity is 0.12 A / mgPt.

[0061] Comparative Example 1

[0062] The commercially available JM 40% platinum carbon catalyst was used as a comparative example. The Pt loading of the catalyst was 40% and the half-cell ECSA was 53.03 m 2 / gPt, and the mass activity is 0.097 A / mgPt. The performance of the platinum-carbon catalyst prepared in Examples 1-4 is better than that of the JM catalyst.

[0063] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell, characterized in that: The following steps are involved: S1, dissolving the biomass-based carbon source in an organic solvent, adding hydrochloric acid for polymerization after stirring, the hydrochloric acid concentration is 1 to 6 mol / L, the stirring time is 0.5 to 12 hours, and after polymerization, the hydrochloric acid and remaining monomers are removed by rotary evaporation; S2, dissolving the substance obtained in step S1 in a mixed aqueous solution of non-precious metal salt hydrate and urea, wherein the concentration of the non-precious metal salt is 0.1-1 mmol / L, and the concentration of urea is 0.1-20 mmol / L, placing the mixed solution in a reactor for hydrothermal reaction, collecting the reaction product by centrifugation, and drying to obtain a polymer containing non-precious metal particles; S3, placing the polymer obtained in step S2 in a tubular furnace for heat treatment to achieve carbonization of the polymer; S4, ball-milling the carbonized material obtained in step S3; S5. Dissolve the powder obtained in step S4 in a hydrochloric acid solution having a pH of 1 to 3, stir evenly, remove non-precious metal particles deposited on the surface of the material, and obtain a defect-rich carbon carrier after rotary evaporation and drying.

2. The method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S1, the biomass-based carbon source is selected from one or more of D-glucose, lactic acid, ethylene glycol, furfuryl alcohol, and 5-hydroxymethylfurfural, and the organic solvent is selected from one or more of methanol, n-propanol, and isopropanol.

3. The method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S2, the non-precious metal salt hydrate is selected from one or more of NiCl2·6H2O, CoCl2·6H2O, FeCl3·6H2O, ZnCl2·4H2O, MnCl2·4H2O, and CuCl2·2H2O.

4. The method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S2, the hydrothermal reaction temperature is 100-120° C., and the reaction time is 10-12 hours.

5. The method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S3, the heat treatment temperature is 800-1000° C., and the heat preservation time is 0.5-5 hours.

6. The method for preparing a defect-rich carbon carrier for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S4, the ball milling speed is 300-900 rpm, and the time is 0.5-3 hours.

7. A defect-rich carbon carrier for a proton exchange membrane fuel cell, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Graphitized nitrogen-doped mesoporous carbon material, preparation method and application

    CN117023572A

  • Precious metal nanoparticle synergistic transition metal monatomic catalyst, preparation and application

    CN117497787A

  • Preparing method for nitrogen-doped porous carbon material, catalyst comprising material and application of material

    CN104689857A

  • Lignin-based transition metal / nitrogen doped carbon material, and preparation and application thereof

    CN109012590A

  • Nitrogen-doped porous carbon non-metal catalyst and preparation method thereof, and application of nitrogen-doped porous carbon non-metal catalyst in oxidation-reduction reaction