A method for preparing Cu-SSZ-13 molecular sieve catalyst using natural minerals
The Cu-SSZ-13 molecular sieve catalyst is prepared by a hydrothermal method using natural mineral silicon and aluminum sources and low amounts of templates, which solves the problems of high preparation costs and easy deactivation at high temperatures, and achieves environmentally friendly, low-cost and efficient denitrification oxides. performance, and the amount of copper introduced is controllable.
Patent Information
- Application Number
- CN202410840274.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing Cu-SSZ-13 molecular sieve has high preparation costs, uses a large amount of chemical reagents, leads to large pollution, and has not improved the problem of easy deactivation at high temperatures.
The natural mineral silicon and aluminum source is used for thermal activation, and combined with an alkali source, activator and low-amount template agent, the reaction gel is prepared by hydrothermal method, followed by crystallization, washing, drying and calcination, and finally Cu- is obtained through ion exchange. SSZ-13 molecular sieve catalyst avoids the use of additional chemical reagents and cumbersome steps.
The preparation of low-cost, environmentally friendly Cu-SSZ-13 molecular sieve has been achieved, with excellent nitrogen oxide removal performance and high temperature stability, reducing environmental pollution and resource consumption, and the amount of copper introduced can be controlled.
Smart Images

Figure CN118371264B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a Cu-SSZ-13 molecular sieve catalyst by utilizing natural minerals, and belongs to the field of catalytic material preparation and waste gas treatment. Background Art
[0002] SSZ-13 molecular sieve catalyst is favored for its special three-dimensional pore structure and large specific surface area. At present, commercial molecular sieve catalysts are widely used in the fields of catalytic cracking of petroleum hydrocarbons, methanol to olefins, industrial denitrification treatment, photoelectrocatalysis, etc., and have broad prospects. Since the silicon and aluminum sources used in most molecular sieve catalysts are chemical reagents, the preparation process will inevitably cause damage to the environment. In addition, in order to obtain molecular sieve catalysts with excellent performance and good crystallinity, it is usually necessary to add a large amount of organic templates to guide the growth of the crystal structure. The calcination step to remove the template will cause environmental pollution, and the template is expensive and has high use costs, which to a certain extent restricts the further development of molecular sieve catalysts. It is imperative to develop an environmentally friendly, low-cost and large-scale promotion process for the preparation of SSZ-13 molecular sieve catalysts, and it also finds a way to solve the green synthesis of large quantities of SSZ-13 molecular sieve catalysts in the future.
[0003] Industrial flue gas nitrogen oxides (NOx) are one of the main air pollutants. Automobile exhaust contains a large amount of NOx. If it is discharged directly without treatment, it will aggravate environmental problems such as photochemical smog, acid rain and ozone layer depletion. As the most mature nitrogen oxide removal technology at present, the catalyst used in ammonia selective catalytic reduction (NH3-SCR) is largely derived from molecular sieves. However, the problem of molecular sieve catalysts being easily deactivated at high temperatures has always been difficult to overcome.
[0004] Patent CN201811354909.1 discloses a method for preparing a mesoporous Fe-Cu-SSZ-3 molecular sieve and its application, using natural minerals to synthesize mesoporous Fe-Cu-SSZ-13 in one pot, and for the first time proposed to combine demolding and two roastings after ion exchange, but the amount of copper introduced in this invention is large and uncontrollable, the acid treatment step consumes a large amount of chemical acid reagents, and the product has poor crystallinity. Patent CN202311640112.9 discloses a method for preparing a Cu-SSZ-13 molecular sieve with high NH3-SCR activity, using water, an alkali source containing alkali metal cations, natural minerals, a supplementary silicon source, and a seed crystal, and obtaining a Cu-SSZ-13 molecular sieve by crystallization and washing, but it requires additional chemical silicon source. Patent CN202111515858.8 discloses a method and application for synthesizing SSZ-13 molecular sieves under an ultra-low template system. The chemical reagent silicon-aluminum source and the template agent are mixed evenly to obtain a gel, and SSZ-13 seed crystals, structural unit assembly promoters, etc. are added to the gel to crystallize to obtain Na-SSZ-13 molecular sieves. The silicon-aluminum sources of this invention are all chemical reagents. Patent CN202110159373.3 discloses a method and application for preparing SSZ-13 molecular sieves at low cost. Kaolin is roasted separately to obtain partial soil and high soil. The mixture of the two is used as a raw material to add chemical reagent silicon source, alkali solution, template agent, and crystallization directing agent. SSZ-13 molecular sieves are crystallized. Silicon source and alkali solution are chemical reagents. Patent CN202110062776.6 discloses a method for synthesizing low-template SSZ-13 molecular sieves. Chemical reagent silicon-aluminum source and organic template agent are used to crystallize to obtain SSZ-13 molecular sieves. Similarly, silicon-aluminum sources are all chemical reagents. Patent CN202311140398.4 discloses a SSZ-13 molecular sieve and its preparation method and application. The natural silica-alumina mineral is activated by a first alkali source, and SSZ-13 seed crystals are added for mechanical treatment. The reaction gel obtained by adding a silicon source, a second alkali source, and water is aged and crystallized to obtain the SSZ-13 molecular sieve. The operation steps are complicated and the high-temperature denitration performance is poor. Patent CN202110698018.3 discloses a SSZ-13 molecular sieve and its preparation method, and a Cu-SSZ-13 molecular sieve. Diatomaceous earth is used as a silicon source, and a chemical reagent aluminum source and a large amount of organic template are added to obtain a SSZ-13 molecular sieve. Further ion exchange is performed to obtain a Cu-SSZ-13 molecular sieve, which improves the high-temperature denitration performance, but requires the addition of a large amount of template.
[0005] The above patents have many limitations in application, such as high preparation cost, large acid consumption, large and uncontrollable amount of copper introduction, and complicated preparation. Therefore, it is of great significance to develop an environmentally friendly, low-cost, and easy-to-implement SSZ-13 molecular sieve catalyst synthesis route. Summary of the invention
[0006] According to the background problem, the problem to be solved by the present invention is:
[0007] The existing Cu-SSZ-13 molecular sieve has high preparation cost, uses a large amount of chemical reagents resulting in serious pollution, and has not improved the problem of easy deactivation at high temperature.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A method for preparing a Cu-SSZ-13 molecular sieve catalyst using natural minerals comprises the following steps:
[0010] (1) Thermally activating natural mineral silicon-aluminum sources to obtain activated natural silicon-aluminum minerals;
[0011] (2) Dispersing activated natural silica-alumina minerals uniformly into water to act as silicon and aluminum sources, with a thermal activation temperature of 600-850°C; adding an alkali source, an activator, and a template agent, stirring for 0.5-6 hours to obtain a reaction gel;
[0012] (3) transferring the reaction gel to a reactor containing a polytetrafluoroethylene liner, crystallizing at 140-170°C for 2-4 days, washing and drying the crystallized product, and calcining at 500-600°C for 3-6 hours to obtain SSZ-13 molecular sieve;
[0013] (4) exchanging the above SSZ-13 molecular sieve with solvent 1 for ammonium ions at a temperature of 70 to 90° C.; washing and drying to obtain an NH4-SSZ-13 molecular sieve catalyst;
[0014] (5) exchanging copper ions with the above NH4-SSZ-13 molecular sieve and solvent 2 at a temperature of 70-90°C; washing, drying and calcining at 500-600°C for 3-6h to obtain a Cu-SSZ-13 molecular sieve catalyst.
[0015] Preferably, the natural mineral silica-alumina source in step (1) is one or more of montmorillonite, kaolin, diatomaceous earth and bentonite; and the activated natural silica-alumina mineral is one or more of metamontmorillonite, metakaolin, metadiatomaceous earth and metabentonite.
[0016] Preferably, the alkali source in step (2) is one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide and cesium hydroxide.
[0017] Preferably, the activator in step (2) is one or more of rare earth chloride, rare earth nitrate, rare earth sulfate, and sodium tungstate.
[0018] Preferably, the template agent in step (2) is one or more of triethylamine, ethylenediamine, N,N,N-trimethyl-1-adamantanammonium hydroxide, and tetraethylammonium hydroxide.
[0019] Preferably, the amount of each substance added to the reaction gel in step (3) satisfies the following molar ratio conditions: 0.001~0.5MO / 1SiO2 / 0.005~0.5Al2O3 / 0.1~0.16Na2O / 44~66H2O / 0.001~0.2 template, and the MO matrix comes from the activator.
[0020] Preferably, the crystallization method in step (3) is static crystallization or dynamic crystallization.
[0021] Preferably, in step (4), solvent 1 is one or more of ammonium nitrate solution, ammonium sulfate solution, ammonium acetate solution and ammonium chloride solution; and the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:20-50.
[0022] Preferably, in step (5), solvent 2 is one or more of copper nitrate solution, copper sulfate solution and copper acetate solution; and the mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 is 1:5-50.
[0023] The beneficial effects of the present invention are:
[0024] (1) Use natural minerals such as montmorillonite, kaolin, diatomaceous earth, bentonite, etc. as silicon sources and aluminum sources, without using additional conventional chemical reagents as silicon sources and aluminum sources, saving preparation costs and being environmentally friendly.
[0025] (2) Using a low amount of template and adding an alkali source as a mineralizer can still achieve good crystallinity and exhibit excellent denitrification performance and nitrogen selectivity, greatly reducing the use of toxic templates and reducing environmental pollution caused by the calcination process.
[0026] (3) Natural minerals contain some Fe and Ti elements, which have a significant effect on the high-temperature denitrification performance of the catalyst, eliminating the ion exchange step and saving resources and time costs.
[0027] (4) The synthesized molecular sieve has high crystallinity and a regular cubic morphology with a smooth surface. Compared with small particles and lamellar morphology, its advantage is that it has more outstanding hydrothermal stability.
[0028] (5) The amount of copper introduced is controllable and easy to adjust. Compared with adding copper in one step during crystallization, the present invention has a more flexible amount of copper introduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 X-ray diffraction spectra of samples of Examples 1 to 5 and Comparative Examples 1 to 2 of the present invention
[0030] Figure 2 Scanning electron microscope images of samples of Example 1 (a) and Comparative Example 1 (b) of the present invention
[0031] Figure 3 The denitration performance diagram of the samples of Example 1 and Comparative Example 1 of the present invention DETAILED DESCRIPTION
[0032] Example 1
[0033] A method for preparing a Cu-SSZ-13 molecular sieve catalyst using natural minerals comprises the following steps:
[0034] (1) Add 5.02 g of diatomaceous earth thermally activated at 800 °C to 69 mL of deionized water, add 5.28 g of kaolin thermally activated at 800 °C, add 0.031 g of rare earth sulfate, add 0.52 g of sodium hydroxide, stir for 1.5 h, add 0.07 g of template N,N,N-trimethyl-1-adamantane ammonium hydroxide solution (N,N,N-trimethyl-1-adamantane ammonium hydroxide mass fraction is 25%), stir for 1 h to obtain a reactant gel.
[0035] (2) The gel was transferred to a polytetrafluoroethylene liner, placed in a hydrothermal reactor, and dynamically crystallized at 140°C for 2 days. After filtration and drying, the SSZ-13 molecular sieve was obtained after calcination at 500°C in a muffle furnace for 6 hours. The amount of each substance added in the reaction gel met the following molar ratio conditions: 0.2MO / 1SiO2 / 0.26Al2O3 / 0.1Na2O / 50H2O / 0.001 template.
[0036] (3) Add 2 g of SSZ-13 molecular sieve to 50 mL of deionized water, stir evenly, add 5.349 g of ammonium chloride, exchange in a water bath at 80 °C for 2 h, filter, and dry to obtain NH4-SSZ-13; the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:27.67.
[0037] (4) 1.5 g of NH4-SSZ-13 molecular sieve was added to 50 mL of deionized water, and 0.11 g of copper nitrate was added. The mixture was exchanged in a water bath at 80 °C for 2 h, filtered, dried, and calcined at 550 °C for 5 h to obtain a Cu-SSZ-13 molecular sieve catalyst; wherein the mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 was 1:33.4.
[0038] Example 2
[0039] A method for preparing a Cu-SSZ-13 molecular sieve catalyst using natural minerals comprises the following steps:
[0040] (1) Add 5.02 g of diatomaceous earth thermally activated at 850 °C to 61 mL of deionized water, add 0.1 g of kaolin thermally activated at 850 °C, add 0.0002 g of rare earth sulfate, add 0.52 g of sodium hydroxide, stir for 0.3 h, add 13.5 g of template N,N,N-trimethyl-1-adamantane ammonium hydroxide solution (N,N,N-trimethyl-1-adamantane ammonium hydroxide mass fraction is 25%), stir for 0.5 h to obtain a reactant gel.
[0041] (2) The gel was transferred to a polytetrafluoroethylene liner, placed in a hydrothermal reactor, and dynamically crystallized at 150°C for 2 days. After filtration and drying, the SSZ-13 molecular sieve was obtained after calcination at 600°C in a muffle furnace for 4 hours. The amount of each substance added in the reaction gel met the following molar ratio conditions: 0.001MO / 1SiO2 / 0.005Al2O3 / 0.1Na2O / 44H2O / 0.2template.
[0042] (3) Add 1.5 g of SSZ-13 molecular sieve to 27 mL of deionized water, stir evenly, add 3.02 g of ammonium chloride, exchange in a 90 °C water bath for 2 h, filter, and dry to obtain NH4-SSZ-13; the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:20.
[0043] (4) 1.0 g of NH4-SSZ-13 molecular sieve was added to 20 mL of deionized water, and 0.05 g of copper nitrate was added. The mixture was exchanged in a water bath at 90 °C for 2.5 h, rotary evaporated to dryness, and calcined at 550 °C for 5 h to obtain a Cu-SSZ-13 molecular sieve catalyst; wherein the mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 was 1:20.
[0044] Example 3
[0045] A method for preparing a Cu-SSZ-13 molecular sieve catalyst using natural minerals comprises the following steps:
[0046] (1) Add 5.02 g of diatomaceous earth thermally activated at 600 °C to 71 mL of deionized water, add 0.4 g of kaolin thermally activated at 600 °C, add 0.016 g of rare earth sulfate, add 0.55 g of sodium hydroxide, stir for 5 h, add 6.1 g of template N,N,N-trimethyl-1-adamantanammonium hydroxide solution (N,N,N-trimethyl-1-adamantanammonium hydroxide mass fraction is 25%), stir for 1 h to obtain a reactant gel.
[0047] (2) The gel was transferred to a polytetrafluoroethylene liner, placed in a hydrothermal reactor, and statically crystallized at 170°C for 4 days. After filtration and drying, the SSZ-13 molecular sieve was obtained after calcination at 500°C in a muffle furnace for 5 hours. The amount of each substance added in the reaction gel met the following molar ratio conditions: 0.09MO / 1SiO2 / 0.02Al2O3 / 0.11Na2O / 60H2O / 0.09 template.
[0048] (3) Add 1 g of SSZ-13 molecular sieve to 45 mL of deionized water, stir evenly, add 4.99 g of ammonium chloride, exchange in a water bath at 80 °C for 2 h, filter, and dry to obtain NH4-SSZ-13; the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:50.
[0049] (4) Add 1.0 g of NH4-SSZ-13 molecular sieve to 5 mL of deionized water, add 0.08 g of copper sulfate pentahydrate, exchange in a water bath at 75°C for 2 h, rotary evaporate to dryness, and calcine at 550°C for 4 h to obtain a Cu-SSZ-13 molecular sieve catalyst; wherein the mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 is 1:5.
[0050] Example 4
[0051] A method for preparing a Cu-SSZ-13 molecular sieve catalyst using natural minerals comprises the following steps:
[0052] (1) Add 5.02 g of diatomaceous earth thermally activated at 800 °C to 62 mL of deionized water, add 4.67 g of kaolin thermally activated at 800 °C, add 0.029 g of rare earth sulfate, add 0.68 g of sodium hydroxide, stir for 1.5 h, add 0.07 g of template N,N,N-trimethyl-1-adamantane ammonium hydroxide solution (N,N,N-trimethyl-1-adamantane ammonium hydroxide mass fraction is 25%), stir for 0.5 h to obtain a reactant gel.
[0053] (2) The gel was transferred to a polytetrafluoroethylene liner, placed in a hydrothermal reactor, and dynamically crystallized at 160°C for 2 days. After filtration and drying, the SSZ-13 molecular sieve was obtained after calcination at 500°C in a muffle furnace for 3 hours. The amount of each substance added in the reaction gel met the following molar ratio conditions: 0.19MO / 1SiO2 / 0.23Al2O3 / 0.13Na2O / 55H2O / 0.001 template.
[0054] (3) Add 1.5 g of SSZ-13 molecular sieve to 45 mL of deionized water, stir evenly, add 4.81 g of ammonium chloride, exchange in a water bath at 80 °C for 2 h, filter, and dry to obtain NH4-SSZ-13; the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:27.67.
[0055] (4) 1.0 g of NH4-SSZ-13 molecular sieve was added to 50 mL of deionized water, and 0.06 g of copper acetate was added. The mixture was exchanged in a water bath at 85°C for 2 h, and then rotary evaporated to dryness. The mixture was calcined at 550°C for 6 h to obtain a Cu-SSZ-13 molecular sieve catalyst. The mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 was 1:50.
[0056] Example 5
[0057] A method for preparing a Cu-SSZ-13 molecular sieve catalyst using natural minerals comprises the following steps:
[0058] (1) Add 5.02 g of diatomaceous earth thermally activated at 800 °C to 60 mL of deionized water, add 1.02 g of kaolin thermally activated at 800 °C, add 0.05 g of rare earth sulfate, add 0.68 g of sodium hydroxide, stir for 1.5 h, add 3.4 g of template N,N,N-trimethyl-1-adamantanammonium hydroxide solution (N,N,N-trimethyl-1-adamantanammonium hydroxide mass fraction is 25%), and stir for 6 h to obtain a reactant gel.
[0059] (2) The gel was transferred to a polytetrafluoroethylene liner, placed in a hydrothermal reactor, and statically crystallized at 170°C for 3 days. After filtration and drying, the SSZ-13 molecular sieve was obtained after calcination at 500°C in a muffle furnace for 4 hours. The amount of each substance added in the reaction gel met the following molar ratio conditions: 0.33MO / 1SiO2 / 0.05Al2O3 / 0.13Na2O / 52H2O / 0.05 template.
[0060] (3) Add 2 g of SSZ-13 molecular sieve to 60 mL of deionized water, stir evenly, add 6.42 g of ammonium chloride, exchange in a 70°C water bath for 2 h, filter, and dry to obtain NH4-SSZ-13; the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:27.67.
[0061] (4) Add 1.5 g of NH4-SSZ-13 molecular sieve to 15 mL of deionized water, stir evenly, add 0.04 g of anhydrous cupric chloride, exchange in a 70 °C water bath for 2 h, rotary evaporate to dryness, and calcine at 550 °C for 5 h to obtain a Cu-SSZ-13 molecular sieve catalyst; wherein the mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 is 1:33.4.
[0062] Comparative Example 1
[0063] The SSZ-13 molecular sieve is prepared by the patent CN201811354909.1 method, including the following steps:
[0064] Weigh 2.79 g of activated rectorite and 4.04 g of sodium hydroxide and dissolve them in 50 g of deionized water, add 6.5 g of tetraethylenepentamine dropwise, stir for 5 min, add 6.7 g of activated black copper ore, stir for 1 h, add 8.08 g of diatomaceous earth, add 1.2 g of sulfuric acid to adjust the pH to 11, then place in a water bath at 70 ° C for 4 h, then cool to room temperature, add 1.3 g of sulfuric acid to adjust the pH to 10, and mix and stir at 35 ° C for 4 h.
[0065] The mixture was poured into a stainless steel crystallization kettle lined with polytetrafluoroethylene, and the temperature was raised to 140°C for static crystallization for 72 hours. After the crystallization was completed, the mixture was cooled, filtered to remove the mother liquor, washed to neutrality, and dried at 120°C to obtain a sodium Fe-Cu-SSZ-13 molecular sieve product.
[0066] The sodium Fe-Cu-SSZ-13 molecular sieve was exchanged with 0.2 mol / L nitric acid at 80°C for 6 hours, the mother liquor was filtered out, the filter cake was washed with deionized water until neutral, and dried to obtain the hydrogen Fe-Cu-SSZ-13 molecular sieve.
[0067] Comparative Example 2
[0068] The SSZ-13 molecular sieve is prepared by the patent CN202311640112.9 method, including the following steps:
[0069] (1) According to the conventional method, a certain amount of alkali, template, deionized water, silicon aluminum source, etc. are mixed uniformly at a certain temperature, the gel is transferred to a hydrothermal kettle, crystallized at a certain temperature, and the crystallized product is washed, dried and calcined to obtain SSZ-13 seed crystals.
[0070] (2) 0.22 g potassium hydroxide, 0.31 g sodium hydroxide and 45 g deionized water were stirred evenly, and then 0.58 g sub-molten salt activated kaolin was added and mixed evenly, followed by adding 1.35 g of supplementary silicon source white carbon black and continuing to stir, adding 0.15 g SSZ-13 seed crystals and continuing to stir for 4 h. The gel was transferred to a hydrothermal autoclave with a polytetrafluoroethylene liner and crystallized at 170 °C for 1.5 days. After the crystallization was completed, the solid product was washed with deionized water until neutral and then dried to obtain SSZ-13 molecular sieve.
[0071] (3) At 80°C, the dried SSZ-13 was ion exchanged with a 1 mol / L aqueous solution of ammonium chloride at a solid-liquid mass ratio of 1:100 for three times, with each exchange time being 2 h. After washing, drying, and calcination, H-SSZ-13 was obtained.
[0072] (4) At 80°C, H-SSZ-13 was ion exchanged twice with a 0.1 mol / L copper nitrate aqueous solution at a solid-liquid mass ratio of 1:50, with each exchange lasting 2 h. After washing, drying, and calcination, Cu-SSZ-13 was obtained.
[0073] The specific embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the scope of the present invention, the technical solution of the present invention can be further modified and combined, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
[0074] X-ray diffraction spectrum of the catalyst
[0075] The structures of Examples 1 to 5 and Comparative Examples 1 to 2 were characterized using a Bruker D8 Advance X-ray diffractometer. Figure 1 As shown, the examples all present a pure CHA phase structure with good crystallinity, while the comparative examples have a CHA phase structure but poor crystallinity.
[0076] SEM image of catalyst
[0077] The morphology of Example 1 and Comparative Example 1 was characterized using a Hitachi S-4800 scanning electron microscope. Figure 2 As shown, Example 1 presents a regular cubic shape, the particles are clear, the morphology is complete, and the surface is smoother and flatter, while Comparative Example 1 is in an irregular stacking state.
[0078] Catalyst denitrification performance test
[0079] The denitrification activity of the prepared samples was measured under simulated flue gas conditions using a fixed bed apparatus. Argon was used as the balance gas, and the flue gas simulated in Examples 1 to 5 and Comparative Example 1 entered a quartz tube reactor with an inner diameter of 8 mm at a total flow rate of 600 mL / min, and the flue gas simulated in Comparative Example 2 entered a quartz tube reactor with an inner diameter of 8 mm at a total flow rate of 400 mL / min. The treated gas was collected and the NO concentration was detected using a flue gas analyzer. The specific reaction conditions and nitrogen oxide conversion rate are shown in Table 1.
[0080]
[0081] Table 1 Denitration reaction conditions and nitrogen oxide conversion rates of the examples and comparative examples
[0082] As shown in Table 1, under the same feed gas and mass space velocity, the results of the denitration performance test using the embodiments are better than those of the comparative examples. Among them, embodiments 1 to 4 can achieve a nitrogen oxide conversion rate of more than 90% in a wide temperature window of 150 to 550°C, and embodiment 5 can achieve a nitrogen oxide conversion rate of more than 90% in a temperature window of 120 to 600°C. Figure 3 It can be seen that Example 1 can also achieve a nitrogen oxide conversion rate of 87% at 600°C, indicating that the example uses natural minerals as silicon-aluminum sources, and the elements such as Fe and Ti contained therein directly play a role in improving the catalytic activity in the high temperature region (400~600°C). In Comparative Example 1, Fe-Cu-SSZ-13 is synthesized by a one-step method, and the amount of copper introduced during crystallization is large and uncontrollable. In subsequent performance tests, the window in which a conversion rate of more than 90% can be achieved is only 200~400°C, and its maximum catalytic effect cannot be exerted. In actual production, this comparative example requires a large amount of acid consumption, causing serious environmental pollution and difficulties in waste liquid treatment. Comparative Example 2 only achieves a nitrogen oxide conversion rate of more than 90% at 150~400°C.
Claims
1. An application of a Cu-SSZ-13 molecular sieve catalyst in denitration, characterized in that: The preparation steps include: (1) Thermally activating natural mineral silicon-aluminum sources to obtain activated natural silicon-aluminum minerals; (2) Dispersing activated natural silica-alumina minerals uniformly into water to act as silicon and aluminum sources, with a thermal activation temperature of 600-850°C; adding an alkali source, an activator, and a template agent, stirring for 0.5-6 hours to obtain a reaction gel; (3) transferring the reaction gel to a reactor containing a polytetrafluoroethylene liner, crystallizing at 140-170°C for 2-4 days, washing and drying the crystallized product, and calcining at 500-600°C for 3-6 hours to obtain SSZ-13 molecular sieve; (4) exchanging the above SSZ-13 molecular sieve with solvent 1 for ammonium ions at a temperature of 70 to 90° C.; washing and drying to obtain NH4-SSZ-13 molecular sieve; (5) exchanging the NH4-SSZ-13 molecular sieve with solvent 2 for copper ions at a temperature of 70 to 90° C.; washing, drying and calcining at 500 to 600° C. for 3 to 6 hours to obtain a Cu-SSZ-13 molecular sieve catalyst; The activator in step (2) is one or more of rare earth chloride, rare earth nitrate, and rare earth sulfate; The amount of each substance added to the reaction gel in step (3) satisfies the following molar ratio conditions: 0.001~0.5MO / 1SiO2 / 0.005~0.5Al2O3 / 0.1~0.16Na2O / 44~66H2O / 0.001~0.2 template, and the MO matrix comes from the activator.
2. The use of a Cu-SSZ-13 molecular sieve catalyst in denitration according to claim 1, characterized in that: The natural mineral silica-aluminum source in step (1) is one or more of montmorillonite, kaolin, diatomaceous earth and bentonite; the activated natural silica-aluminum mineral is one or more of metamontmorillonite, metakaolin, metadiatomaceous earth and metabentonite.
3. The use of a Cu-SSZ-13 molecular sieve catalyst in denitration according to claim 1, characterized in that: The alkali source in step (2) is one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide and cesium hydroxide.
4. The use of a Cu-SSZ-13 molecular sieve catalyst in denitration according to claim 1, characterized in that: The template agent in step (2) is one or more of triethylamine, ethylenediamine, N,N,N-trimethyl-1-adamantanammonium hydroxide, and tetraethylammonium hydroxide.
5. The use of a Cu-SSZ-13 molecular sieve catalyst in denitration according to claim 1, characterized in that: The crystallization method in step (3) is static crystallization or dynamic crystallization.
6. The use of a Cu-SSZ-13 molecular sieve catalyst in denitration according to claim 1, characterized in that: In step (4), the solvent 1 is one or more of ammonium nitrate solution, ammonium sulfate solution, ammonium acetate solution and ammonium chloride solution; and the mass ratio of SSZ-13 molecular sieve to solvent 1 is 1:20-50.
7. The use of a Cu-SSZ-13 molecular sieve catalyst in denitration according to claim 1, characterized in that: In step (5), solvent 2 is one or more of copper nitrate solution, copper sulfate solution and copper acetate solution; the mass ratio of NH4-SSZ-13 molecular sieve to solvent 2 is 1:5-50.