A high heat insulation and high light transmittance PET optical film and preparation method thereof

By using a combination of PET resin, heat-insulating masterbatch and high-transmittance coating in the PET film, combined with specific process processing, the problem of insufficient heat insulation and light-transmittance performance of the existing PET film is solved, and high heat insulation and high transmittance are achieved. The effect of light is suitable for fields such as optical instruments.

CN118374041BActive Publication Date: 2024-10-18NINGBO JIUXIN NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410612560.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-10-18
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Existing PET films have deficiencies in thermal insulation and light transmission properties. In particular, the film raw materials are complex and the preparation cost is high, and the light transmittance needs to be further improved.

Method used

Using a combination of PET resin, thermal insulation masterbatch, light stabilizer, slippery agent, dispersant and high-transparency coating, the thermal insulation masterbatch and high-transmission coating are prepared and coated on the film, combined with specific Process treatments such as melting, stretching and hot press shaping optimize the structure and performance of the film.

Benefits of technology

The thermal insulation and light transmittance of PET film are significantly improved, and it is suitable for optical instruments and other fields, and the process is simple and easy to operate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118374041B_ABST
    Figure CN118374041B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-insulation and high-light-transmittance PET optical film, which includes the following components in mass percentage: 60-80% PET resin, 10-20% heat-insulating masterbatch, 0.5-2% light stabilizer, 0.1-0.5% lubricant, 0.5-5% dispersant, 1-5% antioxidant and 7.5-8% light-transmitting coating. The present application prepares the heat-insulating masterbatch by a suitable ratio of raw materials and a specific method, and then uses the heat-insulating masterbatch as a raw material to prepare a PET film, which can significantly improve the heat resistance of the PET film; in addition, the light transmittance of the PET film is enhanced by preparing the high-light-transmitting coating and coating it on the film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a high-heat-insulating and high-light-transmittance PET optical film and a preparation method thereof. Background Art

[0002] With the rapid development of display technology, solar energy utilization, optical instruments and other fields, the requirements for the light transmittance of optical films are increasing day by day. PET film, as a common polymer material, is widely used due to its good mechanical properties and processing properties. However, the heat insulation and light transmittance of traditional PET film still need to be improved, especially the film exposed outdoors has very poor heat insulation effect, and in the high-band spectral range, its light transmittance is limited by the refractive index and scattering characteristics of the material.

[0003] Patent CN202111611287.8 discloses a method and system for preparing a high-temperature resistant PET film, which is prepared from the following raw materials by mass: polyethylene terephthalate, polyethylene, unsaturated aliphatic polyester, SEBS, polyurethane dispersion, film-forming aid, high-temperature nylon, light and heat stabilizer, antioxidant, Huamingtai calcium stearate, Jinling calcium stearate, coupling agent, polypropylene, silicon carbide and calcium sulfate, and the mixture of high-temperature resistant PET polyester particles and masterbatch slices is melted and plasticized, the pre-treated sheet is longitudinally and transversely stretched, and the high-temperature resistant PET film is rolled up. The prepared high-temperature resistant PET film is smooth, high in clarity and gloss, has excellent physical properties, chemical properties and dimensional stability, transparency, recyclability, and has excellent heat resistance, cold resistance, good chemical resistance and oil resistance, so as to improve the performance of the high-temperature resistant PET film. Although the film disclosed in the patent can withstand a certain high temperature, the preparation materials of the film are complex and the cost is high.

[0004] Patent CN202311858018.0 discloses a slow-release anti-fog high-transmittance PET film and a preparation method thereof, which sequentially include: 1) a PET base film layer; 2) a first anti-fog layer, the raw materials include: a base resin A, an anti-fog masterbatch A, and a nucleating agent; 3) a slow-release layer, the raw materials include: a base resin B, an anti-fog masterbatch B; 4) a second anti-fog layer, the raw materials include: a PET resin, an anti-fog masterbatch C, and a nucleating agent; wherein the anti-fog masterbatch A, the anti-fog masterbatch B and the anti-fog masterbatch C are obtained by mixing and granulating an anti-fog agent with a ternary polyester; the weight of the anti-fog masterbatch A, the anti-fog masterbatch B and the anti-fog masterbatch C respectively accounts for 5-20% of the total weight of the layer in which they are located, and the anti-fog agent content in the first anti-fog layer and the anti-fog agent content in the slow-release layer are both greater than the anti-fog agent content in the second anti-fog layer; the high-transmittance PET film is prepared by four-layer co-extrusion, with a thickness of less than 100 μm, a transmittance of more than 85%, and a haze of less than 5%. Although the PET film provided by this patent has a double-layer effect of light transmittance and anti-fog, its light transmittance needs to be further improved during actual use.

[0005] Therefore, developing a new type of PET film with high thermal insulation and high light transmittance is of great significance to improving the product quality and technical level of related industries. Summary of the invention

[0006] The purpose of the present invention is to provide a high-insulation and high-light-transmittance PET optical film and a preparation method thereof, so as to solve the problems of the existing PET film in that the film raw materials are complex, the preparation cost is high and the light transmittance needs to be further improved.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A high-insulation and high-light-transmittance PET optical film comprises the following components in percentage by mass: 60-80% of PET resin, 10-20% of heat-insulation masterbatch, 0.5-2% of light stabilizer, 0.1-0.5% of lubricant, 0.5-5% of dispersant, 1-5% of antioxidant and 7.5-8% of high-light-transmittance coating.

[0009] Further, the light stabilizer is selected from one of a shielding agent, an absorbent and a free radical scavenger;

[0010] The lubricant is selected from any one of amide compounds, soap compounds or organosilicon compounds.

[0011] The antioxidant is selected from any one of tea polyphenols, tocopherol, flavonoids, butylated hydroxyanisole, butylated hydroxytoluene or tert-butylhydroquinone.

[0012] Further, the amide compound is oleamide or erucamide, the soap compound is calcium stearate, and the organosilicon compound is silicone;

[0013] The shielding agent is selected from any one of carbon black and titanium dioxide; the absorbent is selected from any one of benzophenone, salicylate and benzotriazole; and the free radical scavenger is selected from hindered amine light stabilizer.

[0014] Furthermore, the dispersant is polyethylene wax.

[0015] A method for preparing a high-thermal-insulation and high-light-transmittance PET optical film, the method comprising the following steps:

[0016] S1: Preparation of thermal insulation masterbatch: first prepare cesium tungstate powder, mix the prepared cesium tungstate powder with PET resin, silane coupling agent (here, the silane coupling agent is any one of vinyl silane, aminosilane, and methacryloxysilane) and dispersant, and stir evenly. The mixed material is fed into a twin-screw extruder. The material is heated, melted, sheared, mixed, devolatilized, and sheared again, and then extruded through the extruder die. The melt stream is cooled into a solid state through a water tank, dried by a hair dryer, and then cut into a pelletizer to make a thermal insulation masterbatch;

[0017] S2: Raw material pretreatment and film preparation, slicing the PET resin, weighing the raw materials for preparing the film, stirring and mixing, and then performing surface crystallization and drying treatment;

[0018] The film material components after drying are sent to a twin-screw extruder for melt extrusion to form a molten film, and then the molten film is cast on a cooling roller through a casting die for quenching to form a cast sheet, and then stretched and shaped transversely and longitudinally to obtain a film;

[0019] S3: Preparation of high light transmittance coating: polybutyl methacrylate, vinyl silsesquioxane, silicon dioxide, indium nitride, titanium dioxide and zinc oxide are mixed with an organic solvent ethylene glycol in a high-speed mixer to prepare a high light transmittance coating;

[0020] S4: applying a high light transmittance coating: placing the high light transmittance coating in a coating machine, heating the high light transmittance coating by the coating machine to activate it, and coating the activated high light transmittance coating on the surface of the film obtained in the above step S2 by the coating machine, and forming a high light transmittance layer after drying and curing;

[0021] S5: Post-processing: cutting and trimming the film dried in step S4, and rolling up the cut film to obtain a finished product of a high heat-insulating and high light-transmittance PET film.

[0022] Furthermore, the preparation of cesium tungstate powder in step S1 is as follows: cesium carbonate, tungsten trioxide and deionized water are placed in a high-speed mixer, stirred at a high speed at a temperature of 125 to 145° C., and water vapor is gradually evaporated to obtain powder; the obtained powder is then ground in a grinder, and then sieved with a 100-mesh sieve, and the sieved powder is placed in a tubular furnace, and heated at high temperature in a mixed atmosphere of 5% hydrogen and 95% nitrogen, and dark blue cesium tungstate powder is obtained after 1 hour.

[0023] Furthermore, the temperature of the surface crystallization in step S2 is 120-180° C., and the drying process is carried out in a vacuum drum dryer.

[0024] Furthermore, the extrusion temperature in step S2 is: 190°C-210°C-230°C-250°C-260°C-280°C, the longitudinal stretching is to preheat the cast sheet to 85°C-90°C, and longitudinally stretch it 3-3.5 times at this temperature, and the transverse stretching is to preheat the cast sheet to 95°C-100°C, the stretching temperature is 110°C-120°C, and the stretching ratio is 3.5-4 times.

[0025] Furthermore, the shaping in step S2 is as follows: the stretched film is placed in a shaping machine, the film passes through a hot roller for heat-pressing shaping, and the film after the heat-pressing shaping treatment passes through a cooling roller for cooling and shaping the film.

[0026] Furthermore, the activation temperature in step S4 is 30-40°C.

[0027] In step S3 or step S5, the surface of the prepared PET film is treated by plasma treatment, chemical etching or ultraviolet light irradiation, etc., so as to reduce its surface roughness and reduce diffuse reflection of light. In addition, according to actual needs, the thickness of the PET film can be controlled and adjusted by adjusting the process parameters in the film preparation step S3, such as melting temperature, extrusion speed, etc., so as to optimize its light transmission performance in different spectral ranges.

[0028] The beneficial effects of the present invention are:

[0029] 1. The present invention provides a high-insulation and high-light-transmittance PET optical film. The heat-insulating masterbatch is prepared by a suitable ratio of raw materials and a specific method. Then, the heat-insulating masterbatch is used as a raw material to prepare a PET film, which can significantly improve the heat resistance of the PET film. In addition, the light transmittance of the PET film is enhanced by preparing a high-light-transmittance coating and coating it on the film.

[0030] 2. The present invention provides a high-insulation and high-light-transmittance PET optical film, which uses indium nitride and zinc oxide in the high-light-transmittance coating at the same time, so that the light transmittance of the high-light-transmittance coating is enhanced. Finally, the film prepared by coating the high-light-transmittance coating on the PET film has excellent light transmittance, and the coating process is simple and easy to operate.

[0031] 3. The high heat-insulating and high light-transmittance PET optical film provided by the present invention is very suitable for promotion and application in the fields of optical instruments and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a schematic diagram of the process of preparing a high heat-insulating and high light-transmittance PET film according to Example 1 of the present invention;

[0033] Figure 2 This is a finished product picture of the high heat insulation and high light transmittance PET film prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The reagents and equipment used in the present invention are all known products or obtained by purchasing commercially available products, wherein PET is polyethylene terephthalate.

[0035] Example 1

[0036] S1: Preparation of thermal insulation masterbatch

[0037] Preparation of cesium tungstate powder: put 20% cesium carbonate powder, 75% tungsten trioxide light powder and 5% deionized water into a high-speed mixer according to the mass percentage, stir at a high speed at a temperature of 145°C, and let the water vapor evaporate gradually to obtain powder.

[0038] The obtained powder is then ground in a grinder, sieved with a 100-mesh screen, and the sieved powder is placed in a tubular furnace and heated at a high temperature of 530-550°C in a mixed atmosphere of 5% hydrogen and 95% nitrogen. After 1 hour, dark blue cesium tungstate powder can be obtained.

[0039] According to the mass percentage, 70% of the prepared cesium tungstate powder, 24% of the PET resin, 1% of the silane coupling agent KH560, and 5% of the polyethylene glycol PEG400 are respectively added into a high-speed mixer and stirred evenly at a high speed. The mixed materials are fed into an extruder. The materials are heated, melted, sheared and mixed in the extruder barrel and then extruded. The temperature of the extruder is set to: 180°C-200°C-210°C-220°C-240°C-260°C. The melt stream is cooled into a solid state through a water tank, dried by a hair dryer, and then enters a pelletizer to be cut into thermal insulation masterbatch.

[0040] S2: According to the mass percentage, 78% of PET resin, 10% of thermal insulation masterbatch, 0.5% of carbon black, 0.5% of oleic acid amide, 1.4% of polyethylene wax and 1.6% of tea polyphenols are fed into a mixer for stirring and mixing, and then the mixed raw materials are fed into a crystallizer for surface crystallization. The crystallization temperature is controlled at 160°C, and the crystallized raw materials are then placed in a vacuum drum dryer for drying.

[0041] The film material components after drying are sent to a twin-screw extruder for melt extrusion. The extruder temperature is set to 190℃-210℃-230℃-250℃-260℃-280℃ to form a molten film. The molten film is then cast on a cooling roller through a casting die for rapid cooling to form a cast sheet. The cooled cast sheet is placed in a stretching machine. The longitudinal stretching is to preheat the cast sheet to 90℃ and longitudinally stretch it 3 times at this temperature. The transverse stretching preheating temperature is 95℃, the stretching temperature is 110℃, and the stretching ratio is 4 times. The film is biaxially stretched by the stretching machine to form a film. The stretched film is placed in a setting machine. The film passes through a hot roller for hot pressing and setting. The film after hot pressing and setting passes through a cooling roller, and the film is cooled and set to obtain a film.

[0042] S3: Put 15% of polybutyl methacrylate, 20% of vinyl silsesquioxane, 15% of silicon dioxide, 15% of indium nitride, 10% of titanium dioxide and 15% of zinc oxide into a high-speed mixer according to the mass percentage, and mix them with 10% of organic solvent ethylene glycol to prepare a high light-transmitting coating.

[0043] S4: Put the high-light-transmittance coating into a coating machine, heat the high-light-transmittance coating to 30°C for activation, and apply the activated high-light-transmittance coating on the surface of the film prepared in the above step S2 by the coating machine. The mass percentage of the high-light-transmittance coating is 8%, and then dry and solidify it in a drying machine at 90-120°C to form a high-light-transmittance layer of the film.

[0044] S5: The film dried in step S4 is transported to a cutting machine for cutting and trimming, and the cut film is rolled up to obtain a high-insulation and high-light-transmittance PET film product.

[0045] The specific preparation process of high heat insulation and high light transmittance PET film is as follows Figure 1 As shown; Finally, the finished film of this embodiment is as shown Figure 2 As shown: Specifically, this is a picture of the prepared high-heat-insulating and high-light-transmittance PET film product placed on a brown table.

[0046] Example 2

[0047] S1: Preparation of thermal insulation masterbatch

[0048] Preparation of cesium tungstate powder: put 20% cesium carbonate powder, 75% tungsten trioxide light powder and 5% deionized water into a high-speed mixer according to the mass percentage, stir at a high speed at a temperature of 145°C, and let the water vapor evaporate gradually to obtain powder.

[0049] The obtained powder is then ground in a grinder, sieved with a 100-mesh screen, and the sieved powder is placed in a tubular furnace and heated at a high temperature of 530-550°C in a mixed atmosphere of 5% hydrogen and 95% nitrogen. After 1 hour, dark blue cesium tungstate powder can be obtained.

[0050] According to the mass percentage, 70% of the prepared cesium tungstate powder, 24% of the PET resin, 1% of the silane coupling agent KH560, and 5% of the dispersant polyethylene glycol PEG400 are respectively added into a high-speed mixer and stirred evenly at high speed. The mixed materials are fed into an extruder. The materials are heated, melted, sheared and mixed in the extruder barrel and then extruded. The temperature of the extruder is set to: 180°C-200°C-210°C-220°C-240°C-260°C. The melt stream is cooled into a solid state through a water tank, dried by a hair dryer, and then enters a pelletizer to be cut into thermal insulation masterbatch.

[0051] S2: According to the mass percentage, 60% of PET resin, 14% of thermal insulation masterbatch, 2% of benzophenone, 0.5% of erucamide, 5% of polyethylene wax and 1% of butylated hydroxyanisole are fed into a mixer for stirring and mixing, and then the mixed raw materials are fed into a crystallizer for surface crystallization. The crystallization temperature is controlled at 120°C, and the crystallized raw materials are then placed in a vacuum drum dryer for drying.

[0052] The film material components after drying are sent to a twin-screw extruder for melt extrusion. The extruder temperature is set to 190℃-210℃-230℃-250℃-260℃-280℃ to form a molten film. The molten film is then cast on a cooling roller through a casting die for quenching to form a cast sheet. The cooled cast sheet is placed in a stretching machine, and the longitudinal stretching is to preheat the cast sheet to 85℃, and longitudinally stretch it 3.5 times at this temperature. The transverse stretching preheating temperature is 100℃, the stretching temperature is 120℃, and the stretching ratio is 3.5 times. The film is biaxially stretched by the stretching machine to form a film. The stretched film is placed in a setting machine, and the film passes through a hot roller for hot pressing and setting. The film after hot pressing and setting treatment passes through a cooling roller, and the film is cooled and set to obtain a film.

[0053] S3: According to the mass fractions, 20% of polybutyl methacrylate, 18% of vinyl silsesquioxane, 18% of silicon dioxide, 12% of indium nitride, 10% of titanium dioxide and 12% of zinc oxide are mixed with 10% of organic solvent ethylene glycol in a high-speed mixer to prepare a highly light-transmitting coating.

[0054] S4: Put the high-light-transmittance coating into a coating machine, heat the high-light-transmittance coating to 35°C for activation, and coat the activated high-light-transmittance coating on the surface of the film prepared in the above step S2. The mass percentage of the high-light-transmittance coating is 7.5%. Then, the high-light-transmittance layer of the film is formed after drying and curing in a drying machine.

[0055] S5: The film dried in step S4 is transported to a cutting machine for cutting and trimming, and the cut film is rolled up to obtain a high-insulation and high-light-transmittance PET film product.

[0056] Example 3

[0057] S1: Preparation of thermal insulation masterbatch

[0058] Preparation of cesium tungstate powder: put 20% cesium carbonate powder, 75% tungsten trioxide light powder and 5% deionized water into a high-speed mixer according to the mass percentage, stir at a high speed at a temperature of 145°C, and let the water vapor evaporate gradually to obtain powder.

[0059] The obtained powder is then ground in a grinder, sieved with a 100-mesh screen, and the sieved powder is placed in a tubular furnace and heated at a high temperature of 530-550°C in a mixed atmosphere of 5% hydrogen and 95% nitrogen. After 1 hour, dark blue cesium tungstate powder can be obtained.

[0060] According to the mass percentage, 70% of the prepared cesium tungstate powder, 24% of the PET resin, 1% of the silane coupling agent KH560, and 5% of the dispersant polyethylene glycol PEG400 are respectively added into a high-speed mixer and stirred evenly at high speed. The mixed materials are fed into an extruder. The materials are heated, melted, sheared and mixed in the extruder barrel and then extruded. The temperature of the extruder is set to: 180°C-200°C-210°C-220°C-240°C-260°C. The melt stream is cooled into a solid state through a water tank, dried by a hair dryer, and then enters a pelletizer to be cut into thermal insulation masterbatch.

[0061] S2: According to the mass percentage, 70% of PET resin, 20% of thermal insulation masterbatch, 0.5% of di(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, 0.1% of silicone, 0.5% of polyethylene wax and 1% of tert-butylhydroquinone are fed into a mixer for stirring and mixing, and then the mixed raw materials are fed into a crystallizer for surface crystallization. The crystallization temperature is controlled at 120°C, and the crystallized raw materials are then placed in a vacuum drum dryer for drying.

[0062] The film material components after drying are sent to a twin-screw extruder for melt extrusion. The extruder temperature is set to 190℃-210℃-230℃-250℃-260℃-280℃ to form a molten film. The molten film is then cast on a cooling roller through a casting die for quenching to form a cast sheet. The cooled cast sheet is placed in a stretching machine, and the longitudinal stretching is to preheat the cast sheet to 85℃, and longitudinally stretch it 3.5 times at this temperature. The transverse stretching preheating temperature is 100℃, the stretching temperature is 120℃, and the stretching ratio is 4 times. The film is biaxially stretched by the stretching machine to form a film. The stretched film is placed in a setting machine, and the film passes through a hot roller for hot pressing and setting. The film after hot pressing and setting treatment passes through a cooling roller, and the film is cooled and set to obtain a film.

[0063] S3: Put 18% of polybutyl methacrylate, 15% of vinyl silsesquioxane, 20% of silicon dioxide, 12% of indium nitride, 12% of titanium dioxide and 13% of zinc oxide into a high-speed mixer according to the mass percentage, and mix them with 10% of organic solvent ethylene glycol to prepare a high-light-transmitting coating.

[0064] S4: Put the high-light-transmittance coating into a coating machine, heat the high-light-transmittance coating to 35°C for activation, and coat the activated high-light-transmittance coating on the surface of the film prepared in the above step S2 by the coating machine. The mass percentage of high light transmittance is 8%, and then dry and solidify it in a dryer to form a high-light-transmittance layer of the film.

[0065] S5: The film dried in step S4 is transported to a cutting machine for cutting and trimming, and the cut film is rolled up to obtain a finished product of a high heat-insulating and high light-transmittance PET film.

[0066] Example 4

[0067] S1: Preparation of thermal insulation masterbatch

[0068] Preparation of cesium tungstate powder: put 20% cesium carbonate powder, 75% tungsten trioxide light powder and 5% deionized water into a high-speed mixer according to the mass percentage, stir at a high speed at a temperature of 145°C, and let the water vapor evaporate gradually to obtain powder.

[0069] The obtained powder is then ground in a grinder, sieved with a 100-mesh screen, and the sieved powder is placed in a tubular furnace and heated at a high temperature of 530-550°C in a mixed atmosphere of 5% hydrogen and 95% nitrogen. After 1 hour, dark blue cesium tungstate powder can be obtained.

[0070] According to the mass percentage, 70% of the prepared cesium tungstate powder, 24% of the PET resin, 1% of the silane coupling agent KH560, and 5% of the dispersant polyethylene glycol PEG400 are respectively added into a high-speed mixer and stirred evenly at high speed. The mixed materials are fed into an extruder. The materials are heated, melted, sheared and mixed in the extruder barrel and then extruded. The temperature of the extruder is set to: 180°C-200°C-210°C-220°C-240°C-260°C. The melt stream is cooled into a solid state through a water tank, dried by a hair dryer, and then enters a pelletizer to be cut into thermal insulation masterbatch.

[0071] S2: According to the mass percentage, 70% of PET resin, 16% of thermal insulation masterbatch, 0.5% of salicylate, 0.1% of calcium stearate, 0.5% of polyethylene wax and 5% of tert-butylhydroquinone are fed into a mixer for stirring and mixing, and then the mixed raw materials are fed into a crystallizer for surface crystallization. The crystallization temperature is controlled at 120°C, and the crystallized raw materials are then placed in a vacuum drum dryer for drying.

[0072] The film material components after drying are sent to a twin-screw extruder for melt extrusion. The extruder temperature is set to 190℃-210℃-230℃-250℃-260℃-280℃ to form a molten film. The molten film is then cast on a cooling roller through a casting die for quenching to form a cast sheet. The cooled cast sheet is placed in a stretching machine, and longitudinal stretching is to preheat the cast sheet to 85℃, and longitudinally stretch it 3.5 times at this temperature. The transverse stretching preheating temperature is 100℃, the stretching temperature is 120℃, and the stretching ratio is 3 times. The film is biaxially stretched by the stretching machine to form a film. The stretched film is placed in a setting machine, and the film passes through a hot roller for hot pressing and setting. The film after hot pressing and setting passes through a cooling roller, and the film is cooled and set to obtain a film.

[0073] S3: According to the mass percentage, 20% of polybutyl methacrylate, 15% of vinyl silsesquioxane, 20% of silicon dioxide, 10% of indium nitride, 15% of titanium dioxide and 10% of zinc oxide are mixed with 10% of organic solvent ethylene glycol in a high-speed mixer to prepare a highly light-transmitting coating.

[0074] S4: Put the high-light-transmittance coating into a coating machine, heat the high-light-transmittance coating to 35°C for activation, and coat the activated high-light-transmittance coating on the surface of the film prepared in the above step S2 by the coating machine. The mass percentage of the high-light-transmittance coating is 8%, and then dry and solidify it in a dryer to form a high-light-transmittance layer of the film.

[0075] S5: The film dried in step S4 is transported to a cutting machine for cutting and trimming, and the cut film is rolled up to obtain a finished product of a high heat-insulating and high light-transmittance PET film.

[0076] Example 5 is the same as Example 1, except that in step S2 of Example 5, carbon black is replaced by carbon black and salicylate.

[0077] Comparative Example 1 is the same as Example 1, except that in step S1 of Comparative Example 1, the mass ratio of cesium tungstate powder, PET resin, silane coupling agent and dispersant is.

[0078] Comparative Example 2 is the same as Example 1, except that indium nitride is not added in step S3 of Comparative Example 2.

[0079] Comparative Example 3 is the same as Example 1, except that zinc oxide is not added in step S3 of Comparative Example 3.

[0080] Comparative Example 4 is the same as Example 1, except that indium nitride and zinc oxide are not added in step S3 of Comparative Example 4.

[0081] Comparative Example 5 is the same as Example 1, except that the ethylene glycol in step S3 of Comparative Example 4 is replaced by methanol.

[0082] Comparative Example 6 is the same as Example 1, except that in step S2 of Comparative Example 4, the PET resin is 51%, the thermal insulation masterbatch is 30%, the carbon black is 3%, the oleic acid amide is 1%, the polyethylene wax is 1%, and the tea polyphenols are 1%; in step S4, the mass percentage of the high light transmittance coating in the film after coating is 13%.

[0083] Film product performance test method:

[0084] Thermal insulation effect: Determination of infrared blocking rate

[0085] According to the method specified in 5.13 of GB / T2680-2021, the spectral transmittance, reflectance and film surface emissivity of the finished film are measured, the total solar infrared heat energy transmittance is calculated, and the total solar infrared heat energy blocking rate is calculated according to formula (1) and expressed as a percentage.

[0086] R=1-gm……(1)

[0087] In formula (1), R is the total solar infrared heat energy rejection rate; gm is the total solar infrared heat energy transmittance.

[0088] Test instrument: LAMBDA 1050+ UV-Vis-NIR spectrophotometer, PerkinElmer, USA.

[0089] Transmittance: Determination of visible light transmittance

[0090] Attach three finished films not less than 50mm×50mm to 3mm flat glass of the same size with a visible light transmittance of 95%±1% to make test specimens. Before the test, the specimens should be placed at a temperature of 15-25℃ and a humidity of 40%-80% for at least 24h. The spectral transmittance of 380nm~780nm should be measured according to the method specified in 5.1 of GB / T2680-2021, and the visible light transmittance should be calculated and expressed as a percentage. For products with explicit nominal values, calculate the difference between each measured value and the nominal value; for products without explicit nominal values, calculate the difference between each measured value and the average value.

[0091] Test instrument: LAMBDA 1050+ UV-Vis-NIR spectrophotometer, PerkinElmer, USA.

[0092] The finished films prepared in the above Examples 1-5 were respectively tested for heat insulation effect and light transmittance, and the specific test results are shown in Table 1 below.

[0093] Table 1

[0094] Test items Example 1 Example 2 Example 3 Example 4 Example 5 Infrared blocking rate 90.5% 94.3% 93.1% 96.9% 91.5% Visible light transmittance 92.3% 95.6% 92.1% 96.5% 93.8%

[0095] In order to explore the effects of films prepared under different conditions on thermal insulation effect and light transmittance, the test results of specific comparative examples 1-6 are shown in Table 2 below.

[0096] Table 2

[0097] Test items Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Infrared blocking rate 90.5% 81.4% 91.4% 90.2% 92.1% 91.9% 85.7% Visible light transmittance 92.3% 91.6% 87.3% 84.7% 83.5% 90.1% 88.2%

[0098] As shown in Table 2 above, by changing the mass ratio of each component in the thermal insulation masterbatch, the infrared blocking rate of the film finally prepared is reduced, which indicates that the thermal insulation effect of the film is also reduced. In addition, by not adding indium nitride or zinc oxide to the high-transmittance coating, or by not adding both, or by replacing ethylene glycol with methanol, the visible light transmittance of the high-transmittance coating finally prepared when applied to the film is reduced, and the transmittance performance is deteriorated.

[0099] In order to verify whether increasing the proportion of light-transmitting coating will enhance its light-transmitting effect, it was found from the test results of Comparative Example 6 that the visible light transmittance and infrared blocking rate of the film finally prepared were reduced, and the light-transmitting effect and heat-insulating effect were both worse. This also shows that it is not necessary to increase the amount of light-transmitting coating to increase the light-transmitting effect, and the corresponding amount needs to be controlled.

Claims

1. A high heat insulation and high light transmittance PET optical film, characterized in that: The film comprises the following components in percentage by mass: 60-80% PET resin, 10-20% heat insulation masterbatch, 0.5-2% light stabilizer, 0.1-0.5% lubricant, 0.5-5% dispersant, 1-5% antioxidant and 7.5-8% high light transmittance coating; The method for preparing the high heat-insulating and high light-transmittance PET optical film comprises the following steps: S1: Preparation of thermal insulation masterbatch: first prepare cesium tungstate powder, mix the prepared cesium tungstate powder with PET resin, silane coupling agent and dispersant, and stir evenly. The mixed material is fed into a twin-screw extruder. The material is heated, melted, sheared, mixed, devolatilized, and sheared again, and then extruded through the extruder die. The melt stream is cooled into a solid state through a water tank, dried by a hair dryer, and then cut into a pelletizer to make thermal insulation masterbatch; The silane coupling agent is silane coupling agent KH560, the dispersant is polyethylene glycol PEG400, and the mass percentages of cesium tungstate powder, PET resin, silane coupling agent KH560 and polyethylene glycol PEG400 in the thermal insulation masterbatch are 70%, 24%, 1% and 5% respectively; S2: Raw material pretreatment and film preparation: After the PET resin and the raw materials for preparing the film are stirred and mixed, surface crystallization and drying are performed; The dried film material components are sent to a twin-screw extruder for melt extrusion to form a molten film, and then the molten film is cast on a cooling roller through a casting die for quenching to form a cast sheet, and then stretched transversely and longitudinally and shaped to obtain a film; S3: Preparation of high light transmittance coating: Put polybutyl methacrylate, vinyl silsesquioxane, silicon dioxide, indium nitride, titanium dioxide and zinc oxide and organic solvent ethylene glycol into a high-speed mixer for mixing to prepare a high light transmittance coating; the mass percentages of polybutyl methacrylate, vinyl silsesquioxane, silicon dioxide, indium nitride, titanium dioxide and zinc oxide and organic solvent ethylene glycol are 20%, 15%, 20%, 10%, 15%, 10% and 10% respectively; S4: applying a high-light-transmittance coating: placing the high-light-transmittance coating in a coating machine, heating the high-light-transmittance coating by the coating machine to activate it, and coating the activated high-light-transmittance coating on the surface of the film obtained in the above step S2 by the coating machine, and forming a high-light-transmittance layer after drying and curing; S5: Post-processing: cutting and trimming the film dried in step S4, and rolling up the cut film to obtain a high-insulation and high-light-transmittance PET film finished product.

2. The optical film according to claim 1, characterized in that: The light stabilizer is selected from one of a shielding agent, an absorbent or a free radical trapping agent; The lubricant is selected from any one of amide compounds, soap compounds or organosilicon compounds; The antioxidant is selected from any one of tea polyphenols, tocopherol, flavonoids, butylated hydroxyanisole, butylated hydroxytoluene or tert-butylhydroquinone.

3. The optical film according to claim 2, characterized in that: The amide compound is oleamide or erucamide, the soap compound is calcium stearate, and the organosilicon compound is silicone; The shielding agent is selected from any one of carbon black and titanium dioxide, the absorbent is selected from any one of benzophenone, salicylate and benzotriazole, and the free radical scavenger is selected from hindered amine light stabilizer.

4. The optical film according to claim 1, characterized in that: The dispersant is polyethylene wax.

5. The optical film according to claim 1, characterized in that: Preparation of cesium tungstate powder in step S1: Put cesium carbonate, tungsten trioxide and deionized water into a high-speed mixer, stir at a high speed at a temperature of 125-145° C., and allow water vapor to evaporate gradually to obtain powder; The obtained powder is then ground in a grinder, and then sieved with a 100-mesh sieve. The sieved powder is placed in a tubular furnace and heated at high temperature in a mixed atmosphere of 5% hydrogen and 95% nitrogen. After 1 hour, dark blue cesium tungstate powder is obtained.

6. The optical film according to claim 1, characterized in that: The temperature of the surface crystallization in step S2 is 120-180° C., and the drying process is performed in a vacuum drum.

7. The optical film according to claim 1, characterized in that: The extrusion temperature in step S2 is: 190°C-210°C-230°C-250°C-260°C-280°C, the longitudinal stretching is to preheat the cast sheet to 85°C-90°C, and longitudinally stretch it 3-3.5 times at this temperature, and the transverse stretching is to preheat the cast sheet to 95°C-100°C, the stretching temperature is 110°C-120°C, and the stretching ratio is 3.5-4 times.

8. The optical film according to claim 1, characterized in that: The shaping in step S2 is as follows: the stretched film is placed in a shaping machine, the film passes through a hot roller to be heat-pressed and shaped, and the film after the heat-pressed shaping treatment passes through a cooling roller to be cooled and shaped.

9. The optical film according to claim 1, characterized in that: The activation temperature in step S4 is 30-40°C.

Citation Information

Patent Citations

  • Preparation method and system of high-temperature-resistant PET (Polyethylene Terephthalate) film

    CN114262504A

  • Slow-release antifogging high-transmittance PET (polyethylene terephthalate) film and preparation method thereof

    CN117774476A

  • High-heat-insulation, ultraviolet-isolation and transparent colored master batch and preparation method thereof

    CN103435982A

  • Transparent colored heat and ultraviolet insulation film and preparation method thereof

    CN103435983A

  • PET composite film with multi-layer structure and preparation method of PET composite film

    CN111114060A