Dust suppression material with double network reinforced structure and preparation method thereof

By forming a dual network structure in dust inhibitors and using the combined technology of cross-linking and oxidation reaction, the problems of single function and difficult degradation of traditional dust inhibitors are solved, and efficient and environmentally friendly dust-repressing effects are achieved to meet the environmental needs of coal mines. .

CN118374064BActive Publication Date: 2024-12-03SHANDONG UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410550509.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-06
Publication Date
2024-12-03
Estimated Expiration
2044-05-06

AI Technical Summary

Technical Problem

Traditional chemical dust inhibitors have single functions and are difficult to degrade, resulting in weak mechanical properties and easy to cause secondary pollution.

Method used

Dual-network reinforced structure dust suppression material is used to form a composite dust suppressant through the combination of Tianjing gum, polyacrylamide, carboxymethylcellulose, crosslinking agent, oxidizing agent, water retention agent and wetting agent, and crosslinking and oxidation are used. The reaction forms a tight dual network structure to enhance dust suppression performance.

Benefits of technology

Improve the hydrophilicity, adhesion and anti-interference ability of dust inhibitors, form a dense protective film, significantly improve the dust suppression rate of dust, meet the needs of underground coal mining and open-pit coal pile yards, and avoid secondary pollute.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118374064B_ABST
    Figure CN118374064B_ABST
Patent Text Reader

Abstract

The present invention discloses a double network reinforced structure dust suppression material and a preparation method thereof, which relates to the technical field of dust control, and comprises the following raw materials in parts by weight: 0.1-0.5 parts of sesbania gum, 0.1-0.9 parts of polyacrylamide, 0.1-0.5 parts of carboxymethyl cellulose, 0.06-0.14 parts of a cross-linking agent, 0.11-0.19 parts of an oxidant, 0.1-0.3 parts of a water retaining agent, 0.2-1 parts of a wetting agent, and the balance being distilled water. The double network reinforced structure dust suppressant prepared by the present invention can effectively improve the hydrophilicity and adhesion of dust, and can form a dense protective film on the surface of dust. Tests have shown that the water retention of the dust suppressant prepared by the present invention is 36.0% higher than that of water, and has a high resistance to PM 10 The dust suppression rate reaches 98.67%. It has high dust suppression efficiency, high permeability, and high crust strength. It meets the requirements of underground coal mining operations and open-air coal stacking sites for the adhesion and wettability of dust suppressants, and will not cause secondary pollution to the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dust control, and in particular to a dust suppression material with a double network reinforced structure and a preparation method thereof. Background Art

[0002] At present, in the process of coal dust control, chemical dust suppressants have received widespread attention due to their good dust suppression effects. Dust suppressants have shifted from single type to composite and special type. Traditional single type dust suppressants include wetting type, bonding type, and hygroscopic type, while composite dust suppressants have multiple functions of wetting, bonding, and solidification, but have shortcomings such as weak mechanical properties, difficult degradation, and easy to cause secondary pollution.

[0003] Therefore, there is an urgent need to develop an economical and environmentally friendly composite dust suppression material. Summary of the invention

[0004] In order to solve the technical problems that traditional chemical dust suppressants have single functions and are difficult to degrade, the present invention discloses a dust suppression material with a double network reinforced structure and a preparation method thereof.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The first aspect of the present invention provides a double network reinforced structure dust suppression material, comprising sesbania gum, polyacrylamide, carboxymethyl cellulose, a cross-linking agent, an oxidant, a water retaining agent, a wetting agent and distilled water.

[0007] Optionally, a double network reinforced structure dust suppression material comprises the following raw materials in parts by weight:

[0008] 0.1-0.5 parts of sesbania gum

[0009] Polyacrylamide 0.1-0.9 parts

[0010] Carboxymethyl cellulose 0.1-0.5 parts

[0011] Crosslinking agent 0.06-0.14 parts

[0012] Oxidant 0.11-0.19 parts

[0013] Water retaining agent 0.1-0.3 parts

[0014] Wetting agent 0.2-1 part.

[0015] Sesbania gum is an environmentally friendly natural polysaccharide. Its galactomannan is a long-chain polymer containing a large number of hydroxyl groups. It has a strong affinity for water, has certain viscosity and cross-linking properties, has good biocompatibility, and is easy to be chemically modified.

[0016] Polyacrylamide is a linear high molecular polymer that is non-toxic and has stable properties. Its structural units contain amide groups, are easy to form hydrogen bonds, have good water solubility and high chemical activity, and can be easily grafted or cross-linked to obtain a variety of modified products with a network structure.

[0017] Carboxymethyl cellulose has high solubility and high stability. Due to its unique surface properties, mechanical strength and good adhesion, it can be used as a reinforcing agent for dust suppression materials.

[0018] Optionally, the cross-linking agent is glutaraldehyde, which is one of the most commonly used cross-linking agents and has the characteristics of high reactivity, short cross-linking time and stable products.

[0019] Optionally, the oxidizing agent is sodium periodate.

[0020] Optionally, the water-retaining agent is glycerol, which, as a water-retaining auxiliary material, can prevent the cured film from drying out and cracking.

[0021] Optionally, the wetting agent is sodium dodecyl sulfate, which has good wettability, strong permeability, stability in a wide pH range, rapid biodegradability, and is a non-toxic anionic surfactant.

[0022] The second aspect of the present invention provides a method for preparing the above-mentioned dust suppression material, comprising the following steps:

[0023] (1) Add distilled water and sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution with dilute hydrochloric acid, then slowly add the crosslinking agent, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0024] (2) Add an oxidant to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 hour, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0025] (3) Add polyacrylamide to the mixed solution II, mix well, heat to a certain temperature, react for 20 minutes, add carboxymethyl cellulose, continue heating in a water bath, and obtain a mixed solution III;

[0026] (4) Cooling the mixed solution III to room temperature, adding a wetting agent and a water retaining agent to the mixed solution III to prepare a double network reinforced structure dust suppressant solution.

[0027] Optionally, the cross-linking agent is glutaraldehyde, the oxidizing agent is sodium periodate, the water retaining agent is glycerol, and the wetting agent is sodium dodecyl sulfate.

[0028] Reaction equation of the present invention is as follows:

[0029] (1) Cross-linking reaction

[0030] (2) Oxidation reaction

[0031] (3) Dual network structure

[0032] SG-OH represents sesbania gum, which contains multiple hydroxyl groups on the sesbania gum molecular chain, and cross-linking occurs at the ortho-cis hydroxyl groups. CLSG-CHO represents oxidative cross-linked sesbania gum, and oxidation generally occurs at the C2 and C3 hydroxyl groups, so the product of step (3) exists in the form of CLSG-OH. CMC-OH represents carboxymethyl cellulose.

[0033] Reaction principle of the present invention:

[0034] (1) The hydroxyl groups on the main chain molecules of sesbania gum undergo etherification cross-linking reaction with the aldehyde groups in the glutaraldehyde molecules. The newly generated chemical bonds continuously replace the original hydrogen bonds on the original molecular chain, forming a tight cross-linked network structure.

[0035] (2) The cross-linked sesbania gum was oxidized with sodium periodate, which further oxidized some of the active hydroxyl groups in the cross-linked sesbania gum molecules into aldehyde groups. At the same time, the oxidation reaction caused the glycoside chains to break, and the sesbania gum molecules were partially degraded.

[0036] (3) The oxidized aldehyde groups react with the amino groups of polyacrylamide, and the hydrogen bonds formed between the amino groups of polyacrylamide and the hydroxyl groups of sesbania gum strengthen the intermolecular forces. The linear polyacrylamide is interspersed to form an interpenetrating network, thus forming the first network structure.

[0037] (4) The molecular chains of sesbania gum are entangled with each other as the skeleton, and the oxidative cross-linked sesbania gum and polyacrylamide form an interpenetrating network structure. After the addition of carboxymethyl cellulose, it is cross-linked with polyacrylamide and connected through hydrogen bond adsorption, which strengthens the original network and forms a second network structure.

[0038] The beneficial effects of the present invention are:

[0039] 1. The present invention adopts a composite modification method to modify sesbania gum. The aldehyde group in the glutaraldehyde molecule and the ortho-cis hydroxyl group on the sesbania gum molecule undergo etherification cross-linking reaction. The newly generated chemical bonds continuously replace the hydrogen bonds on the original molecular chain. The cross-linked structure is firm, which increases the strength and cohesion of the sesbania gum. The cross-linked sesbania gum is oxidized by sodium periodate, and part of the active hydroxyl groups in the cross-linked sesbania gum molecules are further oxidized to aldehyde groups. At the same time, the oxidation reaction causes the glycoside chain to break, thereby reducing the viscosity of the sesbania gum and improving fluidity. The oxidized sesbania gum and polyacrylamide and carboxymethyl cellulose are cross-linked, entangled, and interspersed with each other to form a double network structure. Sodium lauryl sulfate is then compounded to enhance the wetting properties, and finally an environmentally friendly, tightly structured dust suppression material is obtained.

[0040] 2. After the dust suppressant prepared by the present invention is sprayed on the coal dust, the wetting agent sodium dodecylbenzene sulfonate molecules can weaken the intermolecular forces, thereby reducing the surface tension, so that the dust suppressant can better penetrate and fill the gaps between the dust particles, and enhance the hydrophilicity and wetting effect of the dust particles. The oxidative cross-linked sesbania gum-polyacrylamide molecules in the dust suppressant contain a large number of hydrophilic groups, which can bind the coal dust particles together through bonding. The added carboxymethyl cellulose strengthens the rigidity of the network structure due to hydrogen bonding to form a hard solidified layer, and the double cross-linked network structure makes the coal dust particles agglomerate better, strengthens the ability to resist external forces, and makes it less susceptible to wind flow. The added glycerol can make the solidified layer retain a certain amount of moisture to prevent the solidified layer from cracking, and the anti-interference ability of the solidified layer is further enhanced, which greatly slows down the continued evaporation of moisture and prolongs the dust suppression time.

[0041] 3. The double network reinforced structure dust suppressant prepared by the present invention can effectively improve the hydrophilicity and adhesion of dust, and can form a dense protective film on the surface of dust. Tests show that the water retention of the dust suppressant prepared by the present invention is 36.0% higher than that of water, and has a great influence on PM 10 The dust suppression rate reaches 98.67%. It has high dust suppression efficiency, high permeability, and high crust strength. It meets the requirements of underground coal mining operations and open-air coal stacking sites for the adhesion and wettability of dust suppressants, and will not cause secondary pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The present invention is a process flow chart of a method for preparing a dust suppression material with a double network reinforced structure. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0044] The invention discloses a dust suppression material with a double network reinforced structure and a preparation method thereof. The raw materials adopted include 0.1-0.5 parts of sesbania gum, 0.1-0.9 parts of polyacrylamide, 0.1-0.5 parts of carboxymethyl cellulose, 0.06-0.14 parts of a cross-linking agent, 0.11-0.19 parts of an oxidant, 0.1-0.3 parts of a water retaining agent, 0.6-1 parts of a wetting agent, and the rest is distilled water.

[0045] Example 1

[0046] (1) Add 100 ml of distilled water and 0.1 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.06 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0047] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0048] (3) Add 0.1 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 50°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0049] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0050] Example 2

[0051] (1) Add 100 ml of distilled water and 0.1 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.1 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0052] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0053] (3) Add 0.9 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 60°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0054] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0055] Example 3

[0056] (1) Add 100 ml of distilled water and 0.1 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.14 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0057] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0058] (3) Add 0.5 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 70°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0059] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0060] Example 4

[0061] (1) Add 100 ml of distilled water and 0.3 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.06 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0062] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0063] (3) Add 0.9 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 70°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0064] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0065] Example 5

[0066] (1) Add 100 ml of distilled water and 0.3 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.1 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0067] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0068] (3) Add 0.5 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 50°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0069] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0070] Example 6

[0071] (1) Add 100 ml of distilled water and 0.3 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.14 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0072] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0073] (3) Add 0.1 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 60°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0074] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0075] Example 7

[0076] (1) Add 100 ml of distilled water and 0.5 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.06 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0077] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0078] (3) Add 0.5 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 60°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0079] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0080] Example 8

[0081] (1) Add 100 ml of distilled water and 0.5 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.1 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0082] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0083] (3) Add 0.1 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 70°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0084] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0085] Example 9

[0086] (1) Add 100 ml of distilled water and 0.5 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.14 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0087] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, and adjust the solution pH to 6-7 to obtain a mixed solution II;

[0088] (3) Add 0.9 g of polyacrylamide to the mixed solution II, mix thoroughly, heat to 50°C and react for 20 min, add 0.2 g of carboxymethyl cellulose, and continue heating in a water bath for 30 min to obtain a mixed solution III;

[0089] (4) Cool the mixed solution III to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol to the mixed solution III, respectively, and mix thoroughly to obtain a double network reinforced structure dust suppressant solution.

[0090] Comparative Example 1

[0091] (1) Add 100 ml of distilled water and 0.3 g of sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution to 4 with dilute hydrochloric acid, then slowly add 0.06 g of glutaraldehyde, heat to 50°C and react for 1.5 hours to obtain a mixed solution I;

[0092] (2) Add 0.15 g of sodium periodate to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 h, adjust the solution pH to 6-7, wait for the solution to cool to room temperature, add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol, and mix thoroughly.

[0093] Comparative Example 2

[0094] (1) Add 100 ml of distilled water to a beaker, then add 0.8 g of sodium dodecyl sulfate and 0.2 g of glycerol, respectively, and stir to dissolve.

[0095] The effects of Examples 1-9 and Comparative Examples 1 and 2 were investigated by testing. The following tests were conducted in accordance with the TB / T3210.1-2020 standard for coal sample preparation, and the coal sample of 200 mesh was screened using a standard sieve. The coal was dried in a drying oven at (50±2)°C for 5 hours to remove moisture, and then taken out and placed at room temperature for 1 hour.

[0096] Test 1

[0097] The dust suppression performance of the double network reinforced structure dust suppressants prepared in Examples 1-9 and Comparative Examples 1 and 2 was tested.

[0098] Test method: Place equal amounts of coal powder in multiple identical culture dishes, scatter for 10 minutes at a wind speed of 12 m / s, then wait for 2 minutes for the dust to settle naturally, and use a handheld laser particle counter (9306-V2) to detect PM 2.5 and PM 10 The concentration was recorded as C0. The Examples 1-9 and Comparative Examples 1 and 2 were sprayed evenly in the culture dish in equal amounts. After 48 hours, the samples were scattered for 10 minutes at a wind speed of 12 m / s. PM was detected after 2 minutes. 2.5 and PM 10 The concentration is recorded as C1.

[0099] The dust suppression rate calculation formula is:

[0100]

[0101] Where: S is the dust suppression rate (%), C0 is PM 2.5 and PM 10 Initial concentration (μg / m 3 ), C1 is the PM after spraying dust suppressant 2.5 and PM 10 Concentration (μg / m 3 ), when calculating C0 and C1, the PM in the initial ambient air must be subtracted 2.5 and PM 10 concentration.

[0102] The test results are shown in Table 1 below.

[0103] Table 1 Dust suppression test

[0104] Experimental samples <![CDATA[PM 2.5 ]]> <![CDATA[PM 10 ]]> Example 1 96.34 97.21 Example 2 97.08 97.54 Example 3 98.03 98.21 Example 4 97.25 97.57 Example 5 97.31 97.64 Example 6 97.69 98.17 Example 7 98.04 98.67 Example 8 98.18 98.34 Example 9 97.77 98.51 Comparative Example 1 79.23 78.12 Comparative Example 2 50.19 53.67

[0105] Analyzing the results of test 1, it was found that all the tested solutions reduced PM 2.5 and PM 10 The dust suppression effect of the comparative example is not as obvious as that of the example. Example 7 can achieve the highest dust suppression rate (PM 2.5 and PM 10 98.18% and 98.34% respectively). Therefore, the above results show that the double network structure dust suppressant does have good dust suppression performance and greatly overcomes the resuspension problem of static dust.

[0106] Test 2

[0107] The double network reinforced structure dust suppressants prepared in Examples 1-9 and Comparative Examples 1 and 2 were tested for water retention, wettability and permeability.

[0108] The test method is as follows: an equal amount of coal dust is placed in multiple culture dishes, 9 samples of the embodiment and 2 samples of the comparative example of the same mass are spread on the surface of the coal dust, and the culture dishes are placed in a vacuum drying oven at 50° C. After 2 hours, the samples are taken out, their masses are weighed, and the cumulative evaporation rate of the samples is calculated.

[0109] Take 30 ml of the solution to be tested in a beaker and place the beaker under the platinum plate. Then, turn on the switch, adjust the lifting platform, wait for the platinum plate to contact the liquid surface, and record the surface tension value to be tested; finally, measure the surface tension value of each solution three times and record the average value.

[0110] Load equal amounts of coal powder into multiple tubes of the same size, then use a burette to suck a certain amount of dust suppressant solution (3±0.5ml) and drop it into the test tubes respectively. Use a stopwatch to record the penetration depth and time and calculate the penetration rate.

[0111] The test results are shown in Table 2 below.

[0112] Table 2 Water retention and wettability test

[0113]

[0114] The results of analysis test 2 show that the water loss rate of comparative examples 1 and 2 is the fastest, and the cumulative evaporation rate after drying for 5 hours is more than 95%. After spraying on the surface of the coal sample and drying, the embodiment will form a dense solidified layer, which can retain a certain amount of moisture and has good water retention performance. From the surface tension test, it can be seen that the embodiment and the comparative example are almost the same, and have good wetting performance. Too slow penetration speed will lead to poor dust fixation effect and easily cause secondary dust. Too fast speed will lead to excessive use of dust suppressant. The embodiment has a faster penetration speed and meets the needs of dust suppression.

[0115] It can be seen that the present invention can test the dust suppression property, water retention, permeability and wettability of the prepared dust suppression material by designing different ratios, so as to judge the actual dust suppression effect of the dust suppression material.

[0116] In summary, the double-network reinforced structure dust suppression material prepared by the present invention combines wettability and adhesion. When sprayed on the surface of a coal mine, it can form a dense protective film to prevent the flying of coal dust. It can meet the actual needs of coal dust suppression and has good social benefits and considerable economic benefits.

[0117] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for preparing a dust suppression material with a double network reinforced structure, characterized in that: The steps include: (1) Add distilled water and sesbania gum to a beaker, stir to dissolve, adjust the pH of the solution with dilute hydrochloric acid, then slowly add the crosslinking agent, heat to 50°C and react for 1.5 hours to obtain a mixed solution I; (2) Add an oxidant to the mixed solution I, adjust the solution temperature to 40°C, heat in a water bath for 1 hour, and adjust the solution pH to 6-7 to obtain a mixed solution II; (3) Add polyacrylamide to the mixed solution II, mix well, heat to a certain temperature, react for 20 minutes, add carboxymethyl cellulose, continue heating in a water bath, and obtain a mixed solution III; (4) cooling the mixed solution III to room temperature, adding a wetting agent and a water retaining agent to the mixed solution III to prepare a double network reinforced structure dust suppressant solution; The dust suppression material comprises sesbania gum, polyacrylamide, carboxymethyl cellulose, a cross-linking agent, an oxidant, a water retaining agent, a wetting agent and distilled water; the weight parts are as follows: 0.1-0.5 parts of sesbania gum Polyacrylamide 0.1-0.9 parts Carboxymethyl cellulose 0.1-0.5 parts Crosslinking agent 0.06-0.14 parts Oxidant 0.11-0.19 parts Water retaining agent 0.1-0.3 parts Wetting agent 0.2-1 part The balance is distilled water.

2. The method for preparing a dust suppression material with a double network reinforced structure according to claim 1, characterized in that: The cross-linking agent is glutaraldehyde, the oxidizing agent is sodium periodate, the water retaining agent is glycerol, and the wetting agent is sodium dodecyl sulfate.

Citation Information

Patent Citations

  • Dust suppressant for suppressing mineral powder and bare ground dust and preparation method thereof

    CN109652016A

  • Dust suppressant and preparation method and application thereof

    CN111349422A

  • Multi-functional gel for inhibiting dust raising of coal pile and preventing spontaneous combustion and preparation method thereof

    CN113717403A

  • Dust suppressant and soil stabilization composition

    US20040091324A1

  • KR20230016522A