A method for preparing polyamide material for large aircraft tires

By using combined extrusion technology of modified polyurethane and modified polyamide with thiol phosphate, silicone rubber and other components in large aircraft tire materials, a flame retardant system with P, S, N, and Si elements is formed to solve the problem Existing materials have shortcomings in flame retardancy and mechanical properties, so efficient flame retardancy and mechanical properties improvements have been achieved.

CN118374144BActive Publication Date: 2024-10-29JIANGSU HONGSHENG NEW MATERIAL LIMITED BY SHARE LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410810203.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-29
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing large aircraft tire materials have deficiencies in flame retardancy and mechanical properties, making it difficult to meet the high safety and durability requirements.

Method used

A preparation method is adopted to form modified polyurethane and modified polyurethane by dissolving polyurethane particles in a dimethylformamide solvent and reacting with compounds such as isothiocyanate methacrylate, diethyl phosphite, and benzomelamine. Amide is melted and extruded with thiol phosphate, silicone rubber and polyamide fiber in a twin-screw extruder to form a flame retardant system with P, S, N and Si elements.

Benefits of technology

The high flame retardant and mechanical properties of large aircraft tire materials are achieved, and the interfacial compatibility and impact resistance of the material are improved through cross-linked networks and addition reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118374144B_ABST
    Figure CN118374144B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyamide materials and discloses a method for preparing a polyamide material for large aircraft tires. The invention provides a method for preparing a polyamide material for large aircraft tires by adding modified polyurethane, modified polyamide, mercaptan phosphate, silicone rubber and polyamide fiber into a twin-screw extruder for melt extrusion to obtain the polyamide material for large aircraft tires. The polyamide material contains a flame retardant system of P, S, N and Si elements for synergistic flame retardancy. In the process of melt extrusion, double bonds in the mercaptan phosphate react with silicone rubber for addition reaction, and terminal chlorine in the modified polyamide reacts with silicone rubber for substitution reaction, so that a cross-linked network is formed between the three, thereby increasing the interface compatibility between each other and making the polyamide material have better mechanical properties. In addition, the silicone rubber itself has better mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyamide materials, in particular to a method for preparing a polyamide material for large aircraft tires. Background Art

[0002] The rubber surface of the aircraft tire is made of wear-resistant and high-temperature resistant special materials bonded with steel wires, is about 20 mm thick, and has high strength. The tire valve is sharp and short, and is made of high-temperature fluoroplastics, so that air intake is smooth and leakage is strictly prevented. In order to enhance its mechanical properties and flame retardant properties, the present invention prepares polyamide materials for large aircraft tires; as reported in the document "Application of Aromatic Polyamide Materials in Laptop Casings", aromatic polyamide materials have the characteristics of good chemical resistance, high flame retardancy, high rigidity, and good flexibility. The present invention introduces benzoguanamine to improve the performance of polyamide materials. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a polyamide material for large aircraft tires, which has good flame retardant effect and mechanical properties.

[0005] (II) Technical solution

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a polyamide material for large aircraft tires, comprising the following preparation method:

[0007] (1) Adding purified polyurethane particles to a dimethylformamide solvent, stirring and dissolving at 70-100° C. for 6-12 hours, and then drying to obtain a polyurethane film; adding methyl methacrylate isothiocyanate to the polyurethane film, passing nitrogen for protection, and then adding triethylamine thereto, and oil bathing at 40-60° C. for 8-14 hours. After the reaction, washing with acetonitrile and drying to obtain an olefinic polyurethane;

[0008] (2) Adding olefinated polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, carrying out addition reaction at 70-90° C. for 10-12 hours, distilling under reduced pressure after the reaction, washing with ether, dissolving the crude product in dichloromethane and recrystallizing, and drying to obtain modified polyurethane;

[0009] (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, react at 60-100°C for 4-8h, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide;

[0010] (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, then adding benzoin dimethyl ether initiator, irradiating with 365 nm ultraviolet light at 20-40° C. for 2-3 h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate;

[0011] (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, melt-extrude at 180-200° C., and obtain polyamide material for large aircraft tires.

[0012] Preferably, the mass ratio of the polyurethane particles, methacrylate isothiocyanate, polyurethane film and triethylamine in (1) is 1.3-1.5:2.1-2.6:1:0.02-0.03.

[0013] Preferably, the mass ratio of olefinic polyurethane to diethyl phosphite in (2) is 1:1.1-1.3.

[0014] Preferably, the mass ratio of benzoguanamine, alkyl diacyl chloride and potassium carbonate in (3) is 1.1-1.5:1:0.02-0.03.

[0015] Preferably, the mass ratio of triallyl phosphate, aminoethanethiol and benzoin dimethyl ether initiator in (4) is 1:0.4-0.8:0.01-0.02.

[0016] Preferably, the mass ratio of the modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber in (5) is 1:1.1-2.5:0.8-1.3:1.1-1.4:100.

[0017] 3. Beneficial technical effects

[0018] The invention obtains the polyamide material for large aircraft tires by adding modified polyurethane, modified polyamide, mercaptan phosphate, silicone rubber and polyamide fiber into a twin-screw extruder for melt extrusion.

[0019] Diethyl phosphite with good flame retardant effect in modified polyurethane, thiol in thiol phosphate, benzoguanamine in modified polyamide, and silicon in silicone rubber together constitute a flame retardant system containing P, S, N, and Si elements, which have synergistic flame retardancy.

[0020] During the melt extrusion process, the double bonds in the thiol phosphate will undergo an addition reaction with the silicone rubber, and the terminal chlorine of the modified polyamide will undergo a substitution reaction with the silicone rubber, forming a cross-linked network among the three, which increases the interfacial compatibility between each other and makes the polyamide material have better mechanical properties; and the silicone rubber itself has good mechanical properties, which synergistically increase the mechanical effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is the preparation route diagram of modified polyurethane. DETAILED DESCRIPTION

[0022] Example 1

[0023] (1) Add purified polyurethane particles to a dimethylformamide solvent, stir and dissolve at 70°C for 6 hours, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, introduce nitrogen for protection, and then add triethylamine, wherein the mass ratio of polyurethane particles, methyl methacrylate isothiocyanate, polyurethane film, and triethylamine is 1.3:2.1:1:0.02, and the reaction is carried out at 40°C in an oil bath for 8 hours. After the reaction, the reaction is washed with acetonitrile and dried to obtain an olefinated polyurethane;

[0024] (2) adding olefinic polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, wherein the mass ratio of olefinic polyurethane to diethyl phosphite is 1:1.1, and performing addition reaction at 70° C. for 10 hours. After the reaction, distillation is performed under reduced pressure, and the crude product is washed with ether, dissolved in dichloromethane, recrystallized, and dried to obtain a modified polyurethane;

[0025] (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, wherein the mass ratio of benzoguanamine, alkyl dichloride and potassium carbonate is 1.1:1:0.02, react at 60° C. for 4 h, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide;

[0026] (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, and then adding benzoin dimethyl ether initiator, wherein the mass ratio of triallyl phosphate, aminoethanethiol, and benzoin dimethyl ether initiator is 1:0.4:0.01, irradiating with 365 nm ultraviolet light at 20° C. for 2 h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate;

[0027] (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, wherein the mass ratio of modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber is 1:1.1:0.8:1.1:100, and melt-extrude at 180° C. to obtain a polyamide material for large aircraft tires.

[0028] Example 2

[0029] (1) Add purified polyurethane particles to a dimethylformamide solvent, stir and dissolve at 100° C. for 12 hours, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, introduce nitrogen for protection, and then add triethylamine, wherein the mass ratio of polyurethane particles, methyl methacrylate isothiocyanate, polyurethane film, and triethylamine is 1.5:2.6:1:0.03, and react at 60° C. in an oil bath for 14 hours. After the reaction, wash with acetonitrile and dry to obtain an olefinated polyurethane;

[0030] (2) Adding olefinic polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, wherein the mass ratio of olefinic polyurethane to diethyl phosphite is 1:1.3, and performing addition reaction at 90° C. for 12 h. After the reaction, performing vacuum distillation, washing with ether, dissolving the crude product in dichloromethane and recrystallizing, and drying to obtain modified polyurethane;

[0031] (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, wherein the mass ratio of benzoguanamine, alkyl dichloride and potassium carbonate is 1.5:1:0.03, react at 100° C. for 8 hours, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide;

[0032] (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, and then adding benzoin dimethyl ether initiator, wherein the mass ratio of triallyl phosphate, aminoethanethiol, and benzoin dimethyl ether initiator is 1:0.8:0.02, irradiating with 365 nm ultraviolet light at 40° C. for 3 h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate;

[0033] (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, wherein the mass ratio of modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber is 1:2.5:1.3:1.4:100, and melt-extrude at 200° C. to obtain a polyamide material for large aircraft tires.

[0034] Example 3

[0035] (1) Add purified polyurethane particles to dimethylformamide solvent, stir and dissolve at 85°C for 9 hours, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, pass nitrogen for protection, and then add triethylamine, wherein the mass ratio of polyurethane particles, methyl methacrylate isothiocyanate, polyurethane film, and triethylamine is 1.4:2.35:1:0.025, and react at 50°C in an oil bath for 11 hours. After the reaction, wash with acetonitrile and dry to obtain an olefinated polyurethane;

[0036] (2) Adding olefinic polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, wherein the mass ratio of olefinic polyurethane to diethyl phosphite is 1:1.2, and performing addition reaction at 80° C. for 11 hours. After the reaction, performing vacuum distillation, washing with ether, dissolving the crude product in dichloromethane and recrystallizing, and drying to obtain modified polyurethane;

[0037] (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, wherein the mass ratio of benzoguanamine, alkyl dichloride and potassium carbonate is 1.3:1:0.025, react at 80° C. for 6 h, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide;

[0038] (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, and then adding benzoin dimethyl ether initiator, wherein the mass ratio of triallyl phosphate, aminoethanethiol, and benzoin dimethyl ether initiator is 1:0.6:0.015, irradiating with 365 nm ultraviolet light at 30° C. for 2.5 h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate;

[0039] (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, wherein the mass ratio of modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber is 1:1.8:1.05:1.25:100, and melt-extrude at 190° C. to obtain a polyamide material for large aircraft tires.

[0040] Example 4

[0041] (1) Add purified polyurethane particles to a dimethylformamide solvent, stir and dissolve at 70°C for 6 hours, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, introduce nitrogen for protection, and then add triethylamine, wherein the mass ratio of polyurethane particles, methyl methacrylate isothiocyanate, polyurethane film, and triethylamine is 1.3:2.1:1:0.02, and the reaction is carried out at 40°C in an oil bath for 8 hours. After the reaction, the reaction is washed with acetonitrile and dried to obtain an olefinated polyurethane;

[0042] (2) adding olefinic polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, wherein the mass ratio of olefinic polyurethane to diethyl phosphite is 1:1.1, and performing addition reaction at 70° C. for 10 hours. After the reaction, distillation is performed under reduced pressure, and the crude product is washed with ether, dissolved in dichloromethane, recrystallized, and dried to obtain a modified polyurethane;

[0043] (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, wherein the mass ratio of benzoguanamine, alkyl dichloride and potassium carbonate is 1.5:1:0.03, react at 100° C. for 8 hours, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide;

[0044] (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, and then adding benzoin dimethyl ether initiator, wherein the mass ratio of triallyl phosphate, aminoethanethiol, and benzoin dimethyl ether initiator is 1:0.8:0.02, irradiating with 365 nm ultraviolet light at 40° C. for 3 h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate;

[0045] (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, wherein the mass ratio of modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber is 1:1.8:1.05:1.25:100, and melt-extrude at 190° C. to obtain a polyamide material for large aircraft tires.

[0046] Example 5

[0047] (1) Add purified polyurethane particles to a dimethylformamide solvent, stir and dissolve at 100° C. for 12 hours, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, introduce nitrogen for protection, and then add triethylamine, wherein the mass ratio of polyurethane particles, methyl methacrylate isothiocyanate, polyurethane film, and triethylamine is 1.5:2.6:1:0.03, and react at 60° C. in an oil bath for 14 hours. After the reaction, wash with acetonitrile and dry to obtain an olefinated polyurethane;

[0048] (2) Adding olefinic polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, wherein the mass ratio of olefinic polyurethane to diethyl phosphite is 1:1.3, and performing addition reaction at 90° C. for 12 h. After the reaction, performing vacuum distillation, washing with ether, dissolving the crude product in dichloromethane and recrystallizing, and drying to obtain modified polyurethane;

[0049] (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, wherein the mass ratio of benzoguanamine, alkyl dichloride and potassium carbonate is 1.3:1:0.025, react at 80° C. for 6 h, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide;

[0050] (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, and then adding benzoin dimethyl ether initiator, wherein the mass ratio of triallyl phosphate, aminoethanethiol, and benzoin dimethyl ether initiator is 1:0.6:0.015, irradiating with 365 nm ultraviolet light at 30° C. for 2.5 h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate;

[0051] (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, wherein the mass ratio of modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber is 1:1.1:0.8:1.1:100, and melt-extrude at 180° C. to obtain a polyamide material for large aircraft tires.

[0052] Comparative Example 1

[0053] Compared with Example 5, no modified polyurethane was added, and other raw materials were the same.

[0054] Comparative Example 2

[0055] Compared with Example 5, modified polyurethane and modified polyamide were not added, and other raw materials were the same.

[0056] Comparative Example 3

[0057] Compared with Example 5, modified polyurethane, modified polyamide and thiol phosphate were not added, and other raw materials were the same.

[0058] The polyamide materials of the embodiment and the comparative example were subjected to mechanical property tests using a universal material testing machine. The test results are shown in Table 1.

[0059] Table 1: Tensile properties tested.

[0060]

[0061] It can be seen from Table 1 that the polyamide material of the present invention has good mechanical properties.

[0062] The oxygen index was determined according to the method specified in GB / T2406-2008. The flame retardant grade was tested according to UL94-2009 standard. FV-0: the burning time does not exceed 10 seconds and does not ignite the absorbent cotton. FV-1: the burning time does not exceed 30 seconds and does not ignite the absorbent cotton. FV-2: the burning time does not exceed 30 seconds and ignites the absorbent cotton. The test results are shown in Table 2.

[0063] Table 2: Flame retardancy tests.

[0064]

[0065] It can be seen from Table 2 that the polyamide material of the present invention has good flame retardant properties.

[0066] The impact resistance of polyamide material was tested by XJJD simple supported beam impact strength tester. The polyamide material sample was placed on the support of the tester so that the impact blade fell on the center of the polyamide material. The energy carrier was released and the change of force over time during the impact process was recorded. The polyamide material sample was 120 mm × 40 mm × 4 cm. The test results are shown in Table 3.

[0067] Table 3: Impact resistance test.

[0068]

[0069] It can be seen from Table 3 that the polyamide material of the present invention has good impact resistance.

[0070] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a polyamide material for large aircraft tires, characterized in that: The invention comprises the following preparation methods: (1) Adding purified polyurethane particles to a dimethylformamide solvent, stirring and dissolving at 70-100° C. for 6-12 hours, and then drying to obtain a polyurethane film; adding methyl methacrylate isothiocyanate to the polyurethane film, passing nitrogen for protection, and then adding triethylamine thereto, and oil bathing at 40-60° C. for 8-14 hours. After the reaction, washing with acetonitrile and drying to obtain an olefinic polyurethane; (2) Adding olefinated polyurethane and diethyl phosphite to N,N-dimethylformamide solvent, carrying out addition reaction at 70-90° C. for 10-12 hours, distilling under reduced pressure after the reaction, washing with ether, dissolving the crude product in dichloromethane and recrystallizing, and drying to obtain modified polyurethane; (3) Add benzoguanamine and alkyl dichloride to N,N-dimethylformamide solvent, stir and dissolve, then add potassium carbonate, react at 60-100°C for 4-8h, and after reaction, remove the solvent by vacuum distillation, filter and dry to obtain modified polyamide; (4) adding triallyl phosphate and aminoethanethiol into a reactor, stirring evenly, then adding benzoin dimethyl ether initiator, irradiating with 365nm ultraviolet light at 20-40°C for 2-3h, centrifuging, washing with deionized water, and drying to obtain thiol phosphate, wherein the mass ratio of triallyl phosphate, aminoethanethiol, and benzoin dimethyl ether initiator is 1:0.4-0.8:0.01-0.02; (5) Adding modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber into a twin-screw extruder, and melt-extruded at 180-200° C. to obtain a polyamide material for large aircraft tires, wherein the mass ratio of the modified polyurethane, modified polyamide, thiol phosphate, silicone rubber and polyamide fiber is 1:1.1-2.5:0.8-1.3:1.1-1.4:

100.

2. The method for preparing a polyamide material for large aircraft tires according to claim 1, characterized in that: The mass ratio of olefinic polyurethane to diethyl phosphite in (2) is 1:1.1-1.

3.

3. The method for preparing a polyamide material for large aircraft tires according to claim 1, characterized in that: The mass ratio of benzoguanamine, alkyl diacyl chloride and potassium carbonate in (3) is 1.1-1.5:1:0.02-0.03.

Citation Information

Patent Citations

  • Oligomeric HALS-phosphites and HALS-phosphonites as stabilisers

    CA2150641A1

  • Thermoplastic composition

    CN112074571A