Para-aramid fiber and preparation method thereof
Para-aramid fiber is prepared by low-temperature solution polymerization method by replacing NMP with amide solvent, which solves the problems of uneven polymer properties and particle size distribution, inorganic salt residue and high production cost, and achieves the improvement of fiber performance and production efficiency. optimization.
Patent Information
- Application Number
- CN202410814516.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-24
AI Technical Summary
In the production of existing para-aramid fibers, there are problems such as uneven polymer intrinsic viscosity and particle size distribution, residual inorganic salts and high production costs, resulting in unstable fiber quality and performance.
Amide solvents are used to replace NMP, and para-aramid fibers are prepared through low-temperature solution polymerization. Only a small amount of inorganic salt cosolvents are needed, which reduces the water consumption and operation complexity of washing and improves the mechanical properties of the fibers.
The para-aramid fiber has a narrow intrinsic viscosity distribution and uniform particle size distribution, which reduces production costs, improves the mechanical properties and production efficiency of the fiber, reduces inorganic salt residues, and improves product stability.
Smart Images

Figure CN118374899B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a para-aramid fiber and a preparation method thereof, belonging to the technical field of aramid fibers. Background Art
[0002] Para-aramid is an advanced composite material that can be used in many structural materials, protective materials, and building structure reinforcement materials. Para-aramid composite reinforcement materials have the characteristics of light weight, high strength, high modulus, corrosion resistance, and durability. At the same time, para-aramid has strong alkali corrosion resistance, is non-conductive, and has good dynamic load, impact resistance, and fatigue resistance. Para-aramid can also be used to replace asbestos to manufacture friction materials, and can be used in cables and conveyor belts. At present, the application of para-aramid materials is mainly based on its excellent characteristics such as high strength and high elastic modulus. It is reported that aramid products are used in bulletproof vests, helmets, etc., accounting for about 7% to 8%, aerospace materials, and sports materials account for about 40%; tire skeleton materials, conveyor belt materials, etc. account for about 20%, and high-strength ropes account for about 13%.
[0003] Although great progress has been made in the localization of para-aramid, the following problems still exist: First, the characteristic viscosity and particle size distribution of the para-aramid polymer currently produced are uneven, resulting in quality problems such as fiber fuzz, loops, and balls, which need to be further improved. Second, the price of NMP, the solvent used for polymerization, is expensive, resulting in high production costs for para-aramid. Third, in the preparation process of para-aramid, more inorganic salts need to be added as co-solvents during the polymerization reaction, and after the polymerization reaction, the inorganic salts need to be removed by washing. This operation consumes a lot of water in the industrial production process, and there is a problem of incomplete washing. The residual inorganic salts in the polymer will also affect the performance of the para-aramid fiber. For example, the para-aramid preparation methods disclosed in Chinese patent applications CN110499542A, CN114456596A, and CN114351276A all require the addition of a large amount of inorganic salt cosolvents such as lithium chloride or calcium chloride. Moreover, when preparing para-aramid using these traditional methods, if the strength performance of para-aramid is to be improved, special monomers are often required to be added, resulting in high raw material costs and high operating costs for the entire preparation process. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a para-aramid fiber and a preparation method thereof. The preparation process requires only a small amount of inorganic salt as a co-solvent, thereby solving the problems of incomplete water washing and inorganic salt residue that are prone to occur in the traditional process, and preparing a para-aramid fiber product with excellent mechanical properties. In addition, the characteristic viscosity distribution of the para-aramid polymer is narrow, and the product performance is stable.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing para-aramid fiber, the preparation method comprising: performing polymerization reaction between para-phenylenediamine and terephthaloyl chloride in an amide solvent, and obtaining polymer powder through post-treatment after the reaction is completed; dissolving the polymer powder in concentrated sulfuric acid to obtain spinning solution; and obtaining the para-aramid fiber through dry-jet wet spinning of the spinning solution;
[0006] The amide solvent is at least one of the following structural formulas: ;
[0007] R 1 , R 2 , R 3 Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl.
[0008] Furthermore, inorganic salt calcium chloride is added as a co-solvent during the polymerization reaction, and the mass fraction of the co-solvent in the amide solvent is 1-2%.
[0009] Further, the amide solvent is selected from at least one of 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-propoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide;
[0010] The purity of the amide solvent is greater than 95%, and the water content is less than 700 ppm.
[0011] Furthermore, when concentrated sulfuric acid is used as a dissolving medium for the polymer powder, the intrinsic viscosity at 25° C. is in the range of 9.0-9.5 dL / g.
[0012] Furthermore, the polymerization reaction temperature is -5 to 5°C; the molar ratio of the amount of terephthaloyl chloride added to the amount of p-phenylenediamine added is (0.998-1.002):1;
[0013] Furthermore, during the polymerization reaction, terephthaloyl chloride is added to the reaction system in two batches, with the weight of the first batch being 30-60% of the total amount and the weight of the second batch being 40-70% of the total amount.
[0014] Furthermore, the temperature at which the concentrated sulfuric acid dissolves the polymer powder is 80-100° C.; and the mass content of the polymer powder in the spinning solution is 19%-25%.
[0015] Furthermore, the dry-jet wet spinning process is as follows: the spinning solution is squeezed out from the spinneret by a gear pump, stretched by an air layer, coagulated in a coagulation bath, and then the filament bundle is washed with water, washed with alkali, washed with water again, and then dried, hot stretched, oiled, and wound to obtain the para-aramid fiber.
[0016] Furthermore, during the air layer stretching, the air bath height is 2-10 mm, and the stretching multiple is 5-12 times; the coagulation bath is a dilute sulfuric acid solution, and the mass concentration of the dilute sulfuric acid solution is not greater than 15%.
[0017] Furthermore, the drying temperature is 150-200°C, and the heat drawing temperature is 300-450°C.
[0018] The present invention also discloses a para-aramid fiber, which is prepared by the preparation method of the present invention; the para-aramid fiber has a tensile strength of 27-30 cN / dtex, an elongation at break of 3.2-4.2%, and an elastic modulus of 750-800 cN / dtex.
[0019] The beneficial effects of the present invention are:
[0020] The invention prepares para-aramid fiber by low-temperature solution polymerization; uses amide solvents instead of NMP in the para-aramid polymerization process, reduces the production cost of the para-aramid, and achieves cost reduction and efficiency improvement.
[0021] In the preparation method of the present invention, an amide solvent is used to prepare the polymer powder. Since the amide solvent has a linear structure and has an additional oxygen heteroatom in the NMP molecule, the hydrogen bonding between the amide solvent and the polymer macromolecular chain is stronger than that between NMP and the polymer macromolecular chain, thereby increasing the solubility of the polymer. Therefore, only a small amount of inorganic salt is needed as a co-solvent. If NMP is used as a solvent, the mass fraction of calcium chloride is generally 7-10%. Therefore, the preparation method of the present invention can reduce the raw material cost in the production process, reduce the difficulty of water washing, reduce the amount of water used for water washing, and reduce the residual inorganic salt in the fiber, thereby improving production efficiency. The action principle of the amide solvent and the para-aramid polymer is as follows:
[0022] .
[0023] The para-aramid polymer powder produced by the present invention using amide solvents has a narrow intrinsic viscosity range and a narrow particle size distribution, and the para-aramid fiber products produced in different batches have stable performance. The defects of fiber fuzz and hair balls prepared thereby are greatly improved, and the mechanical properties of the fiber are stable. DETAILED DESCRIPTION
[0024] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0026] A method for preparing para-aramid fiber, the preparation method comprising: performing polymerization reaction between para-phenylenediamine and terephthaloyl chloride in an amide solvent, and obtaining polymer powder through post-treatment after the reaction is completed; dissolving the polymer powder in concentrated sulfuric acid to obtain spinning solution; and obtaining the para-aramid fiber through dry-jet wet spinning of the spinning solution;
[0027] The amide solvent is at least one of the following structural formulas: ;
[0028] R 1 , R 2 , R 3 Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl.
[0029] Specifically, the amide solvent is selected from at least one of 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-propoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide.
[0030] When R 1 , R 2 , R 3 When all R are methyl, it is named 3-methoxy-N,N-dimethylpropionamide, abbreviated as MMPA. 1 , R 2 All are methyl, R 3 It is ethyl and named 3-ethoxy-N,N-dimethylpropionamide, referred to as MEPA. 1 , R 2 All are methyl, R 3 is a n-propyl group, named 3-propoxy-N,N-dimethylpropionamide, referred to as MIPA. 1 , R 2 All are methyl, R 3 It is n-butyl and is named 3-butoxy-N,N-dimethylpropionamide, abbreviated as MBPA. Other types of new amide solvents are named in the same way.
[0031] Specifically, the co-solvent is calcium chloride, and the added mass fraction is 1-2%.
[0032] Specifically, the purity of the amide solvent is greater than 95%, and the water content is less than 700 ppm.
[0033] Specifically, when the polymer powder is dissolved in concentrated sulfuric acid (mass concentration is 98% or more) as a dissolving medium, the intrinsic viscosity of the polymer powder at 25° C. is in the range of 9.0-9.5 dL / g.
[0034] Specifically, the polymerization reaction temperature is -5 to 5°C; the molar ratio of the amount of terephthaloyl chloride added to the amount of p-phenylenediamine added is (0.998-1.002):1;
[0035] During the polymerization reaction, terephthaloyl chloride is added into the reaction system in two batches, the weight of the first batch is 30-60% of the total amount, and the weight of the second batch is 40-70% of the total amount.
[0036] Specifically, the temperature at which the concentrated sulfuric acid dissolves the polymer powder is 80-100° C.; the mass content of the polymer powder in the spinning solution is 19%-25%.
[0037] More specifically, the preparation method of the para-aramid fiber is:
[0038] S1. Preparation of polymer powder: Under nitrogen protection, in a reactor, p-phenylenediamine (PPD) is dissolved in a new amide solvent containing a small amount of calcium chloride, and the mixture is stirred and mixed evenly. The system temperature is controlled by a refrigerant in the reactor jacket, and terephthaloyl chloride (TPC) is added twice. After the reaction is completed, it is first neutralized with alkali solution (according to the theoretical amount of HCl generated by the polymerization reaction, the corresponding alkali solution is added to neutralize the theoretical amount of HCl), then washed with water, and finally dried to obtain polymer powder.
[0039] S2. Preparation of spinning solution: The polymer powder obtained by the above process is dissolved in concentrated sulfuric acid (mass concentration of concentrated sulfuric acid is 99.8%) in a dissolving kettle at a temperature of 80-100°C in a multi-stage partitioned jacket of the dissolving kettle under nitrogen sealing. The temperature of the system is controlled by a heat medium in the jacket of the dissolving kettle. After filtration, a spinning solution with a mass concentration of 19.0-25.0% is prepared.
[0040] S3, dry-jet wet spinning process: the spinning solution is squeezed out from the spinneret by a gear pump, stretched by an air layer, coagulated in a coagulation bath, and then the tow is washed with water, alkaline washed with alkali solution, washed with water again, and then dried, hot stretched, oiled, and wound to obtain para-aramid fiber.
[0041] More specifically, the alkali solution in step S1 and step S3 is any one of sodium hydroxide, calcium hydroxide, potassium hydroxide, lithium hydroxide, diethylamine, ammonia, dimethylamine, methylamine, ethylamine, and propylamine aqueous solutions, with a mass fraction of 10 to 40%.
[0042] More specifically, during the preparation of the polymer powder, the drying temperature is 120-160°C.
[0043] Specifically, during the air layer stretching, the air bath height is 2-10 mm, and the stretching multiple is 5-12 times;
[0044] The coagulation bath is a dilute sulfuric acid solution (an aqueous solution of sulfuric acid), and the mass concentration of the dilute sulfuric acid solution is not greater than 15%.
[0045] Specifically, in the dry-jet wet spinning process, the drying temperature is 150-200°C, and the heat drawing temperature is 300-450°C.
[0046] A para-aramid fiber is prepared by the preparation method of the present invention; the para-aramid fiber has a tensile strength of 27-30 cN / dtex, an elongation at break of 3.2-4.2%, and an elastic modulus of 750-800 cN / dtex.
[0047] The detection method involved in the embodiment is:
[0048] Intrinsic viscosity test method: Turn on the viscometer (instrument model, ViscoQC100), turn on the heating, and keep the water temperature at 25°C. Weigh 0.125 g of para-aramid polymer powder and dissolve it in 25 ml of concentrated sulfuric acid, transfer it to the Ubbelohde viscometer, and measure the outflow time of pure concentrated sulfuric acid and concentrated sulfuric acid solution of dissolved polymer powder respectively. According to the corresponding calculation formula, the intrinsic viscosity of the prepared polymer powder at 25°C is obtained.
[0049] Test method for fiber mechanical properties: GB / T 42823-2023. The specific test method is: first weigh a certain amount of fiber filaments, test the linear density of the fiber, and then set the twist according to the linear density for twisting. Fix the twisted fiber on the tensile test fixture, measure the mechanical properties 10 times, and take the average. The electric tensile machine model is Instron34TM-30.
[0050] Determination method and standard reference for calcium ion content in fiber: GB 7476-87.
[0051] Example 1
[0052] (1) Preparation of polymer powder:
[0053] At room temperature, p-phenylenediamine (43.20 kg) is added to a MMPA solution (350 kg) containing 1% by mass of calcium chloride, stirred at 25°C for 1 hour under nitrogen protection, cooled to -5°C, and then terephthaloyl chloride (81.20 kg) is added in two batches, with a batch interval of 30 minutes (the molar ratio of the first batch of terephthaloyl chloride added to the second batch is 50:50). After the reaction is completed, it is neutralized with a 40% sodium hydroxide aqueous solution, and then washed with water in multiple stages, ground, and dried to obtain a polymer powder. When the polymer powder is dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C is 9.0 dL / g, and the particle size distribution is: Dv (10): 79 μm, Dv (50): 350 μm, Dv (90): 656 μm.
[0054] (2) Preparation of spinning solution:
[0055] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 99.8%, and kept at 90°C to obtain a spinning solution, in which the mass content of the polymer powder is 22%.
[0056] (3) Dry-jet wet spinning process:
[0057] The spinning solution was extruded from the spinneret by a gear pump, the air bath height was 9 mm, and the drafting ratio was 7 times. Then it was formed by a coagulation bath, the coagulation bath composition was a concentrated sulfuric acid aqueous solution with a mass fraction of 5%, the temperature was 30 ℃; neutralized by a 17% sodium hydroxide aqueous solution, washed with a water bath (residence time 10 s); then dried at 150 ℃, entered the 350 ℃ hot drawing process, and finally oiled and wound into a tube to obtain para-aramid fiber.
[0058] The linear density of the para-aramid fibers is 1580 dtex, the tensile strength is 27.6 cN / dtex, the elongation at break is 3.6%, the elastic modulus is 758 cN / dtex, and the calcium ion content is zero.
[0059] Example 2
[0060] (1) Preparation of polymer powder:
[0061] At room temperature, p-phenylenediamine (43.20 kg) is added to a MEPA solution (350 kg) containing 1% by mass of calcium chloride, stirred at 25°C for 1 hour under nitrogen protection, cooled to 5°C, and then terephthaloyl chloride (81.04 kg) is added in two batches, with an interval of 60 minutes between the batches (the mass ratio of the first batch of terephthaloyl chloride to the second batch is 60:40). After the reaction is completed, it is neutralized with a 40% sodium hydroxide aqueous solution, and then washed with water in multiple stages, ground, and dried to obtain a polymer powder. When the polymer powder is dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C is 9.2 dL / g, and the particle size distribution is: Dv (10): 81 μm, Dv (50): 362 μm, Dv (90): 658 μm.
[0062] (2) Preparation of spinning solution:
[0063] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 98%, and kept at 100°C to obtain a spinning solution, in which the mass content of the polymer powder is 25%.
[0064] (3) Dry-jet wet spinning process:
[0065] The spinning solution was extruded from the spinneret by a gear pump, the air bath height was 2 mm, and the drafting ratio was 5 times. Then it was formed by a coagulation bath, the coagulation bath composition was a concentrated sulfuric acid aqueous solution with a mass fraction of 5%, and the temperature was 30 ℃; neutralized by a 17% sodium hydroxide aqueous solution, washed with a water bath (residence time 10 s); then dried at 200 ℃ (residence time 3s), entered the 450 ℃ hot drawing process (residence time 2s), and finally oiled and wound into a tube to obtain para-aramid fiber.
[0066] The linear density of the para-aramid fibers is 1680 dtex, the tensile strength is 29.4 cN / dtex, the elongation at break is 3.5%, the elastic modulus is 780 cN / dtex, and the calcium ion content is zero.
[0067] Example 3
[0068] (1) Preparation of polymer powder:
[0069] At room temperature, p-phenylenediamine (43.20 kg) was added to a MIPA solution (350 kg) containing 1% calcium chloride by mass, stirred at 25°C for 1 hour under nitrogen protection, cooled to 0°C, and then terephthaloyl chloride (81.36 kg) was added in two batches, with a batch interval of 15 minutes (the mass ratio of the first batch of terephthaloyl chloride to the second batch was 30:70). After the reaction was completed, it was neutralized with a 40% sodium hydroxide aqueous solution, and then washed with water in multiple stages, ground, and dried to obtain a polymer powder. When the polymer powder was dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C was 9.2 dL / g, and the particle size distribution was: Dv (10): 85 μm, Dv (50): 375 μm, Dv (90): 686 μm.
[0070] (2) Preparation of spinning solution:
[0071] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 98%, and the solution is kept at 80°C to obtain a spinning solution, wherein the mass content of the polymer powder in the spinning solution is 19%.
[0072] (3) Dry-jet wet spinning process:
[0073] The spinning solution was extruded from the spinneret by a gear pump, the air bath height was 10 mm, and the drafting ratio was 12 times. Then it was formed by a coagulation bath, the coagulation bath composition was a concentrated sulfuric acid aqueous solution with a mass fraction of 10%, and the temperature was 30 ℃; neutralized by a 17% potassium hydroxide aqueous solution, and washed with a water bath (residence time 10 s); then dried at 150 ℃, entered the 300 ℃ hot drawing process, and finally oiled and wound into a tube to obtain para-aramid fiber.
[0074] The linear density of the para-aramid fibers is 1450 dtex, the tensile strength is 29.5 cN / dtex, the elongation at break is 3.7%, the elastic modulus is 790 cN / dtex, and the calcium ion content is zero.
[0075] Example 4
[0076] (1) Preparation of polymer powder:
[0077] At room temperature, p-phenylenediamine (43.20 kg) is added to a MBPA solution (350 kg) containing 1% calcium chloride by mass, stirred at 25°C for 1 hour under nitrogen protection, cooled to 0°C, and then terephthaloyl chloride (81.20 kg) is added in two batches, with a batch interval of 30 minutes (the mass ratio of the first batch of terephthaloyl chloride to the second batch is 40:60). After the reaction is completed, it is neutralized with a 40% potassium hydroxide aqueous solution, and then washed with water in multiple stages, ground, and dried to obtain a polymer powder. When the polymer powder is dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C is 9.3 dL / g, and the particle size distribution is: Dv (10): 65 μm, Dv (50): 338 μm, Dv (90): 636 μm.
[0078] (2) Preparation of spinning solution:
[0079] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 98%, and the solution is kept at 90°C to obtain a spinning solution, wherein the mass content of the polymer powder in the spinning solution is 20%.
[0080] (3) Dry-jet wet spinning process:
[0081] The spinning solution was extruded from the spinneret by a gear pump, the air bath height was 9 mm, and the drafting ratio was 7 times. Then it was formed by a coagulation bath, the coagulation bath composition was a concentrated sulfuric acid aqueous solution with a mass fraction of 12%, and the temperature was 30 ℃; neutralized by a 17% sodium hydroxide aqueous solution, and washed with a water bath (residence time 10 s); then dried at 150 ℃, entered the 350 ℃ hot drawing process, and finally oiled and wound into a tube to obtain para-aramid fiber.
[0082] The linear density of the para-aramid fibers is 1580 dtex, the tensile strength is 29.2 cN / dtex, the elongation at break is 4.2%, the elastic modulus is 766 cN / dtex, and the calcium ion content is zero.
[0083] Example 5
[0084] (1) Preparation of polymer powder:
[0085] At room temperature, p-phenylenediamine (43.20 kg) is added to a MMPA solution (350 kg) containing 2% by mass of calcium chloride, stirred at 25°C for 1 hour under nitrogen protection, cooled to -5°C, and then terephthaloyl chloride (81.20 kg) is added in two batches, with a batch interval of 30 minutes (the molar ratio of the first batch of terephthaloyl chloride added to the second batch is 50:50). After the reaction is completed, it is neutralized with a 40% sodium hydroxide aqueous solution, and then washed with water in multiple stages, ground, and dried to obtain a polymer powder. When the polymer powder is dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C is 9.5 dL / g, and the particle size distribution is: Dv (10): 79 μm, Dv (50): 350 μm, Dv (90): 656 μm.
[0086] (2) Preparation of spinning solution:
[0087] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 99.8%, and kept at 90°C to obtain a spinning solution, in which the mass content of the polymer powder is 22%.
[0088] (3) Dry-jet wet spinning process:
[0089] The spinning solution was extruded from the spinneret by a gear pump, the air bath height was 9 mm, and the drafting ratio was 7 times. Then it was formed by a coagulation bath, the coagulation bath composition was a concentrated sulfuric acid aqueous solution with a mass fraction of 5%, the temperature was 30 ℃; neutralized by a 17% sodium hydroxide aqueous solution, washed with a water bath (residence time 10 s); then dried at 150 ℃, entered the 350 ℃ hot drawing process, and finally oiled and wound into a tube to obtain para-aramid fiber.
[0090] The linear density of the para-aramid fibers is 1580 dtex, the tensile strength is 28.6 cN / dtex, the elongation at break is 3.9%, the elastic modulus is 798 cN / dtex, and the calcium ion content is zero.
[0091] Comparative Example 1
[0092] The para-aramid fiber was prepared by the same method as in Example 1, except that NMP solvent was used in the preparation of the polymer powder, and the water washing time was 60 s. It was found in the experiment that when NMP solvent was used, the solubility of p-phenylenediamine was poor, so a large amount of co-solvent calcium chloride needed to be added. The specific preparation process was as follows:
[0093] (1) Preparation of polymer powder:
[0094] At room temperature, p-phenylenediamine (43.20 kg) was added to NMP solvent (350 kg) containing 9% by mass of calcium chloride, stirred at 25°C for 1 hour under nitrogen protection, cooled to -5°C, and then terephthaloyl chloride (81.20 kg) was added in two batches, with a batch interval of 30 minutes (the mass ratio of the first batch of terephthaloyl chloride added to the second batch was 50:50). After the reaction was completed, it was neutralized with a 40% sodium hydroxide aqueous solution, and then washed with multiple stages of water (residence time 60 s), ground, and dried to obtain a polymer powder. When the polymer powder is dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C is 7.0 dL / g, and the particle size distribution is: Dv (10): 111 μm, Dv (50): 527 μm, Dv (90): 1240 μm.
[0095] (2) Preparation of spinning solution:
[0096] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 98%, and the solution is kept at 90°C to obtain a spinning solution, wherein the mass content of the polymer powder in the spinning solution is 22%.
[0097] (3) Dry-jet wet spinning process:
[0098] The spinning solution is squeezed out from the spinneret by a gear pump, the air bath height is 9 mm, and the drafting ratio is 7 times. Then it is formed by a coagulation bath, the coagulation bath composition is a concentrated sulfuric acid aqueous solution with a mass fraction of 5%, and the temperature is 30 ℃; neutralized by a 17% sodium hydroxide aqueous solution, washed with a water bath; then dried at 150 ℃, entered the 350 ℃ hot drawing process, and finally oiled and wound into a tube to obtain para-aramid fiber.
[0099] The linear density of the para-aramid fibers is 1580 dtex, the tensile strength is 19.6 cN / dtex, the elongation at break is 3.0%, the elastic modulus is 550 cN / dtex, and the calcium ion content is zero.
[0100] From the experimental comparison of Example 1 and Comparative Example 1, it can be found that due to the addition of an oxygen heteroatom, the hydrogen bond interaction between the amide solvent and the aramid polymer macromolecular chain is stronger than the interaction between NMP and the macromolecular chain, so the new amide solvent has a stronger dissolving ability, which leads to a delayed precipitation time of the polymer in the solvent, and the molecular weight of the polymer is larger than when NMP is used as a solvent, thereby significantly improving the mechanical properties of the fiber. In addition, due to the enhanced dissolving ability of the new amide solvent, the amount of calcium chloride required as a co-solvent is greatly reduced, saving production costs.
[0101] Comparative Example 2
[0102] The para-aramid fiber was prepared by the same method as in Example 1, except that NMP solvent was used in the preparation of the polymer powder. The specific preparation process is as follows:
[0103] (1) Preparation of polymer powder:
[0104] At room temperature, p-phenylenediamine (43.20 kg) was added to NMP solvent (350 kg) containing 9% by mass of calcium chloride, stirred at 25°C for 1 hour under nitrogen protection, cooled to -5°C, and then terephthaloyl chloride (81.20 kg) was added in two batches, with a batch interval of 30 minutes (the mass ratio of the first batch of terephthaloyl chloride added to the second batch was 50:50). After the reaction was completed, it was neutralized with a 40% sodium hydroxide aqueous solution, and then washed with multiple stages of water (residence time 10 s), ground, and dried to obtain a polymer powder. When the polymer powder is dissolved in concentrated sulfuric acid as a dissolving medium, the intrinsic viscosity range at 25°C is 7.0 dL / g, and the particle size distribution is: Dv (10): 120 μm, Dv (50): 650 μm, Dv (90): 1380 μm.
[0105] (2) Preparation of spinning solution:
[0106] The polymer powder is dissolved in a concentrated sulfuric acid solution with a mass fraction of 98%, and the solution is kept at 90°C to obtain a spinning solution, wherein the mass content of the polymer powder in the spinning solution is 22%.
[0107] (3) Dry-jet wet spinning process:
[0108] The spinning solution is squeezed out from the spinneret by a gear pump, the air bath height is 9 mm, and the drafting ratio is 7 times. Then it is formed by a coagulation bath, the coagulation bath composition is a concentrated sulfuric acid aqueous solution with a mass fraction of 5%, and the temperature is 30 ℃; neutralized by a 17% sodium hydroxide aqueous solution, washed with a water bath; then dried at 150 ℃, entered the 350 ℃ hot drawing process, and finally oiled and wound into a tube to obtain para-aramid fiber.
[0109] The linear density of the para-aramid fibers is 1580 dtex, the tensile strength is 19.3 cN / dtex, the elongation at break is 3.0%, the elastic modulus is 520 cN / dtex, and the residual calcium ion content in the fibers is 50 mg / L.
[0110] From the experimental comparison of Example 1 and Comparative Example 2, it can be found that: in step (1), when Example 1 and Comparative Example 2 use the same water washing time, the calcium ions in the fiber of Comparative Example 2 cannot be washed clean. It can be seen that the use of the amide solvent of the present invention for polymerization reaction has better solubility for the reaction raw materials, and only 1-2% of the cosolvent needs to be added to effectively reduce the residence time of water washing and the complexity of the water washing operation. In addition, from the performance indicators of the para-aramid fiber, it can be seen that the mechanical properties of the para-aramid fiber prepared by the preparation method of the present invention are more excellent, because the cosolvent is washed cleanly, so that the defects caused by the presence of the cosolvent in the fiber are fewer, and the mechanical properties of the fiber are better and more stable.
[0111] The polymer powder produced by the new amide solvent has a narrow intrinsic viscosity and a narrow particle size distribution, which makes the tensile strength and elastic modulus of the produced fiber stable, the coefficient of variation of related indicators is small, and the hair phenomenon is significantly reduced. This saves production costs, improves production efficiency, and is conducive to large-scale production.
[0112] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0113] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing para-aramid fiber, characterized in that: The preparation method comprises: performing polymerization reaction between p-phenylenediamine and terephthaloyl chloride in an amide solvent, and obtaining polymer powder through post-treatment after the reaction is completed; dissolving the polymer powder in concentrated sulfuric acid to obtain spinning solution; and obtaining the p-aramid fiber through dry-jet wet spinning of the spinning solution. The amide solvent is at least one of the following structural formulas: ; R 1 , R 2 , R 3 Each independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl; Inorganic salt calcium chloride is added as a co-solvent during the polymerization reaction, and the mass fraction of the co-solvent in the amide solvent is 1-2%.
2. The method for preparing para-aramid fiber according to claim 1, characterized in that: The amide solvent is selected from at least one of 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-propoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; The purity of the amide solvent is greater than 95%, and the water content is less than 700 ppm.
3. The method for preparing para-aramid fiber according to claim 1, characterized in that: When concentrated sulfuric acid is used as a dissolving medium for the polymer powder, the intrinsic viscosity at 25° C. is in the range of 9.0-9.5 dL / g.
4. The method for preparing para-aramid fiber according to claim 1, characterized in that: The polymerization reaction temperature is -5 to 5°C; the molar ratio of the amount of terephthaloyl chloride added to the amount of p-phenylenediamine added is (0.998-1.002):1; During the polymerization reaction, terephthaloyl chloride is added into the reaction system in two batches, the weight of the first batch is 30-60% of the total amount, and the weight of the second batch is 40-70% of the total amount.
5. The method for preparing para-aramid fiber according to claim 1, characterized in that: The temperature at which the concentrated sulfuric acid dissolves the polymer powder is 80-100°C; the mass content of the polymer powder in the spinning solution is 19%-25%.
6. The method for preparing para-aramid fiber according to claim 1, characterized in that: The dry-jet wet spinning process is as follows: the spinning solution is squeezed out from the spinneret by a gear pump, stretched by an air layer, coagulated and formed in a coagulation bath, and then the tow is washed with water, washed with alkali, washed with water again, and then dried, hot stretched, oiled, and rolled to obtain the para-aramid fiber.
7. The method for preparing para-aramid fiber according to claim 6, characterized in that: During the air layer stretching, the air bath height is 2-10 mm and the stretching multiple is 5-12 times; The coagulation bath is a dilute sulfuric acid solution, and the mass concentration of the dilute sulfuric acid solution is not greater than 15%.
8. The method for preparing para-aramid fiber according to claim 6, characterized in that: The drying temperature is 150-200°C, and the heat drawing temperature is 300-450°C.
9. A para-aramid fiber, characterized in that: The para-aramid fiber is prepared by the preparation method according to any one of claims 1 to 8; The tensile strength of the para-aramid fiber is 27.6-29.5 cN / dtex, the elongation at break is 3.5-4.2%, and the elastic modulus is 758-798 cN / dtex.