A method for preparing high-performance polyamide fiber
By adding epoxidized phenolic resin, aminated carbon nanotubes and silicon-containing hyperbranched polymers to polyamide fibers for melt blending and injection molding, the problem of insufficient mechanical and flame retardant properties of polyamide fibers was solved and high-performance fibers were realized. preparation.
Patent Information
- Application Number
- CN202410805466.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Existing polyamide fibers have deficiencies in mechanical properties and flame retardant properties, making it difficult to meet high-performance requirements.
Polyamide fiber, epoxidized phenolic resin, aminated carbon nanotubes and silicon-containing hyperbranched polymer are melt-blended and extruded in a twin-screw extruder, and then injection molded with an injection molding machine to form high-performance polyamide fiber .
By forming a stable cross-linked network and winding structure, the mechanical properties of polyamide fiber are significantly improved, and its flame retardant properties are enhanced through the combination of phenolic resin and carbon nanotubes.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyamide fibers, in particular to a method for preparing high-performance polyamide fibers. Background Art
[0002] Polyamide fiber is commonly known as polyamide fiber (commonly known as nylon), with a density of 1.15 g / cm3; it is a general term for thermoplastic resins containing repeated amide groups — [NHCO] — on the main chain of the molecule. It includes aliphatic PA, aliphatic-aromatic PA and aromatic PA. Among them, aliphatic PA has many varieties, large output and wide application. Its name is determined by the specific number of carbon atoms in the synthetic monomer.
[0003] The use of polymers such as thermoplastic resins and hyperbranched polymers to fill and modify nylon 6 is a research hotspot. The document "Preparation and Application of Hyperbranched Polyesters in Plastic Processing" reports that a nylon-6 / glass fiber composite material modified with a new type of carboxyl-terminated hyperbranched polyester increases the interface interaction and compatibility of the composite material. The tensile strength and other properties of the composite material are improved. The present invention uses hyperbranched polyester to improve the tensile properties of polyamide fibers. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing high-performance polyamide fibers, which have good mechanical properties and flame retardant properties.
[0006] (II) Technical solution
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a method for preparing high-performance polyamide fiber, comprising the following steps: adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer into a twin-screw extruder, melt-blending and extruding at 230-250° C., and then injection molding with an injection molding machine to obtain high-performance polyamide fiber.
[0008] Preferably, the mass ratio of the polyamide fiber, the epoxidized phenolic resin, the amino carbon nanotubes, and the silicon-containing hyperbranched polymer is 100:0.2-0.5:1-2:3-6.
[0009] Preferably, the preparation method of the silicon-containing hyperbranched polymer is:
[0010] (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, then add stannous octoate, and react at 110-130°C for 3-8 hours. After the reaction is completed, dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation 3-5 times, and vacuum dry the product to obtain hydroxylated tricyclodecane;
[0011] (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer;
[0012] (3) Add phosphorus oxychloride and pentaerythritol methyl silicate into a flask containing acetonitrile solvent, introduce nitrogen protection, stir and disperse, react at 60-90°C for 6-12h, filter while hot, evaporate the solvent from the filtrate, and cool to room temperature to obtain modified pentaerythritol methyl silicate;
[0013] (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, reacting at 30-60°C for 6-12 hours to carry out substitution reaction, and then performing reduced pressure distillation, filtering and drying to obtain terminal hydroxy silicone oil;
[0014] (5) Adding terminal hydroxyl silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, adding p-toluenesulfonic acid catalyst, and after reaction, precipitating, filtering, and washing to obtain silicon-containing hyperbranched polymer.
[0015] Preferably, the mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate in (1) is 1:1.1-1.3:0.01-0.03.
[0016] Preferably, the mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide in (2) is 1.1-1.3:1:0.02-0.04:0.01-0.02.
[0017] Preferably, the mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate in (3) is 1.2-1.5:1.
[0018] Preferably, the mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil in (4) is 0.8-1.2:1.
[0019] Preferably, the (5) mid-terminal hydroxyl silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are 1.2-1.5:1:0.02-0.03.
[0020] 3. Beneficial technical effects
[0021] The invention prepares high-performance polyamide fiber by adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotube and silicon-containing hyperbranched polymer into a twin-screw extruder, melting and blending and extruding, and then injection molding by an injection molding machine.
[0022] During the melt blending process, the epoxy groups in the epoxidized phenolic resin will undergo a ring-opening reaction with the amino groups in the amino carbon nanotubes and the hydroxyl groups in the silicon-containing hyperbranched polymer, forming a stable cross-linked network between the three, which work together to increase the mechanical properties of the polyamide fiber. The long chains in the silicon-containing hyperbranched polymer will entangle with the polyamide fiber, making it more tightly connected and enhancing its mechanical properties. In addition, the phenolic resin and carbon nanotubes themselves have good mechanical properties and flame retardant properties. DETAILED DESCRIPTION
[0023] Preparation method of pentaerythritol methyl silicate: add 0.1 mol of pentaerythritol and 0.1 mol of methyltrimethoxysilane to diethylene glycol dimethyl ether, stir and disperse, heat to 165°C, reflux for 6 hours, and after the reaction is completed, cool to room temperature, filter, and dry to obtain pentaerythritol methyl silicate.
[0024] The preparation reaction process of epoxy phenolic resin is as follows: 2g phenolic resin and 2.6g epichlorohydrin are mixed evenly, reacted at 75°C for 6h, and then concentrated and washed under reduced pressure to obtain epoxy phenolic resin. Embodiment 1:
[0025] (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, and then add stannous octoate, wherein the mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate is 1:1.1:0.01, react at 110°C for 3 hours, and after the reaction is completed, first dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation for 3 times, and vacuum dry the product to obtain hydroxylated tricyclodecane;
[0026] (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, and then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, wherein the mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine, and N,N-dicyclohexylcarbodiimide is 1.1:1:0.02:0.01, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer;
[0027] (3) Phosphorus oxychloride and pentaerythritol methyl silicate are added into a flask containing acetonitrile solvent, wherein the mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate is 1.2:1, nitrogen is introduced for protection, the mixture is stirred and dispersed, reacted at 60°C for 6 hours, filtered while hot, the solvent is evaporated from the filtrate, and cooled to room temperature to obtain modified pentaerythritol methyl silicate;
[0028] (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, wherein the mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil is 0.8:1, reacting at 30° C. for 6 hours to carry out substitution reaction, and then performing reduced pressure distillation after completion, filtering and drying to obtain terminal hydroxy silicone oil;
[0029] (5) adding terminal hydroxyl silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst, wherein the terminal hydroxyl silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are in a ratio of 1.2:1:0.02, and after reaction, precipitating, filtering, and washing to obtain a silicon-containing hyperbranched polymer;
[0030] (6) Adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer into a twin-screw extruder, wherein the mass ratio of polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer is 100:0.2:1:3, melt-blending and extruding at 230° C., and then injection molding by an injection molding machine to obtain high-performance polyamide fiber. Embodiment 2:
[0031] (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, and then add stannous octoate, wherein the mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate is 1:1.3:0.03, react at 130°C for 8 hours, and after the reaction is completed, first dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation for 5 times, and vacuum dry the product to obtain hydroxylated tricyclodecane;
[0032] (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, and then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, wherein the mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine, and N,N-dicyclohexylcarbodiimide is 1.3:1:0.04:0.02, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer;
[0033] (3) Phosphorus oxychloride and pentaerythritol methyl silicate are added into a flask containing acetonitrile solvent, wherein the mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate is 1.5:1, nitrogen is introduced for protection, the mixture is stirred and dispersed, reacted at 90° C. for 12 h, filtered while hot, the solvent is evaporated from the filtrate, and cooled to room temperature to obtain modified pentaerythritol methyl silicate;
[0034] (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, wherein the mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil is 1.2:1, reacting at 60° C. for 12 hours to carry out substitution reaction, and then performing reduced pressure distillation after completion, filtering and drying to obtain terminal hydroxy silicone oil;
[0035] (5) adding terminal hydroxyl silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst, wherein the terminal hydroxyl silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are in a ratio of 1.5:1:0.03, and after reaction, precipitating, filtering, and washing to obtain a silicon-containing hyperbranched polymer;
[0036] (6) Adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer into a twin-screw extruder, wherein the mass ratio of polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer is 100:0.5:2:6, melt-blending and extruding at 250°C, and then injection molding by an injection molding machine to obtain high-performance polyamide fiber. Embodiment 3:
[0037] (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, and then add stannous octoate, wherein the mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate is 1:1.2:0.02, react at 120°C for 5.5 hours, and after the reaction is completed, first dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation for 4 times, and vacuum dry the product to obtain hydroxylated tricyclodecane;
[0038] (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, and then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, wherein the mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine, and N,N-dicyclohexylcarbodiimide is 1..2:1:0.03:0.015, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer;
[0039] (3) Phosphorus oxychloride and pentaerythritol methyl silicate are added into a flask containing acetonitrile solvent, wherein the mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate is 1.35:1, nitrogen is introduced for protection, the mixture is stirred and dispersed, reacted at 75°C for 9 hours, filtered while hot, the solvent is evaporated from the filtrate, and cooled to room temperature to obtain modified pentaerythritol methyl silicate;
[0040] (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, wherein the mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil is 1.0:1, reacting at 45° C. for 9 hours to carry out substitution reaction, and then performing reduced pressure distillation after completion, filtering and drying to obtain terminal hydroxy silicone oil;
[0041] (5) Adding terminal hydroxyl silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, adding p-toluenesulfonic acid catalyst, wherein the terminal hydroxyl silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are 1.35:1:0.025, and after reaction, precipitating, filtering, and washing to obtain a silicon-containing hyperbranched polymer;
[0042] (6) Adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer into a twin-screw extruder, wherein the mass ratio of polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer is 100:0.35:1.5:4.5, melt-blending and extruding at 240° C., and then injection molding by an injection molding machine to obtain high-performance polyamide fiber. Embodiment 4:
[0043] (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, and then add stannous octoate, wherein the mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate is 1:1.1:0.01, react at 110°C for 3 hours, and after the reaction is completed, first dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation for 3 times, and vacuum dry the product to obtain hydroxylated tricyclodecane;
[0044] (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, and then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, wherein the mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine, and N,N-dicyclohexylcarbodiimide is 1.1:1:0.02:0.01, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer;
[0045] (3) Phosphorus oxychloride and pentaerythritol methyl silicate are added into a flask containing acetonitrile solvent, wherein the mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate is 1.5:1, nitrogen is introduced for protection, the mixture is stirred and dispersed, reacted at 90° C. for 12 h, filtered while hot, the solvent is evaporated from the filtrate, and cooled to room temperature to obtain modified pentaerythritol methyl silicate;
[0046] (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, wherein the mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil is 1.2:1, reacting at 60° C. for 12 hours to carry out substitution reaction, and then performing reduced pressure distillation after completion, filtering and drying to obtain terminal hydroxy silicone oil;
[0047] (5) Adding terminal hydroxyl silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, adding p-toluenesulfonic acid catalyst, wherein the terminal hydroxyl silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are 1.35:1:0.025, and after reaction, precipitating, filtering, and washing to obtain a silicon-containing hyperbranched polymer;
[0048] (6) Adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer into a twin-screw extruder, wherein the mass ratio of polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer is 100:0.35:1.5:4.5, melt-blending and extruding at 240° C., and then injection molding by an injection molding machine to obtain high-performance polyamide fiber. Embodiment 5:
[0049] (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, and then add stannous octoate, wherein the mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate is 1:1.3:0.03, react at 130°C for 8 hours, and after the reaction is completed, first dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation for 5 times, and vacuum dry the product to obtain hydroxylated tricyclodecane;
[0050] (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, and then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, wherein the mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine, and N,N-dicyclohexylcarbodiimide is 1.3:1:0.04:0.02, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer;
[0051] (3) Phosphorus oxychloride and pentaerythritol methyl silicate are added into a flask containing acetonitrile solvent, wherein the mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate is 1.35:1, nitrogen is introduced for protection, the mixture is stirred and dispersed, reacted at 75°C for 9 hours, filtered while hot, the solvent is evaporated from the filtrate, and cooled to room temperature to obtain modified pentaerythritol methyl silicate;
[0052] (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, wherein the mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil is 1.0:1, reacting at 45° C. for 9 hours to carry out substitution reaction, and then performing reduced pressure distillation after completion, filtering and drying to obtain terminal hydroxy silicone oil;
[0053] (5) adding terminal hydroxyl silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst, wherein the terminal hydroxyl silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are in a ratio of 1.2:1:0.02, and after reaction, precipitating, filtering, and washing to obtain a silicon-containing hyperbranched polymer;
[0054] (6) Adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer into a twin-screw extruder, wherein the mass ratio of polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes, and silicon-containing hyperbranched polymer is 100:0.2:1:3, melt-blending and extruding at 230° C., and then injection molding by an injection molding machine to obtain high-performance polyamide fiber.
[0055] Comparative Example 1
[0056] Compared with Example 5, no silicon-containing hyperbranched polymer was added, and other raw material components were the same.
[0057] Comparative Example 2
[0058] Compared with Example 5, no silicon-containing hyperbranched polymer, epoxidized phenolic resin, and amino carbon nanotubes were added, and other raw material components were the same.
[0059] The tensile properties of polyamide fiber were tested by a universal material testing machine. The test results are shown in Table 1.
[0060] Table 1: Tensile properties tested.
[0061]
[0062] It can be seen from Table 1 that the present invention has good mechanical properties.
[0063] The oxygen index was determined according to the method specified in GB / T2406-2008. The flame retardant grade was tested according to UL94-2009 standard. FV-0: the burning time does not exceed 10 seconds and does not ignite the absorbent cotton. FV-1: the burning time does not exceed 30 seconds and does not ignite the absorbent cotton. FV-2: the burning time does not exceed 30 seconds and ignites the absorbent cotton. The test results are shown in Table 2.
[0064] Table 2: Flame retardancy tests.
[0065]
[0066] It can be seen from Table 2 that the polyamide fiber of the present invention has good flame retardant properties.
[0067] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing high-performance polyamide fiber, characterized in that: The method comprises the following steps: adding polyamide fiber, epoxidized phenolic resin, amino carbon nanotubes and silicon-containing hyperbranched polymer into a twin-screw extruder, melt-blending and extruding at 230-250° C., and then injection molding with an injection molding machine to obtain high-performance polyamide fiber; The mass ratio of the polyamide fiber, the epoxidized phenolic resin, the amino carbon nanotubes, and the silicon-containing hyperbranched polymer is 100:0.2-0.5:1-2:3-6; The preparation method of the silicon-containing hyperbranched polymer is: (1) Add tricyclodecane dimethanol and ε-caprolactone into a reactor and stir evenly, introduce nitrogen, then add stannous octoate, and react at 110-130°C for 3-8 hours. After the reaction is completed, dissolve the crude product with chloroform, then precipitate with anhydrous ether, repeat the dissolution and precipitation 3-5 times, and vacuum dry the product to obtain hydroxylated tricyclodecane; (2) dissolving nitrilotriacetic acid and hydroxylated tricyclodecane in a reaction solvent, then adding 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide, and after the reaction, precipitating, filtering, and washing to obtain a carboxyl hyperbranched polymer; (3) Add phosphorus oxychloride and pentaerythritol methyl silicate into a flask containing acetonitrile solvent, introduce nitrogen protection, stir and disperse, react at 60-90°C for 6-12h, filter while hot, evaporate the solvent from the filtrate, and cool to room temperature to obtain modified pentaerythritol methyl silicate; (4) Adding modified pentaerythritol methyl silicate and hydroxy silicone oil to N,N-dimethylformamide solvent, reacting at 30-60°C for 6-12 hours to carry out substitution reaction, and then performing reduced pressure distillation, filtering and drying to obtain terminal hydroxy silicone oil; (5) adding hydroxy-terminated silicone oil and carboxyl hyperbranched polymer to N,N-dimethylformamide solvent, stirring evenly, adding p-toluenesulfonic acid catalyst, precipitating, filtering and washing after reaction to obtain silicon-containing hyperbranched polymer; The mass ratio of tricyclodecane dimethanol, ε-caprolactone and stannous octoate in (1) is 1:1.1-1.3:0.01-0.03; The mass ratio of nitrilotriacetic acid, hydroxylated tricyclodecane, 4-dimethylaminopyridine and N,N-dicyclohexylcarbodiimide in (2) is 1.1-1.3:1:0.02-0.04:0.01-0.02; The mass ratio of phosphorus oxychloride to pentaerythritol methyl silicate in (3) is 1.2-1.5:
1.
2. The method for preparing high-performance polyamide fiber according to claim 1, characterized in that: The mass ratio of modified pentaerythritol methyl silicate to hydroxy silicone oil in (4) is 0.8-1.2:
1.
3. The method for preparing high-performance polyamide fiber according to claim 1, characterized in that: The (5) mid-terminal hydroxy silicone oil, carboxyl hyperbranched polymer, and p-toluenesulfonic acid catalyst are 1.2-1.5:1:0.02-0.03.
Citation Information
Patent Citations
Water-based polycarbodiimide as well as preparation method and application thereof
CN114920896A
Method for manufacturing resin pattern, method for manufacturing conductive pattern and laminate
CN116149134A