A titanium alloy salt spray corrosion resistance test device and test method

By designing a titanium alloy salt spray corrosion resistance test device to simulate the salt spray airflow in the marine environment to conduct corrosion tests on titanium alloy samples, the problem of testing the salt spray corrosion resistance of titanium alloys in the marine environment has been solved, and the testing of titanium alloy materials has been realized. accurate evaluation and application guidance.

CN118376568BActive Publication Date: 2024-10-01CHINA STATE SHIPBUILDING CORP LTD RESEARCH INSTITUTE 719
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410783386.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

In a marine environment, titanium alloy high-pressure air bottles are susceptible to salt spray corrosion. It is difficult to effectively detect its salt spray corrosion resistance with existing technology, which affects the application of the material.

Method used

A titanium alloy salt spray corrosion resistance test device was designed, including a container, a salt spray generating tube, a scour pipe and an air pipe, to simulate the salt spray airflow in the marine environment. By conducting salt spray erosion corrosion tests on titanium alloy samples, combined with The water bath controls the temperature to ensure the authenticity and consistency of test conditions.

Benefits of technology

It achieves accurate and fast detection of the corrosion resistance of titanium alloy materials in salt spray atmosphere, effectively guides its application in high-pressure air bottles in marine environments, and provides a test method that is closer to actual application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118376568B_ABST
    Figure CN118376568B_ABST
Patent Text Reader

Abstract

The invention discloses a titanium alloy salt spray corrosion resistance test device and test method, the test device comprises: a container, a receiving cavity for receiving liquid is formed inside the container, and the top and side of the container are respectively provided with an air outlet and an air inlet connected to the receiving cavity; a salt spray generating tube, which comprises an air inlet end and an air outlet end, and the air inlet end extends from the air outlet into the receiving cavity; a flushing tube, which is connected with the air outlet end of the salt spray generating tube, one end of the flushing tube forms a salt spray nozzle, and the other end of the flushing tube is used to connect an air compressor; an air pipe, one end of which extends from the air inlet into the receiving cavity, and the other end is exposed outside the receiving cavity, and is used to communicate with the external atmosphere. The titanium alloy salt spray corrosion resistance test device and test method of the invention can simulate the situation that the titanium alloy is corroded by salt spray under the air flow, can accurately and conveniently detect and evaluate the corrosion resistance of the titanium alloy under the salt spray atmosphere, and effectively guide the application of titanium alloy materials in the marine environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material testing and detection, and in particular to a titanium alloy salt spray corrosion resistance testing device and a testing method. Background Art

[0002] High-pressure air cylinders refer to bottled containers that store compressed air with a working pressure greater than or equal to 10MPa. Among them, titanium alloy cylinders made of titanium alloy have the advantages of light weight and high specific strength, and are the development direction of high-pressure gas cylinders in marine environments. Compared with conventional application environments, there are special environmental atmospheres such as salt spray in marine environments, which are more likely to cause corrosion to metal materials in the environment. Therefore, there are strict corrosion resistance requirements for materials used in marine environments. For ease of application, high-pressure air cylinders are usually inflated and replenished in coastal docks or air compressors are installed on ships to directly inflate and replenish high-pressure air cylinders. Due to the presence of salt spray atmosphere in the marine environment, during the inflation process of the high-pressure air cylinder, the compressed air will carry a large amount of salt spray. The compressed air carrying salt spray will continuously flush the high-pressure air cylinder body during the inflation process, causing salt spray scouring corrosion to the bottle body. Since different types of titanium alloys have different salt spray corrosion resistance, in order to screen out titanium alloy types with good salt spray scouring corrosion resistance suitable for the preparation of high-pressure air cylinders for marine environments, a test device and test method that can test the salt spray scouring corrosion resistance of titanium alloys is required. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a titanium alloy salt spray corrosion resistance test device and test method.

[0004] In a first aspect, the present application provides a titanium alloy salt spray corrosion resistance test device, the test device comprising:

[0005] A container, wherein a receiving cavity for receiving liquid is defined in the container, and a gas outlet and a gas inlet communicating with the receiving cavity are respectively provided on the top and the side of the container;

[0006] A salt mist generating tube, comprising an air inlet end and an air outlet end, wherein the air inlet end extends from the air outlet into the containing cavity;

[0007] A flushing pipe, which is connected to the gas outlet end of the salt mist generating pipe, one end of the flushing pipe forms a salt mist nozzle, and the other end of the flushing pipe is used to connect to an air compressor;

[0008] An air pipe, one end of which extends from the air inlet into the containing cavity and is immersed in the test liquid during the salt spray corrosion resistance test, and the other end of which is exposed outside the containing cavity and is used to communicate with the external atmosphere.

[0009] In one embodiment, the flushing pipe includes a first tube body and a second tube body that are connected to each other, one end of the first tube body away from the second tube body is connected to the air compressor, and a first control valve for controlling the flow of compressed air is provided on the first tube body, one end of the second tube body away from the first tube body forms a salt spray nozzle, and the air outlet end of the salt spray generating tube is connected to the first tube body;

[0010] Wherein, the second tube body and the first tube body form a first angle, and the first angle is 90° to 180°.

[0011] In one embodiment, the air pipe forms a second angle with the vertical center line of the container, and a second control valve for controlling the air flow is provided on the air pipe;

[0012] Wherein, the second angle is 40° to 50°.

[0013] In one embodiment, the salt mist generating pipe is provided with a third control valve for controlling the flow rate of the salt mist; and / or,

[0014] The test device also includes a water bath, and the container is placed in the water bath.

[0015] In a second aspect, the present application also provides a method for testing the salt spray corrosion resistance of titanium alloy, the method comprising the following steps:

[0016] Prepare the samples to be tested and record their appearance and quality;

[0017] Placing the sample in the test area, and using the titanium alloy salt spray corrosion resistance test device described in the first aspect to flush the surface of the sample with salt spray to conduct a corrosion test;

[0018] After the preset test time, the appearance of the sample after the test is recorded, and the sample is taken out from the test area and weighed to calculate the corrosion rate of the sample;

[0019] Based on the appearance comparison results of the sample before and after the test and the corrosion rate of the sample, the salt spray corrosion resistance of the sample was obtained.

[0020] In one embodiment, the step of preparing a sample to be tested comprises:

[0021] Cutting the titanium alloy material according to predetermined specifications to obtain titanium alloy sheets;

[0022] Grinding the surface to be tested of the titanium alloy sheet so that the roughness of the surface to be tested of the titanium alloy sheet reaches a preset value;

[0023] Clean and blow dry the surface of the titanium alloy sheet to be tested.

[0024] In one embodiment, the preset roughness value Ra of the surface to be tested of the titanium alloy sheet is 3.2μm.

[0025] In one embodiment, the step of using the titanium alloy salt spray corrosion resistance test device described in the first aspect to flush salt spray on the surface of the sample to perform a corrosion test comprises:

[0026] Injecting artificial seawater into the test device container, and controlling the temperature of the artificial seawater in the test device container to be between 33° C. and 37° C.;

[0027] Use an air compressor to pass compressed air into one end of the flushing tube to make the salt spray generating tube produce salt spray. The generated salt spray acts on the surface of the sample along with the compressed air.

[0028] In one embodiment, a spray angle of 30° to 40° is formed between the salt spray nozzle of the flushing pipe and the surface of the sample.

[0029] In one embodiment, the preset test duration is 200 hours to 230 hours.

[0030] Compared with the prior art, the above technical solution provided by this application has the following beneficial effects:

[0031] The titanium alloy salt spray corrosion resistance test device of the present application can generate a flushing airflow carrying a salt spray atmosphere, and can truly simulate the inflation airflow during the inflation process of a high-pressure air bottle in an actual marine environment. The test is closer to the actual application scenario. The titanium alloy salt spray corrosion resistance test device and test method of the present application can simulate the situation in which the titanium alloy is corroded by salt spray under the inflation airflow in a marine environment. The corrosion resistance of the titanium alloy under the salt spray atmosphere can be accurately, conveniently and quickly tested and evaluated, and the application of titanium alloy materials in high-pressure air bottles in marine environments can be effectively guided. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a structural schematic diagram of a titanium alloy salt spray corrosion resistance test device of the present application;

[0033] Figure 2 It is a flow chart of a titanium alloy salt spray corrosion resistance test method of the present application.

[0034] Numbers in the figure:

[0035] 10. Container; 10a. Receiving cavity; 20. Salt spray generating tube; 30. Flushing tube; 31. First tube body; 32. Second tube body; 40. Air tube; 50. Sample; 60. First control valve; 70. Second control valve; 80. Third control valve; a. First angle; b. Injection angle; c. Second angle. DETAILED DESCRIPTION

[0036] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific embodiments of the present invention are now described in detail with reference to the accompanying drawings. In the following description, it should be understood that the directions or positional relationships indicated by "front", "back", "up", "down", "left", "right", "longitudinal", "horizontal", "vertical", "horizontal", "top", "bottom", "inside", "outside", "head", "tail", etc. are based on the directions or positional relationships shown in the accompanying drawings, are constructed and operated in a specific direction, and are only for the convenience of describing the present technical solution, rather than indicating that the device or element referred to must have a specific direction, and therefore cannot be understood as a limitation to the present invention.

[0037] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0038] Titanium alloy is a metal material with excellent performance. It is widely used in aerospace, shipbuilding, chemical industry, medical equipment and other fields. High-pressure air cylinder refers to a bottled container that stores compressed air with a working pressure greater than or equal to 10MPa. High-pressure air cylinders are widely used in marine industry, marine navigation and other fields. Titanium alloy has a wide range of application prospects in the preparation of high-pressure gas cylinders in marine environments due to its excellent strength, heat resistance, corrosion resistance and other characteristics. In marine environment applications, the corrosive environment in which high-pressure air cylinders are located is more severe than that in conventional land environments, such as the salt spray atmosphere in the environment. In addition, when used in marine-related fields, for the convenience of application, high-pressure air cylinders are usually inflated and replenished in coastal docks or air compressors are installed on board to directly inflate and replenish high-pressure air cylinders. Due to the presence of salt spray atmosphere in the marine environment, during the inflation process of the high-pressure air cylinder, the compressed air will carry a large amount of salt spray. The compressed air carrying salt spray will continuously flush the high-pressure air cylinder body during the inflation process, causing salt spray scouring corrosion to the bottle body. Compared with the corrosion in static salt spray atmosphere, the corrosion caused by salt spray scouring to the bottle body material is more serious. In order to accurately and conveniently detect and evaluate the corrosion resistance of materials under salt spray atmosphere scouring conditions, so as to screen out titanium alloy materials that meet the requirements for the use of high-pressure air bottles in marine environments, this application provides a titanium alloy salt spray corrosion resistance test device and experimental method.

[0039] Please refer to Figure 1 The present application provides a titanium alloy salt spray corrosion resistance test device, which includes a container 10, a salt spray generating tube 20, a flushing tube 30 and an air tube 40.

[0040] Specifically, the interior of the container 10 is defined to form a accommodating cavity 10a for accommodating liquid, and the top and side of the container 10 are respectively provided with an air outlet and an air inlet connected to the accommodating cavity 10a; the salt spray generating tube 20 includes an air inlet end and an air outlet end, and its air inlet end extends from the air outlet of the container 10 into the accommodating cavity 10a; the flushing tube 30 is connected to the air outlet end of the salt spray generating tube 20, one end of the flushing tube 30 forms a salt spray nozzle and extends to the surface of the sample 50 to be tested, and the other end of the flushing tube 30 is used to connect to the air compressor; one end of the air pipe 40 extends from the air inlet of the container 10 into the accommodating cavity 10a and is immersed in the test liquid during the salt spray corrosion resistance test, and the other end is exposed outside the accommodating cavity 10a for communication with the external atmosphere.

[0041] Exemplarily, an air pipe 40 is extended from the air inlet of the container 10 into the container 10 so that the air pressure in the accommodating chamber 10a is the same as the atmospheric pressure, and then compressed air is introduced into the flushing pipe 30 by the air compressor. When the compressed air passes through the salt mist generating pipe 20, the pressure inside the container 10 is reduced. At this time, the air in the atmosphere enters the liquid (artificial seawater) in the container 10 through the air pipe 40, so that the liquid forms bubbles, and then a salt mist atmosphere is generated in the container 10. The generated salt mist enters the flushing pipe 30 through the salt mist generating pipe 20 and is sprayed from the salt mist nozzle at one end of the flushing pipe 30 with the compressed air to flush the surface of the test sample 50 to be tested. The test device can generate a flushing airflow carrying a salt mist atmosphere, and can truly simulate the inflation airflow during the inflation process of a high-pressure air bottle in an actual marine environment. The test is closer to the actual application scenario, and the test device has a simple structure and is easy to operate.

[0042] The above-mentioned test device can truly simulate the situation in which the titanium alloy material of the high-pressure air cylinder is corroded by the salt spray atmosphere during the inflation process of the high-pressure air cylinder in the actual marine environment, and test the salt spray corrosion resistance of the titanium alloy. It can more conveniently and quickly evaluate the salt spray corrosion resistance of the titanium alloy, and effectively guide the application of titanium alloy materials in related marine environment fields.

[0043] In one embodiment, the flushing pipe 30 includes a first tube body 31 and a second tube body 32 that are connected to each other. The end of the first tube body 31 away from the second tube body 32 is connected to the air compressor, and the first tube body 31 is provided with a first control valve 60 for controlling the flow of compressed air. The end of the second tube body 32 away from the first tube body 31 forms a salt spray nozzle and extends to the surface of the sample to be tested 50. The air outlet end of the salt spray generating tube 20 is connected to the first tube body 31; wherein the second tube body 32 and the first tube body 31 form a first angle a, and the first angle a is 90° to 180°.

[0044] Exemplarily, the scouring pipe 30 is formed by connecting a first tube body 31 and a second tube body 32, and the second tube body 32 forms a first angle a with the first tube body 31, so that the salt mist sprayed from the scouring pipe 30 can scour the test surface of the fixedly placed test sample 50 at a certain spray angle, so as to more realistically and accurately simulate the situation in which the titanium alloy material is corroded by the scouring of the salt mist atmosphere airflow under different application conditions in the marine environment (such as different inflation angles, different scouring angles), and can more accurately evaluate the salt mist scouring and corrosion resistance of the titanium alloy material in the marine environment.

[0045] In addition, the first control valve 60 may be a flow control valve, which can be used to control the amount of compressed air introduced by the air compressor to adjust the flow rate of the salt spray acting on the surface of the sample 50 to be tested.

[0046] Optionally, more than two second tube bodies 32 may be provided to test a plurality of samples simultaneously, so that a plurality of samples can be tested under the same test conditions, thereby improving the accuracy of the test and evaluation.

[0047] In one embodiment, the air pipe 40 forms a second angle c with the vertical center line of the container 10, and a second control valve 70 for controlling the air flow is provided on the air pipe 40; wherein the second angle c is 40° to 50°.

[0048] It should be noted that the vertical center line of the container 10 is a line passing through the midpoint of the container 10 in the vertical direction. It is a virtual reference line for the convenience of describing the angle at which the air tube 40 is inserted into the container 10. Figure 1 X-rays in.

[0049] Exemplarily, the air pipe 40 is used to balance the pressure in the container 10 with the atmospheric pressure, so that after the pressure in the container 10 is reduced, the air in the atmosphere enters the liquid from the air pipe 40 to generate bubbles, thereby forming a salt mist atmosphere. It should be noted that the air pipe 40 forms a second angle c of 40° to 50° with the vertical center line of the container 10, so that the air enters the liquid at an inclined angle, which makes it easier to generate bubbles, thereby stably generating salt mist.

[0050] In addition, the second control valve 70 may be a flow control valve, which can be used to control the amount of air entering the liquid to adjust the amount of salt mist generated in the container 10 .

[0051] In one embodiment, a third control valve 80 for controlling the flow rate of salt mist is provided on the salt mist generating pipe 20. The amount of salt mist entering the flushing pipe 30 can be controlled by the third control valve 80 to meet different test requirements.

[0052] In one embodiment, the test device further includes a water bath, and the container 10 is placed in the water bath to ensure that the temperature of the liquid in the container 10 is maintained within a certain range, such as 33° C. to 37° C. In this way, salt mist can be stably generated to avoid affecting the amount of salt mist generated due to too high or too low temperature, thereby affecting the accuracy of the test.

[0053] Please refer to Figure 2 The present application also provides a titanium alloy salt spray corrosion resistance test method, which is performed using the titanium alloy corrosion resistance test device of the above embodiment. The titanium alloy salt spray corrosion resistance test method comprises the following steps:

[0054] S100, prepare the sample to be tested, and record the appearance and quality of the sample.

[0055] Exemplarily, preparing the sample 50 to be tested may include determining factors such as the size of the sample, the roughness of the surface to be tested, and the shape, so as to ensure that no error occurs when testing different types of titanium alloys. In addition, it should be noted that the appearance of the sample can be recorded by taking a photo with a camera so that after the corrosion test is completed, the appearance of the sample before and after corrosion can be intuitively compared; similarly, the mass of the sample can be recorded by weighing it with a weighing device such as an electronic scale, so as to obtain the mass change during the corrosion process, thereby calculating the corrosion rate.

[0056] S200, placing the sample in the test area, and using the test device in the above embodiment to flush the surface of the sample with salt spray to perform a corrosion test.

[0057] S300, after the preset test time, the appearance of the sample after the test is recorded, and the sample is taken out from the test area for weighing, and the corrosion rate of the sample is calculated.

[0058] It should be noted that the "preset test duration" mentioned above is determined based on factors such as the service life of products made of titanium alloy materials (such as high-pressure gas cylinders) in the marine environment and the scouring angle they are subjected to, and is determined based on actual conditions.

[0059] For example, after the surface of the sample 50 to be tested is flushed with salt spray for a preset test time, the sample 50 is photographed with a camera, and then the corrosion condition can be visually observed by comparing the sample photograph before the corrosion test.

[0060] In addition, the sample 50 is weighed after corrosion in order to obtain the weight lost during the corrosion process, and then the corrosion rate of the sample is calculated based on the lost weight. For example, the test time t is preset, and the weight of the sample before the test is The weight of the sample after the test is , the corrosion rate of the sample can be calculated according to the following formula:

[0061] ;

[0062] Where: X-corrosion rate of the sample, unit: mm / h; -The weight of the sample before the test, in g; -The weight of the sample after the test, unit: g; A-the surface area of ​​the sample, unit: cm 2 ; t-preset test duration, unit: h; D-density of sample material, unit: g / cm 3 .

[0063] S400. Based on the appearance comparison results of the sample before and after the test and the corrosion rate of the sample, the salt spray corrosion resistance of the sample is obtained.

[0064] By using the above-mentioned titanium alloy salt spray corrosion resistance test device and test method, it is possible to simulate the situation in which the titanium alloy is corroded by salt spray under an inflated airflow in a marine environment. The corrosion resistance of the titanium alloy under the erosion of a salt spray atmosphere can be accurately, conveniently and quickly tested and evaluated, and the application of titanium alloy materials in high-pressure air cylinders in a marine environment can be effectively guided.

[0065] In one embodiment, the step of preparing a sample to be tested includes:

[0066] Cutting the titanium alloy material according to predetermined specifications to obtain titanium alloy sheets;

[0067] Grinding the surface to be tested of the titanium alloy sheet so that the roughness of the surface to be tested of the titanium alloy sheet reaches a preset value;

[0068] Clean and blow dry the surface of the titanium alloy sheet to be tested.

[0069] Exemplarily, the size of the sample is first determined, and then the titanium alloy material is cut according to the determined size to obtain a titanium alloy sheet that meets the size requirements. The surface of the titanium alloy sheet is then polished until the roughness of the surface to be tested of the titanium alloy sheet reaches a preset value. Finally, the surface to be tested is cleaned and dried to ensure that the influence of other factors is reduced during the salt spray corrosion resistance test. For example, when conducting multiple groups of comparison experiments, the roughness of the surface to be tested of the sample is different, resulting in different conditions of salt spray action on each sample when it is flushed with salt spray, which leads to errors in the corrosion resistance evaluation conclusion.

[0070] It should be noted that the cutting of titanium alloy materials can be automated by machines, which can effectively improve cutting efficiency and accuracy.

[0071] In one embodiment, the preset roughness value Ra of the surface to be tested of the titanium alloy sheet is 3.2μm.

[0072] In one embodiment, the steps of using the test device in the above embodiment to flush salt spray on the surface of the sample to perform a corrosion test include:

[0073] Inject artificial seawater into the test device container 10, and control the temperature of the artificial seawater in the test device container 10 to be between 33° C. and 37° C.;

[0074] Compressed air is introduced into one end of the flushing tube 30 by using an air compressor, so that the salt mist generating tube 20 generates salt mist, and the generated salt mist acts on the surface of the sample 50 along with the compressed air.

[0075] Exemplarily, the prepared artificial seawater is injected into the test device container 10, and then compressed air is introduced into one end of the flushing tube 30 by an air compressor. When the compressed air passes through the salt mist generating tube 20, the pressure inside the container 10 is reduced. At this time, the air in the atmosphere enters the artificial seawater in the container 10 through the air tube 40, so that the liquid forms bubbles, and then a salt mist atmosphere is generated in the container 10. The generated salt mist enters the flushing tube 30 through the salt mist generating tube 20 and is sprayed from the salt mist nozzle at one end of the flushing tube 30 with the compressed air to the test surface of the test sample 50, thereby realizing the use of salt mist to flush the test surface of the sample, thereby simulating the situation in which the titanium alloy is corroded by the salt mist atmosphere in the marine environment.

[0076] Exemplarily, the temperature of the artificial seawater in the container 10 is controlled at 33°C to 37°C to ensure that salt mist can be stably generated, so as to avoid affecting the amount of salt mist generated due to excessively high or low temperature, thereby affecting the accuracy of the test. In addition, it should be noted that the temperature of the artificial seawater in the container can be maintained by placing the entire container 10 in a warmer (such as a water bath). The above is only an example, but is not limited thereto.

[0077] In one embodiment, a spray angle b of 30° to 40° is formed between the salt spray nozzle of the scouring pipe 30 and the surface to be tested of the sample 50. In this way, the salt spray can be used to scour the surface to be tested of the sample at an inclination angle of 30° to 40°, so as to more realistically and accurately simulate the situation in which the titanium alloy material is corroded by the scouring of the salt spray atmosphere airflow under specific application conditions (such as specific inflation angles and specific scouring action angles) in the marine environment, and the salt spray scouring corrosion resistance of the titanium alloy material in the marine environment can be more accurately evaluated.

[0078] In one embodiment, the preset test time is 200 h to 230 h.

[0079] In order to facilitate the understanding of the above test method, the following is a specific description taking BTi431 titanium alloy material as an example.

[0080] Sample preparation: Cut the BTi431 titanium alloy material according to the size specifications of 120mm long, 60mm wide and 5mm thick, and grind the surface of the cut sample to be tested until the roughness Ra≤3.2μm;

[0081] Test content: (1) Record the shape and weight of the sample, and then place the sample in the test area; (2) Inject artificial seawater into the container, and then use an air compressor to pass compressed air with a pressure of 0.8MPa into one end of the flushing pipe to make the salt spray generating tube generate salt spray. The generated salt spray acts on the test surface of the sample with the compressed air flushing; (3) After the test lasts for 200h, stop flushing the test surface of the sample, record the shape and weight of the sample after the test, and calculate the corrosion rate of the sample; (4) Based on the comparison results of the appearance of the sample before and after the test and the corrosion rate, the salt spray corrosion resistance of BTi431 titanium alloy material is obtained.

[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A titanium alloy salt spray corrosion resistance test device, characterized in that: The test device includes: A container, wherein a receiving cavity for receiving liquid is defined in the container, and a gas outlet and a gas inlet communicating with the receiving cavity are respectively provided on the top and the side of the container; A salt mist generating tube, comprising an air inlet end and an air outlet end, wherein the air inlet end extends from the air outlet into the containing cavity; A flushing pipe, which is connected to the gas outlet end of the salt mist generating pipe, one end of the flushing pipe forms a salt mist nozzle, and the other end of the flushing pipe is used to connect to an air compressor; an air pipe, one end of which extends from the air inlet into the containing cavity and is immersed in the test liquid during the salt spray corrosion resistance test, and the other end of which is exposed outside the containing cavity and is used to communicate with the external atmosphere, so that after the pressure in the container is reduced, the air in the atmosphere enters the test liquid through the air pipe to generate bubbles, thereby forming a salt spray atmosphere; A water bath, wherein the container is placed in the water bath; The flushing pipe includes a first tube body and a second tube body that are connected and communicated, one end of the first tube body away from the second tube body is connected to the air compressor, one end of the second tube body away from the first tube body forms a salt spray nozzle, and the gas outlet end of the salt spray generating pipe is communicated with the first tube body; the second tube body and the first tube body form a first angle, and the first angle is 90° to 180°; The air pipe forms a second angle with the vertical center line of the container, and the second angle is 40° to 50°.

2. The titanium alloy salt spray corrosion resistance testing device according to claim 1 is characterized in that: The first pipe body is provided with a first control valve for controlling the flow of compressed air.

3. The titanium alloy salt spray corrosion resistance testing device according to claim 1, characterized in that: The air pipe is provided with a second control valve for controlling the air flow.

4. The titanium alloy salt spray corrosion resistance testing device according to claim 1, characterized in that: The salt mist generating pipe is provided with a third control valve for controlling the flow rate of the salt mist.

5. A method for testing the salt spray corrosion resistance of titanium alloy, characterized in that: The method comprises the following steps: Prepare the samples to be tested and record their appearance and quality; Placing the sample in the test area, and using the titanium alloy salt spray corrosion resistance test device according to any one of claims 1 to 4 to flush the surface of the sample with salt spray to conduct a corrosion test; After the preset test time, the appearance of the sample after the test is recorded, and the sample is taken out from the test area and weighed to calculate the corrosion rate of the sample; Based on the appearance comparison results of the sample before and after the test and the corrosion rate of the sample, the salt spray corrosion resistance of the sample was obtained.

6. The method for testing the titanium alloy's salt spray corrosion resistance according to claim 5, characterized in that: The step of preparing the sample to be tested comprises: Cutting the titanium alloy material according to predetermined specifications to obtain titanium alloy sheets; Grinding the surface to be tested of the titanium alloy sheet so that the roughness of the surface to be tested of the titanium alloy sheet reaches a preset value; Clean and blow dry the surface of the titanium alloy sheet to be tested.

7. The method for testing the titanium alloy's salt spray corrosion resistance according to claim 6, characterized in that: The preset roughness value of the surface to be tested of the titanium alloy sheet .

8. The method for testing the titanium alloy's salt spray corrosion resistance according to claim 5, characterized in that: The step of using the titanium alloy salt spray corrosion resistance test device according to any one of claims 1 to 4 to flush salt spray on the surface of the sample to conduct a corrosion test comprises: Injecting artificial seawater into the test device container, and controlling the temperature of the artificial seawater in the test device container to be between 33° C. and 37° C.; Use an air compressor to pass compressed air into one end of the flushing tube to make the salt spray generating tube produce salt spray. The generated salt spray acts on the surface of the sample along with the compressed air.

9. The method for testing the titanium alloy's salt spray corrosion resistance according to claim 8, characterized in that: A spray angle of 30° to 40° is formed between the salt spray nozzle of the flushing pipe and the surface to be tested of the sample.

10. The method for testing the titanium alloy's salt spray corrosion resistance according to claim 5, characterized in that: The preset test duration is 200h to 230h.

Citation Information

Patent Citations

  • Salt mist test box for batteries and use method of salt mist test box

    CN105547984A

  • Ultra-high cycle fatigue performance testing device

    CN113702218A

  • Jet spray type sample corrosion testing device and method under thin liquid film

    CN117740666A

  • Semi-automatic salt spray test device

    CN212364019U

  • Low-temperature circulating type salt spray corrosion testing device

    CN218481379U