Boiling water resistant adhesive and flame retardant prepared from biomass polyamine and application thereof

The reaction of maleic anhydride with polyamine and lactose is made into branched biomass adhesives, and combined with ATMP to prepare a full biomass adhesive with flame retardant properties, which solves the formaldehyde release problem in artificial boards and realizes the biomass glue Boiling water resistance and flame retardant effect meet the needs of the wood glue industry.

CN118388364BActive Publication Date: 2024-12-03KUNMING METALLURGY COLLEGE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410508091.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-12-03
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

There is a problem of formaldehyde release in existing artificial boards, which is a harmful and irritating carcinogen, which has led to an increase in the development demand for biomass glue, especially in the wood glue industry, seeking non-toxic and environmentally friendly biomass adhesives and flame retardant materials.

Method used

A full biomass adhesive and flame retardant liquid is prepared by reacting maleic anhydride with polyamine and lactose to form branched biomass polyamines and combined with aminotrimethylenephosphonic acid (ATMP) to improve the plywood Boiling water resistance and flame retardant properties. The method includes mixing maleic anhydride with methanol, stirring ultrasonic until dissolved, adding tetraethylenepentaamine and diethylenetriamine to react, then reacting with lactose to form an adhesive, and reacting with ATMP to prepare a flame retardant liquid.

Benefits of technology

It realizes a non-toxic and environmentally friendly biomass adhesive, has good dissolution properties and hot press curing capabilities, has flame retardant properties, meets the use requirements of wooden boards, and reduces the risk of formaldehyde release.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118388364B_ABST
    Figure CN118388364B_ABST
Patent Text Reader

Abstract

The present invention discloses a boiling water resistant adhesive and a flame retardant prepared from biomass polyamine and their application. The adhesive is obtained by reacting branched polyamine and lactose, and the mass ratio of the branched polyamine and lactose is 1:0.5-4. The present invention utilizes branched biomass polyamine and lactose to carry out Schiff base reaction, and the bonding strength and water resistance of the adhesive are significantly improved. The dry strength of plywood can reach more than 2MPa, and the strength can reach more than 1MPa after soaking in 63°C hot water and 93°C hot water. The present invention proposes a new type of adhesive using biomass as raw material and without the release of harmful gases such as formaldehyde, which is expected to replace petrochemical industrial glue with biomass glue and promote the development of biomass-based chemical industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a full-biomass adhesive based on maleic anhydride branched biomass polyamine and lactose, a flame retardant liquid prepared by using the branched polyamine and aminotrimethylenephosphonic acid (ATMP), and application of the flame retardant liquid in preparing multifunctional plywood, and belongs to the field of adhesives. Background Art

[0002] At present, the most commonly used wood-based panels are still urea-formaldehyde resin, melamine and melamine-urea-formaldehyde resin. In this case, the release of formaldehyde from wood-based panels and furniture becomes a serious problem, especially indoors. The reason why formaldehyde needs to be removed is that it exists in the product in a free state and is highly toxic. Formaldehyde is an irritant and a carcinogen, which can cause rhinitis, discomfort in the eyes, nose, throat, etc.

[0003] The harm of formaldehyde to human body has greatly promoted the development of biomass glue. Sugars account for a large proportion of the adhesives that can be used to make biomass. Among the disaccharides that have been reported, biomass adhesives with sucrose and glucose as the main raw materials have good mechanical properties and water resistance. They are all renewable energy sources. Lactose is similar to them, a disaccharide composed of one molecule of glucose and one molecule of galactose forming a glycosidic bond through the β-1,4 position. In addition, branched polyamines synthesized based on maleic anhydride are important "amine sources" participating in Schiff base reactions. Therefore, from the perspective of the chemical properties of the material, the development of non-toxic and environmentally friendly biomass glue is of great significance to the development of the current wood glue industry. Summary of the invention

[0004] The purpose of the present invention is to provide a boiling water resistant adhesive and flame retardant prepared from biomass polyamine and their application. The adhesive is prepared by reacting polyamine prepared from maleic anhydride with lactose to generate a branched high molecular polymer, which is used in plywood production to improve bonding strength, thereby achieving the purpose of boiling water resistance. The flame retardant is prepared by reacting branched polyamine developed based on maleic anhydride with aminotrimethylenephosphonic acid (ATMP) to prepare a flame retardant impregnation liquid, which is applied on the surface of plywood to make it have flame retardant properties, thereby achieving the purpose of flame retardancy.

[0005] The present invention first provides a method for preparing a branched polyamine, the steps of which are as follows:

[0006] (1) mixing maleic anhydride and methanol, and stirring by ultrasonication to completely dissolve the maleic anhydride;

[0007] (2) while stirring, slowly dropwise adding tetraethylenepentamine to maleic anhydride, and reacting at 70 to 90° C. for 1 to 5 hours;

[0008] The molar ratio of tetraethylenepentamine to maleic anhydride is 1:4-5;

[0009] (3) removing excess methanol solvent using a rotary evaporator, and then adding diethylenetriamine dropwise to the reaction mixture, and continuing to react at 100 to 120° C. for 1 to 5 hours in an open atmosphere, until the reaction is completed to obtain maleic branched biomass polyamine;

[0010] The molar ratio of tetraethylenepentamine to diethylenetriamine is 1:4-5;

[0011] (4) After the reaction is completed, the maleic branched biomass polyamine is cooled to room temperature, and deionized water is added according to its solid content of 50% to completely dissolve it, thereby obtaining the branched polyamine.

[0012] The present invention further provides a full biomass adhesive, which is obtained by reacting the branched polyamine and lactose, wherein the mass ratio of the branched polyamine to lactose is 1:0.5-4

[0013] Preferably, the mass ratio of the branched polyamine to lactose is 1:2.

[0014] Preferably, the reaction temperature of the branched polyamine and lactose is 70-90° C., and the reaction time of the branched polyamine and lactose is 1-6 hours.

[0015] Preferably, the all-biomass adhesive further comprises potassium persulfate and / or glycerol glycidyl ether;

[0016] The addition amount of potassium persulfate is 1%-8%;

[0017] The added amount of the glycerol glycidyl ether is 1%-3%.

[0018] The present invention also provides an application of the all-biomass adhesive in the preparation of plywood. Further, the plywood is three-layered, and the preparation process is as follows:

[0019] First step drying: the poplar veneer is dried until the moisture content is less than 10%;

[0020] The second step is gluing: the full biomass adhesive is applied on the poplar veneer by double-sided gluing, and the single-sided gluing amount is 160g / m 2 ;

[0021] The third step is assembly: based on vertical grain method;

[0022] The fourth step is hot pressing: the hot pressing temperature is 180°C, the hot pressing pressure is 1.5MPa, and the hot pressing time is 6min.

[0023] The invention also provides a flame retardant liquid, which is prepared by reacting the branched polyamine and an aminotrimethylenephosphonic acid (ATMP) aqueous solution.

[0024] Preferably, the solid content of the aminotrimethylenephosphonic acid (ATMP) aqueous solution is 50%;

[0025] The mass ratio of the branched polyamine to aminotrimethylene phosphine (ATMP) is 1:5.

[0026] The present invention also provides a three-layer plywood with flame retardant properties, which is prepared using the prepared flame retardant liquid, and the steps include:

[0027] The first step is coating: evenly apply the prepared flame retardant liquid on the surface of the three-layer plywood;

[0028] The second step is vacuum impregnation: put the three-layer plywood coated with flame retardant liquid into a vacuum dryer and store it in a negative pressure environment of 0.05MPa for 24h;

[0029] The third step of drying: take out the plywood from the vacuum dryer and place it in an oven at 60°C to dry for 5 hours.

[0030] The specific preparation method of the branched biomass polyamine and lactose all-biomass adhesive of the present invention comprises the following steps:

[0031] (1) First, 19.6 g of maleic anhydride and an appropriate amount of methanol solution were added to a 200 mL round-bottom flask at room temperature, and ultrasonic stirring was performed to completely dissolve the maleic anhydride therein;

[0032] (2) Subsequently, 7.57 g of tetraethylenepentamine (the molar ratio of tetraethylenepentamine to maleic anhydride is 1:5) is slowly added dropwise to the round-bottom flask while stirring, and then a circulating condenser is connected, and the mixture is reacted in a metal sand bath at 80° C. for 1 hour;

[0033] (3) Finally, the methanol solvent was recovered by a rotary evaporator, and 20.6 g of diethylenetriamine was slowly added dropwise to the above round-bottom flask (the molar ratio of tetraethylenepentamine to diethylenetriamine was 1:5), and the reaction was continued in an open metal sand bath at 110°C for 3 h. After the reaction was completed, maleic branched biomass polyamines were obtained;

[0034] (4) After the reaction is completed, the maleic branched biomass polyamine is cooled to room temperature, and deionized water is added according to its solid content of 50% to completely dissolve it;

[0035] (5) mixing the maleic branched biomass polyamine obtained in step (4) with lactose in a mass ratio of 1:0.5-4, placing the mixture in a reactor at 70° C.-90° C. for reaction for 1 h-6 h to prepare a lactose-based adhesive LMP;

[0036] (6) adding 1% to 8% potassium persulfate to the lactose-based adhesive of step (5), placing the mixture in a reactor at 70° C. to 90° C. for reaction for 1 h to prepare a modified lactose-based adhesive LMP-PP;

[0037] (7) adding 1% to 3% of glycerol glycidyl ether to the lactose-based adhesive of step (5), placing the mixture in a reactor at 70° C. to 90° C. for reaction for 1 h to prepare a modified lactose-based adhesive LMP-G;

[0038] (8) First, 5% potassium persulfate was added to the lactose-based adhesive of step (5), and the mixture was placed in a reactor at 70° C.-90° C. for reaction for 1 h, and then 3% glycerol glycidyl ether was added, and the mixture was placed in a reactor at 70° C.-90° C. for reaction for 1 h to prepare a modified lactose-based adhesive LMP-PP-G;

[0039] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0040] (1) Safe raw material sources: Since biological materials are used, there will be no problem of volatilization of harmful substances. Commercial lactose is mainly extracted from whey protein, a by-product of cheese and casein production, through crystallization. Lactose used in industry mainly comes from cow whey and goat whey. The global annual lactose production reaches 6 million tons. Maleic anhydride (dehydrated malic anhydride) is a fermented product with guaranteed safety, so its demand is growing rapidly worldwide.

[0041] (2) The adhesive prepared by this method has good solubility and does not require the addition of a catalyst. During the hot pressing curing process, no curing agent needs to be added; the plywood has good boiling water resistance and the prepared plywood can not only meet the use requirements of wood panels, but also has a certain flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of the preparation of branched polyamines prepared based on maleic anhydride in the present invention;

[0043] Figure 2 The figure is a schematic diagram of the preparation of the all-biomass adhesive based on branched polyamine and lactose prepared from maleic anhydride according to the present invention;

[0044] Figure 3 This is a mechanism diagram of the flame retardant liquid prepared by the reaction of branched polyamines prepared based on maleic anhydride and aminotrimethylene phosphine (ATMP) according to the present invention.

[0045] Figure 4 Comparison diagram of the combustion process of two groups of samples in Example 26. DETAILED DESCRIPTION

[0046] Hereinafter, the technical solution of the present invention is described in detail through specific examples to facilitate a better understanding of the present invention, but the present invention is not limited thereto.

[0047] The preparation method of the maleic branched polyamine used in the following examples is as follows:

[0048] (1) Add 19.6 g of maleic anhydride and 50 mL of methanol solution into a 200 mL round-bottom flask at room temperature and stir ultrasonically to completely dissolve the maleic anhydride therein;

[0049] (2) while stirring, 7.57 g of tetraethylene pentamine (the molar ratio of tetraethylene pentamine to maleic anhydride is 1:5) is slowly added dropwise to the round-bottom flask, and then a circulating condenser is connected, and the mixture is reacted in a metal sand bath at 80° C. for 1 hour;

[0050] (3) Recover the methanol solvent using a rotary evaporator, then slowly drop 20.6 g of diethylenetriamine into the round-bottom flask (the molar ratio of tetraethylenepentamine to diethylenetriamine is 1:5), and continue to react in a metal sand bath at 110° C. for 3 h. After the reaction is completed, maleic branched biomass polyamines can be obtained;

[0051] (4) After the maleic branched biomass polyamine is cooled to room temperature, deionized water is added according to its solid content of 50% to completely dissolve it, thereby obtaining maleic branched polyamine.

[0052] Example 1

[0053] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0054] At room temperature, 12 g of maleic branched polyamine (50% solid content) and 3 g of lactose were weighed, mixed, 3 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 5 h.

[0055] Example 2

[0056] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0057] At room temperature, 12 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 5 h.

[0058] Example 3

[0059] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0060] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 5 h.

[0061] Example 4

[0062] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0063] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 12 g of lactose were weighed, mixed, and 12 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 5 h.

[0064] Example 5

[0065] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0066] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 1 h.

[0067] Example 6

[0068] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0069] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 2 h.

[0070] Example 7

[0071] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0072] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 3 h.

[0073] Example 8

[0074] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0075] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 4 h.

[0076] Example 9

[0077] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0078] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 6 h.

[0079] Example 10

[0080] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0081] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 70° C. for 5 h.

[0082] Embodiment 11

[0083] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0084] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and the mixture was stirred in a sand bath at 90° C. for 5 h.

[0085] Example 12

[0086] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0087] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 10.5 g of deionized water were added, and the mixture was stirred in a sand bath at 80° C. for 5 h.

[0088] Example 13

[0089] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0090] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, 3 g of deionized water was added, and the mixture was stirred in a sand bath at 80° C. for 5 h.

[0091] Embodiment 14

[0092] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0093] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 1% potassium persulfate (0.18 g) was added and the reaction was continued for 1 h.

[0094] Embodiment 15

[0095] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0096] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 2% potassium persulfate (0.36 g) was added and the reaction was continued for 1 h.

[0097] Example 16

[0098] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0099] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 3% potassium persulfate (0.54 g) was added and the reaction was continued for 1 h.

[0100] Embodiment 17

[0101] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0102] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 4% potassium persulfate (0.72 g) was added and the reaction was continued for 1 h.

[0103] Embodiment 18

[0104] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0105] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 5% potassium persulfate (0.90 g) was added and the reaction was continued for 1 h.

[0106] Embodiment 19

[0107] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0108] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 6% potassium persulfate (1.08 g) was added and the reaction was continued for 1 h.

[0109] Embodiment 20

[0110] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0111] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 7% potassium persulfate (1.26 g) was added and the reaction was continued for 1 h.

[0112] Embodiment 21

[0113] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0114] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 8% potassium persulfate (1.44 g) was added and the reaction was continued for 1 h.

[0115] Embodiment 22

[0116] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0117] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 1% of glycerol glycidyl ether (0.18 g) was added and reacted for 1 h.

[0118] Embodiment 23

[0119] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0120] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80°C for 5 h. After the reaction was completed, the reaction was continued for 1 h. 2% of glycerol glycidyl ether (0.36 g) was added and the reaction was continued for 1 h.

[0121] Embodiment 24

[0122] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0123] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80° C. for 5 h. After the reaction was completed, 3% of glycerol glycidyl ether (0.54 g) was added and reacted for 1 h.

[0124] Embodiment 25

[0125] This embodiment provides a method for preparing a full biomass adhesive based on branched polyamines and lactose prepared from maleic anhydride, which is prepared according to the following method:

[0126] At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added, and stirred in a sand bath pot at 80°C for 5 h. After the reaction was completed, 5% potassium persulfate (0.90 g) was added and the reaction continued for 1 h. 3% of glycerol glycidyl ether (0.54 g) was added and the reaction continued for 1 h.

[0127] Embodiment 26

[0128] This embodiment provides a method for preparing a full biomass adhesive and a flame retardant based on branched polyamines and lactose prepared from maleic anhydride, and a method for coating the flame retardant, which are prepared according to the following method:

[0129] (1) At room temperature, 6 g of maleic branched polyamine (50% solid content) and 6 g of lactose were weighed, mixed, and 6 g of deionized water was added. The mixture was stirred in a sand bath at 80°C for 5 h. After the reaction was completed, 5% potassium persulfate (0.90 g) was added and the reaction was continued for 1 h. 3% of glycerol glycidyl ether (0.54 g) was added and the reaction was continued for 1 h.

[0130] (2) 2.5 g of maleic branched polyamine and 20 g of aminotrimethylenephosphonic acid (50% solid content) were weighed at room temperature, mixed, and then 2.5 g of deionized water was added. The mixture was stirred for 0.5 h at room temperature. After the reaction was completed, 20 mL of deionized water was added to the reaction bottle to adjust the solution to neutrality, and a flame retardant liquid was obtained.

[0131] (3) Use the adhesive prepared in step (1) to press two three-layer plywood boards, and take one of them and evenly apply the flame retardant liquid prepared in step (2) on the surface of the three-layer plywood at room temperature. Then put the three-layer plywood coated with the flame retardant liquid into a vacuum dryer and store it in a negative pressure environment of 0.05 MPa for 24 hours. Finally, take out the plywood from the vacuum dryer and place it in an oven at 60°C to dry for 5 hours.

[0132] In Example 26, the plywood coated with flame retardant liquid was cut into 15 samples of equal length (80mm×10mm), and the plywood not coated with flame retardant liquid was cut into 15 samples of equal length (80mm×10mm) by the same method, and then the limiting oxygen index (LOI) of these two groups of samples was tested respectively. The test results are shown in Table 1 below, and the comparison diagram of the combustion process of the two groups of samples is attached Figure 4 .

[0133] Table 1 Limiting oxygen index (LOI) of two groups of samples

[0134] Plywood samples coated with flame retardant liquid Plywood sample without flame retardant liquid coating LOI(%) 30.5 23.0

[0135] The hot pressing temperature used in Examples 1 to 13 of the preparation of poplar three-layer plywood is 200°C, and the hot pressing temperature used in Examples 14 to 25 is 180°C. Then according to the GB / T17657-2013 standard, the plywood specimens were sawn into equal lengths (100mm×25mm), and a 25mm×25mm glue layer section was cut out on the specimens. Soak in a water bath at 63±3°C and 93±3°C for 3h, then take it out and let it stand at room temperature for 10 minutes, and measure the bonding strength with an electronic universal mechanical testing machine. The test results are shown in Tables 2 and 3 below:

[0136] Table 2 Properties of plywood prepared with different adhesives under hot pressing at 200℃

[0137]

[0138] Table 3 Properties of plywood prepared with different adhesives under hot pressing at 180℃

[0139]

[0140]

[0141] The above examples are preferred embodiments of the present invention, but they are not limited to the above embodiments. Any other replacement, modification, combination, simplification made without departing from the essence and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing a branched polyamine, characterized in that: Here are the steps: (1) mixing maleic anhydride and methanol, and stirring by ultrasonication to completely dissolve the maleic anhydride; (2) while stirring, slowly dropwise adding tetraethylenepentamine to maleic anhydride, and reacting at 70 to 90° C. for 1 to 5 hours; The molar ratio of tetraethylenepentamine to maleic anhydride is 1:4-5; (3) removing excess methanol solvent with a rotary evaporator, and then adding diethylenetriamine dropwise to the reaction mixture, and continuing to react at 100-120° C. for 1-5 hours in an open atmosphere, until the reaction is completed to obtain maleic branched biomass polyamine MP; The molar ratio of tetraethylenepentamine to diethylenetriamine is 1:4-5; (4) After the reaction is completed, the maleic branched biomass polyamine is cooled to room temperature, and deionized water is added according to its solid content of 40-60% to completely dissolve it to obtain the branched polyamine.

2. A full biomass adhesive, characterized in that: The method is obtained by reacting the branched polyamine prepared by the method of claim 1 with lactose, wherein the mass ratio of the branched polyamine to lactose is 1:0.5-4.

3. The all-biomass adhesive according to claim 2, characterized in that: The mass ratio of the branched polyamine to lactose is 1:

2.

4. The all-biomass adhesive according to claim 2, characterized in that: The reaction temperature of the branched polyamine and lactose is 70-90° C., and the reaction time of the branched polyamine and lactose is 1-6 hours.

5. The all-biomass adhesive according to any one of claims 2 to 4, characterized in that: Potassium persulfate and / or glycerol glycidyl ether are also added; The amount of potassium persulfate added is 1%-8% of the mass of the all-biomass adhesive; The added amount of the glycerol glycidyl ether accounts for 1%-3% of the mass of the all-biomass adhesive.

6. Use of the all-biomass adhesive as claimed in any one of claims 2 to 5 in the preparation of plywood.

7. The use of the all-biomass adhesive in the preparation of plywood according to claim 6, characterized in that: The plywood is three-layered and the preparation process is as follows: First step drying: the poplar veneer is dried until the moisture content is less than 10%; The second step is gluing: the full biomass adhesive is applied on the poplar veneer by double-sided gluing, and the single-sided gluing amount is 150-170g / m 2 ; The third step is to assemble the blanks: assemble the blanks based on the vertical texture method; The fourth step is hot pressing: hot pressing is performed at a temperature of 180° C. or 200° C., a pressure of 1.5 to 1.6 MPa, and a time of 6 to 8 minutes to obtain the plywood.

8. A flame retardant liquid, characterized in that: The product is prepared by reacting the branched polyamine prepared by the method according to claim 1 with an aqueous solution of aminotrimethylenephosphonic acid (ATMP).

9. The flame retardant liquid according to claim 8, characterized in that: The solid content of the aminotrimethylenephosphonic acid aqueous solution is 40-60%; The mass ratio of the branched polyamine to aminotrimethylene phosphine is 1:4-6.

10. A three-layer plywood with flame retardant properties, characterized in that: The flame retardant liquid according to claim 9 is used for preparation, and the steps include: The first step of coating: evenly coating the flame retardant liquid on the surface of the three-layer plywood; The three-layer plywood is obtained according to the method of claim 7; The second step is vacuum impregnation: put the three-layer plywood coated with flame retardant liquid into a vacuum dryer and store it in a negative pressure environment of 0.05-0.06MPa for 20-30h; The third step is drying: take out the plywood from the vacuum dryer and place it in an oven at 55-65°C to dry for 4-6 hours.

Citation Information

Patent Citations

  • Biomass formaldehyde-free adhesive as well as preparation method and application method thereof

    CN112322254A

  • Full-biomass adhesive based on maleic anhydride and glycerol as well as preparation method and application of full-biomass adhesive

    CN115895554A

  • Wood adhesive based on biomass hyperbranched polyol-biomass polyacid as well as preparation method and application of wood adhesive

    CN116478649A

  • Preparation and use methods of formaldehyde-free synthetic resin adhesive

    CN117801750A

  • Biomass polyester wood adhesive and preparation method thereof

    CN117801751A