A highly flame-retardant and heat-stable modified polyvinyl chloride material and a preparation method thereof

By introducing bio-based resin and a unique curing method into PVC materials, the problem of reduced flame retardancy and thermal stability of PVC cable materials is solved, achieving high flame retardancy and thermal stability while maintaining flexibility. , suitable for safety applications of wires and cables.

CN118388902BActive Publication Date: 2024-10-01ZHEJIANG CHINT BUILDING ELECTRICS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410835314.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-01
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

The flame retardant performance and thermal stability of PVC cable materials are easy to decrease during the traditional modification process, making it more flammable and reducing the oxygen index, making it unable to meet the safety requirements of wires and cables.

Method used

Through physical doping and chemical modification, bio-based resin is mixed with polyvinyl chloride, and bio-based resin is prepared using raw materials such as hydrogenated rosin alcohol, furandicarboxyl chloride, epichlorohydrin and tetrabutylammonium bromide, and It is melt-blended with polychloride-based polymers and combined with a unique curing method to form a high molecular weight bio-based resin containing furan rings, which enhances the flame retardant performance and thermal stability of the material.

Benefits of technology

It achieves high flame retardancy and thermal stability of polyvinyl chloride materials while maintaining good flexibility, improving the material's fracture toughness and strength, delaying the plasticization process, and enhancing its ability to withstand high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_11
    Figure SMS_11
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyvinyl chloride cable materials, and in particular, relates to a highly flame-retardant and heat-stable modified polyvinyl chloride material and a preparation method thereof. The method comprises: (1) uniformly mixing rosin derivatives, polymerized monomers, cyclic hydrocarbons and organic ammonium salts in proportion to prepare a bio-based resin liquid; (2) uniformly mixing polyvinyl chloride-based polymers, bio-based resin liquid and curing agents in proportion to prepare a modified resin; (3) adding the modified resin to a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material. The present invention constructs a special lattice structure inside the polyvinyl chloride material through bio-based resins and a unique curing method, optimizes the polyvinyl chloride material, and makes it have high flame retardancy and thermal stability while maintaining good flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyvinyl chloride cable materials, and in particular relates to a highly flame-retardant and heat-stable modified polyvinyl chloride material and a preparation method thereof. Background Art

[0002] Polyvinyl chloride, as a polar non-crystalline polymer, has significant advantages in many fields due to its high strength, high modulus and low shrinkage. In the wire and cable industry, the application of soft modified polyvinyl chloride is particularly critical, mainly assuming the functions of insulation layer and protective layer of wires and cables. Among the current technical means, plasticizers are widely used for modification in order to increase its flexibility. However, this addition method will cause changes in the interaction between polyvinyl chloride molecules, making it more flammable, reducing the oxygen index and reducing the flame retardant properties. For the wire and cable industry, improving the flame retardant properties of polyvinyl chloride has become an urgent need. By developing new flame retardants, optimizing modification processes and exploring alternative materials, it is expected to improve the flame retardant properties of polyvinyl chloride to meet the requirements for safe use of wires and cables. Summary of the invention

[0003] The technical solution of the present invention aims at the problem that the flame retardancy and thermal stability of polyvinyl chloride of wires and cables in the traditional technical solution decrease, and provides a highly flame retardant and thermally stable modified polyvinyl chloride material and a preparation method thereof.

[0004] The main purpose of the present invention is to optimize the polyvinyl chloride material by physical doping and chemical modification so that it has high flame retardancy and thermal stability as well as good flexibility.

[0005] To achieve the above objectives, the present invention adopts the following technical solutions.

[0006] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material.

[0007] The method comprises:

[0008] (1) Mixing rosin derivatives, polymer monomers, cyclic hydrocarbons and organic ammonium salts in proportion to prepare a bio-based resin solution;

[0009] (2) uniformly mixing a polyvinyl chloride based polymer, a bio-based resin liquid and a curing agent in proportion to prepare a modified resin;

[0010] (3) Adding the modified resin into a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material.

[0011] As a preference,

[0012] The rosin derivative in step (1) is hydrogenated abietic alcohol;

[0013] The polymerization monomer in step (1) is furan dicarbonyl chloride;

[0014] The cyclic hydrocarbon in step (1) is epichlorohydrin;

[0015] The organic ammonium salt in step (1) is tetrabutylammonium bromide.

[0016] As a preference,

[0017] In step (1), the rosin derivative, polymerization monomer, cyclic hydrocarbon and organic ammonium salt are uniformly mixed in a mass ratio of (3-7):15:(3-5):1.

[0018] As a preference,

[0019] The prepared bio-based resin liquid in step (1) is stirred for 8 to 12 hours under a nitrogen atmosphere at a temperature of -5 to 10°C and a rotation speed of 1000 to 1500 r / min.

[0020] As a preference,

[0021] The polyvinyl chloride-based polymer in step (2) is SG-5 type polyvinyl chloride resin;

[0022] The curing agent in step (2) is bisphenol A containing a β-amino alcohol structure.

[0023] As a preference,

[0024] In step (2), the polyvinyl chloride based polymer, bio-based resin liquid and curing agent are uniformly mixed in a mass ratio of (3-4): (1.8-2.2): 1.

[0025] As a preference,

[0026] The specific operation of preparing the modified resin in step (2) is: first, drying in a vacuum environment at a temperature of 30 to 40 °C for 4 to 6 h, then pre-curing in an environment at a temperature of 60 to 70 °C for 2 to 3 h, and then heating and curing at a heating rate of 10 °C / h for 8 to 12 h.

[0027] As a preference,

[0028] The operating parameters of the twin-screw extruder in step (3) are as follows: the screw zone temperatures are: zone 1 temperature is 140-160°C, zone 2 temperature is 140-160°C, zone 3 temperature is 135-155°C, zone 4 temperature is 130-150°C and zone 5 temperature is 130-150°C.

[0029] A highly flame retardant and heat stable modified polyvinyl chloride material.

[0030] In the technical solution of the present invention, the core lies in optimizing the polyvinyl chloride material by physical doping and chemical modification, so that it has flexibility, high flame retardancy and thermal stability. Polyvinyl chloride, due to its homopolymer structure, shows lower thermal stability, impact strength and heat deformation temperature compared with cross-linked rubber. In addition, the plasticized resilience of polyvinyl chloride products is also insufficient, which limits its application range. In order to improve these properties, the present invention proposes a technical solution: bio-based resin and polyvinyl chloride are mixed evenly to prepare modified polyvinyl chloride materials, wherein the bio-based resin is prepared from hydrogenated rosin alcohol, furan dicarboxylic chloride and epichlorohydrin as raw materials and tetrabutylammonium bromide as a catalyst. Rosin, as a key biomass resource, has been widely used in the modification of coating materials such as coatings and inks. The large volume rigid ternary phenanthrene ring and polar carboxyl group contained in its molecular structure play a key role in improving the strength and adhesion of the modified system. The reactivity of the carboxyl group makes it possible to introduce polymerizable groups on the basis of the rosin structure, and then to achieve material modification by incorporating these groups into the side chains of macromolecules. However, although the introduction of rosin improves the hardness of the polyvinyl chloride material system, it leads to a decrease in the toughness of the polyvinyl chloride material system and produces brittleness. In addition, the unsaturated double bonds in the molecular structure of rosin will produce activating groups with other components and have an adverse effect. The present invention uses hydrogenated rosin that has been hydrogenated to reduce 1 to 2 double bonds while retaining the reactive carboxyl groups, thereby achieving a balance between rigidity and flexibility. Due to the particularity of the chemical structure, the biomass resin prepared by the present invention has high mechanical strength and excellent high temperature resistance. Through low-temperature solution polycondensation, an aromatic heterocyclic structure is introduced into the main chain of the molecule to generate a high molecular weight furan ring-containing bio-based resin, thereby obtaining a high-performance biomass resin with excellent heat resistance and flame retardant properties. In the technical solution of the present invention, the bio-based resin and polyvinyl chloride form a liquid film that can wrap around the resin surface, reduce the friction between the polyvinyl chloride resin particles and between the polyvinyl chloride resin particles and the curing agent, thereby reducing the generation of shear heat of polyvinyl chloride and delaying plasticization. In addition, under the catalytic action of tetrabutylammonium bromide, the bio-based resin liquid can penetrate between the polyvinyl chloride molecular chains, play the role of an internal lubricant, enhance the stress propagation ability between the molecular chains under the influence of external forces, reduce the internal structure damage caused by the friction between the molecular chains inside the resin, and enhance the flexibility of the modified polyvinyl chloride material. At the same time, the polyvinyl chloride molecular chains are modified through coordination grafting, so that some groups show better affinity, enhance the interaction between the molecular chains, and promote the plasticization process of the modified polyvinyl chloride.

[0031] In the technical solution of the present invention, another core point is that the present invention uses a staged curing method to treat modified polyvinyl chloride. In the technical solution of the present invention, through the interaction between the bio-based resin and polyvinyl chloride, the compatibility between the two phases is enhanced. With the further implementation of the pre-curing operation, an obvious interface layer appears between the two phases. At the same time, in the molecular structure of vinyl chloride, the mutual repulsion between chlorine atoms leads to a configuration similar to syndiotactic structure, so that polyvinyl chloride has a certain degree of crystallinity and mainly contains an amorphous phase. In this process, the molecular chains of polyvinyl chloride are repeatedly folded and orderly arranged to form folded chain crystals and micelle crystals formed by parallel arrangement of molecular chains, and a complex morphology of continuous "sea-island" structure coexisting with the bio-based resin appears. At this time, further curing is carried out, and the change of crystal shape in the material system leads to stress relaxation at the crack tip, thereby inducing a stress phase transition of the material. During the phase transition, the volume expansion causes the surrounding matrix to be compressed, thereby promoting the closure of the crack, which helps to improve the fracture toughness and strength of the material. Through lattice expansion and shearing, a shield is formed at the crack tip, which can release the expansion driving force of the crack tip, thereby further improving the fracture toughness of the material. In addition, after the staged curing, the modified polyvinyl chloride material is affected by the external high temperature environment, and the molecular chain of polyvinyl chloride partially unfolds inside the material to form a honeycomb structure, which can increase the path of heat transfer to the external environment and improve the thermal stability of the material. As the temperature of the system continues to rise, the modified polyvinyl chloride material undergoes pyrolysis, resulting in a large number of polyvinyl chloride main chain breaks. In this case, the aromatic structure in the bio-based resin escapes from the system and reacts with the curing agent bisphenol A containing a β-amino alcohol structure. The curing agent bisphenol A containing a β-amino alcohol structure comes from the scientific research cooperation unit Ningbo Institute of Materials Technology and Engineering (NIMTE). This process increases the cross-linking density of the system, thereby enhancing the connection between the carbonaceous layers, improving the carbonization ability, and improving the flame retardant properties of the system.

[0032] The advantages of the present invention are as follows: the present invention constructs a special lattice structure inside the polyvinyl chloride material through bio-based resin and a unique curing method, optimizes the polyvinyl chloride material, makes it have high flame retardancy and thermal stability, and keeps good flexibility. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0034] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0035] Example 1

[0036] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material.

[0037] The method comprises:

[0038] (1) Hydroabietyl alcohol, furandicarboxylic acid chloride, epichlorohydrin and tetrabutylammonium bromide were uniformly mixed in a mass ratio of 3:15:3:1, and stirred for 12 h under a nitrogen atmosphere at a temperature of -5 °C and a rotation speed of 1000 r / min to prepare a bio-based resin liquid;

[0039] (2) SG-5 polyvinyl chloride resin, bio-based resin liquid and curing agent bisphenol A containing a β-amino alcohol structure were uniformly mixed in a mass ratio of 3:1.8:1, first dried in a vacuum environment at a temperature of 30 °C for 6 h, then pre-cured in an environment at a temperature of 60 °C for 3 h, and then heated and cured at a heating rate of 10 °C / h for 12 h to prepare a modified resin;

[0040] (3) The modified resin is added into a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material, wherein the screw zone temperatures are as follows: zone 1 temperature is 140°C, zone 2 temperature is 140°C, zone 3 temperature is 135°C, zone 4 temperature is 130°C and zone 5 temperature is 130°C.

[0041] The modified polyvinyl chloride material prepared in the example was subjected to performance testing, and the specific characterization results are as follows.

[0042] Vertical combustion test: Referring to the detection method of vertical combustion test in ASTM D3801, the modified polyvinyl chloride material prepared in the embodiment was made into a test sample with a size of 120×20×3 mm, and two ignition tests were carried out. Each time the ignition contact flame was maintained for 10 s, the flame was removed, and the time when the sample was extinguished each time was recorded as the initial ignition combustion time and the re-ignition combustion time.

[0043] Limiting oxygen index test: Referring to the limiting oxygen index standard test in ASTM D2863-97, the modified polyvinyl chloride material prepared in the embodiment was made into a test sample with a size of 100×10×5 mm, and the test sample was placed in a glass chimney. A mixed environment of nitrogen and oxygen was established through the airflow at the bottom of the chimney. The upper part of the test sample was ignited, and the oxygen concentration in the flow decreased until the flame no longer burned. The limiting oxygen index was recorded using a 5801 digital oxygen index analyzer.

[0044]

[0045] Mechanical testing: With reference to the mechanical strength test in GB 13022-91, the modified vinyl chloride material prepared in the embodiment was made into a type I dumbbell test sample, the width and thickness of the test sample were measured using a vernier caliper, and the test sample was subjected to mechanical testing using a tensile testing machine, an impact testing machine and a hardness tester.

[0046]

[0047] In addition, the modified polyvinyl chloride material prepared in the embodiment was made into a test sample with a size of 120×50×5 mm, and thermal gravimetric tests were carried out in air and nitrogen atmospheres, respectively. When the temperature was gradually increased from 25°C to 800°C and the heating rate was 10°C / min, the 5% thermal weight loss, the first-stage weight loss temperature range and the first-stage total weight loss rate of the modified polyvinyl chloride material were recorded.

[0048]

[0049] By analyzing the above characterization results, it can be observed that under the modified conditions of the technical solution of the present invention, the polyvinyl chloride material prepared by the embodiment has excellent flame retardancy and self-extinguishing ability, no molten droplets will appear during the combustion process, and also has good mechanical and mechanical properties. The burning speed of the polyvinyl chloride material during the combustion process is related to the degree of dehydrogenation in the polyvinyl chloride material. In the scheme of the present invention, the main chain structure of the bio-based resin molecule contains a high proportion of benzene rings, which is prone to surface carbonization. The surface carbonization can effectively isolate oxygen, thereby preventing the diffusion of combustible gases and producing a flame retardant effect. At the same time, after the staged curing operation, a morphology with a honeycomb structure is formed inside the polyvinyl chloride material, which can increase the path for heat transfer to the external environment and improve the thermal stability of the material. It can also be seen from the fact that the upper limit of the first weight loss temperature interval under the above air atmosphere conditions is close to the nitrogen atmosphere that for the present invention, compared with conventional PVC, it can more effectively inhibit the thermal decomposition weight loss process in the air atmosphere. In addition, the addition of bio-based resin increases the cross-linking density of the molecular chain in the system, further strengthens the interaction between the carbonaceous layers, improves the carbonization efficiency, and enhances the overall flame retardant properties. In the scheme of the present invention, the bio-based resin interacts with polyvinyl chloride to enhance the compatibility of the two phases, thereby forming a distinct interface layer. In this process, the polyvinyl chloride molecular chain is folded and arranged in order to generate folded chains and micellar crystals, which together with the bio-based resin build a "sea-island" structure. As the curing process progresses, the change in crystal morphology leads to stress relaxation and phase change, and the volume expansion promotes crack closure, thereby improving the fracture toughness and strength of the material, while maintaining the flexibility of the cable. In addition, the lattice expansion and shearing action produce a shielding effect at the crack tip, releasing the expansion driving force, which can further enhance the fracture toughness of the material.

[0050] Example 2

[0051] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material.

[0052] The method comprises:

[0053] (1) Hydrogenated rosin alcohol, furan dicarboxylic acid chloride, epichlorohydrin and tetrabutylammonium bromide were uniformly mixed in a mass ratio of 5:15:4:1, and stirred for 10 h under a nitrogen atmosphere at a temperature of 0 °C and a rotation speed of 1250 r / min to prepare a bio-based resin liquid;

[0054] (2) SG-5 polyvinyl chloride resin, bio-based resin liquid and curing agent bisphenol A containing a β-amino alcohol structure were uniformly mixed in a mass ratio of 3.5:2:1, first dried in a vacuum environment at a temperature of 35 °C for 5 h, then pre-cured in an environment at a temperature of 65 °C for 2.5 h, and then heated and cured at a heating rate of 10 °C / h for 10 h to prepare a modified resin;

[0055] (3) Adding the modified resin into a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material, wherein the screw zone temperatures are as follows: zone 1 temperature is 150°C, zone 2 temperature is 150°C, zone 3 temperature is 145°C, zone 4 temperature is 140°C and zone 5 temperature is 140°C.

[0056] The characterization test was performed in this example using the same characterization method as in Example 1, and the results are as follows.

[0057]

[0058] By analyzing the above characterization results, it can be observed that under the modified conditions of the technical solution of the present invention, the polyvinyl chloride material prepared in the embodiment has excellent flame retardancy, no droplets will appear during the combustion process, and also has good mechanical and mechanical properties. It has a hardness close to that of conventional PVC cable materials or even slightly lower than the Shore hardness of conventional PVC cable materials, maintains good flexibility, and is easy to maintain the bendability of the cable when used as a cable material, but has higher tensile strength and elongation at break close to that of conventional PVC cable materials.

[0059] Example 3

[0060] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material.

[0061] The method comprises:

[0062] (1) Hydroabietyl alcohol, furan dicarboxylic acid chloride, epichlorohydrin and tetrabutylammonium bromide were uniformly mixed in a mass ratio of 7:15:5:1, and stirred for 9 h under a nitrogen atmosphere at a temperature of 5 °C and a rotation speed of 1400 r / min to prepare a bio-based resin liquid;

[0063] (2) SG-5 polyvinyl chloride resin, bio-based resin liquid and curing agent bisphenol A containing a β-amino alcohol structure were uniformly mixed in a mass ratio of 4:2.2:1, first dried in a vacuum environment at a temperature of 40 °C for 4 h, then pre-cured in an environment at a temperature of 70 °C for 2 h, and then heated and cured at a heating rate of 10 °C / h for 8 h to prepare a modified resin;

[0064] (3) The modified resin is added into a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material, wherein the screw zone temperatures are as follows: zone 1 temperature is 160°C, zone 2 temperature is 160°C, zone 3 temperature is 155°C, zone 4 temperature is 150°C and zone 5 temperature is 150°C.

[0065] The characterization test was performed in this example using the same characterization method as in Example 1, and the results are as follows.

[0066]

[0067] By analyzing the above characterization results, it can be observed that under the modification conditions of the technical solution of the present invention, the polyvinyl chloride material prepared in the embodiment has excellent flame retardancy, no droplets will appear during the combustion process, and also has good mechanical and mechanical properties.

[0068] Example 4

[0069] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material.

[0070] The method comprises:

[0071] (1) Hydroabietyl alcohol, furandicarboxylic acid chloride, epichlorohydrin and tetrabutylammonium bromide were uniformly mixed in a mass ratio of 7:15:5:1, and stirred for 8 h under a nitrogen atmosphere at a temperature of 10 °C and a rotation speed of 1500 r / min to prepare a bio-based resin liquid;

[0072] (2) SG-5 polyvinyl chloride resin, bio-based resin liquid and curing agent bisphenol A containing a β-amino alcohol structure were uniformly mixed in a mass ratio of 4:2.2:1, first dried in a vacuum environment at a temperature of 40 °C for 4 h, then pre-cured in an environment at a temperature of 70 °C for 2 h, and then heated and cured at a heating rate of 10 °C / h for 8 h to prepare a modified resin;

[0073] (3) The modified resin is added into a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material, wherein the screw zone temperatures are as follows: zone 1 temperature is 160°C, zone 2 temperature is 160°C, zone 3 temperature is 155°C, zone 4 temperature is 150°C and zone 5 temperature is 150°C.

[0074] The characterization test was performed in this example using the same characterization method as in Example 1, and the results are as follows.

[0075]

[0076] By analyzing the above characterization results, it can be observed that under the modification conditions of the technical solution of the present invention, the polyvinyl chloride material prepared in the embodiment has excellent flame retardancy, no droplets will appear during the combustion process, and also has good mechanical and mechanical properties.

[0077] Comparative Example 1

[0078] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material, wherein the specific preparation method is the same as that in Example 1, and the comparative example only prepares and uses the bio-based resin material component unique to the present invention to prepare the modified polyvinyl chloride material, which are respectively marked as Comparative Example 1-a, Comparative Example 1-b and Comparative Example 1-c. The modified polyvinyl chloride materials prepared by Comparative Example 1-a, Comparative Example 1-b and Comparative Example 1-c are subjected to performance testing in the same manner as in Example 1.

[0079] In the comparative example 1-a, only the hydrogenated rosin alcohol component in the bio-based resin material component unique to the present invention is changed, and an equal amount of rosin alcohol is used to replace hydrogenated rosin alcohol to prepare the modified polyvinyl chloride material;

[0080] In the comparative example 1-b, only the furan dicarboxylic acid chloride component in the bio-based resin material component unique to the present invention is changed, and an equal amount of terephthalic acid is used to replace furan dicarboxylic acid chloride to prepare the modified polyvinyl chloride material;

[0081] In the comparative example 1-c, only the tetrabutylammonium bromide component in the bio-based resin material component unique to the present invention is changed, and tetrabutylammonium bromide is not used to prepare the modified polyvinyl chloride material.

[0082] The characterization results are shown in Tables D1-1, D1-2 and D1-3 below. The final value of weight loss temperature in Table D1-3 only represents the maximum value of the weight loss temperature range in the first stage.

[0083] Table D1-1.

[0084]

[0085] Table D1-2.

[0086]

[0087] Table D1-3.

[0088]

[0089] Analysis of the above characterization results shows that the polyvinyl chloride materials prepared by the three groups of comparative examples are compared with those in Example 1. Each group has a molten droplet phenomenon during the combustion process, and the flame retardancy, mechanical properties, mechanical properties and thermal stability of each item of the comparative example are reduced, but the degree of reduction is different. Further research and analysis, combined with the characterization data of each table, comparative example 1-a uses an equal amount of rosin alcohol instead of hydrogenated rosin alcohol. Due to the introduction of too many unsaturated double bonds in the prepared material, side reactions with unsaturated rings affect the final material properties. Some double bonds are coordinated and grafted on the polyvinyl chloride molecular chain to enhance the bonding degree between the molecular chains, so that the modified polyvinyl chloride is over-plasticized and brittle, resulting in a decrease in the flexibility of the material prepared in the comparative example. In addition, excessive unsaturated bonds will also lead to the production of dehydrogenation oxidation, thereby reducing the flame retardant properties of the material.

[0090] In comparative example 1-b, an equal amount of terephthalic acid is used instead of furan dicarboxylic acid chloride. Melt droplets still appear during the combustion process. Further observation of the dripping melt droplets during the combustion process shows that the melt droplets are not completely burned. The reason for the generation of melt droplets is that the carbon layer structure inside the material is unevenly distributed, resulting in the ineffective transfer of heat. The heat accumulates at the end of the transfer, causing the polyvinyl chloride material to be ignited. This shows that terephthalic acid cannot meet the flame retardant performance requirements of the present invention.

[0091] Comparative Example 1-c does not use tetrabutylammonium bromide as a catalyst. The material prepared in Comparative Example 1-c is observed in more detail. Specifically, the state of the material when the modified polyvinyl chloride material prepared in Comparative Example 1-c is tested for performance is observed. Black smoke appears during the second ignition process during the combustion process, and the burning time is significantly prolonged. The reason for this phenomenon is that after the first combustion occurs, the internal structure of the material is disordered, resulting in serious carbon loss during the second ignition process. After analysis, it should be due to the lack of the addition of a suitable catalyst, which makes it impossible to form a large-area effective flame-retardant carbon layer inside the polyvinyl chloride under high temperature conditions. , which makes it difficult to extinguish the flame and causes the loss of carbon in the material; when conducting mechanical tests such as tensile strength and yield strength, the material shows obvious stress whitening. At this time, the test is suspended and a detailed observation of the material reveals that a large number of microcracks have formed in the material. After analysis, it is found that this is due to the low compatibility between the components within the material, which results in the inability of the polyvinyl chloride molecular chains to be arranged regularly, resulting in structural voids in the material under the action of external forces, and then defect sites appear. The external force cannot be transmitted, resulting in damage at the defect sites, which is manifested macroscopically as the generation of microcracks, affecting the fracture toughness and strength of the material.

[0092] Comparative Example 2

[0093] A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material, wherein the specific preparation method is the same as that of Example 2, except that the modified polyvinyl chloride is not treated by the staged curing method unique to the present invention, and the modified polyvinyl chloride material is prepared by a conventional one-step curing method. The modified polyvinyl chloride material prepared by the comparative example is tested for performance in the same manner as that of Example 1, and the characterization results are as follows.

[0094]

[0095] Analyzing the above-mentioned table results, the polyvinyl chloride material prepared in comparative example 2 is compared with example 2. The material prepared in comparative example shows a molten droplet phenomenon during the combustion process. At the same time, the flame retardancy, mechanical properties, mechanical properties and thermal stability are all reduced compared with example 1. The state of the modified polyvinyl chloride material prepared in comparative example 1-c during performance testing is further observed. After the flame retardancy test, the dripping molten droplets are observed, and the whole appears as a charred smooth solid, without a honeycomb flame-retardant carbon layer, resulting in poor flame retardancy of the modified polyvinyl chloride material prepared in comparative example; when performing mechanical tests such as tensile strength and yield strength, some obvious phase interfaces can be observed at the fracture, the bonding strength between the components inside the material is not high, and a complete lattice barrier is not constructed. At this time, the crystal formation changes in irregular shape, resulting in the inability to effectively transmit the lattice changes caused by external force changes, further affecting the fracture toughness and strength of the modified polyvinyl chloride material.

[0096] Comparative Example 3

[0097] A commercially available polyvinyl chloride cable material was subjected to performance testing in the same manner as in Example 1, and the characterization results are as follows.

[0098]

[0099] By analyzing the above characterization results, it can be observed that the flame retardancy and mechanical strength of the present invention are significantly stronger than those of commercially available polyvinyl chloride cable materials. After further research, it was found that the thermal degradation of commercially available polyvinyl chloride materials is divided into two steps: the first step is the first stage of thermal weight loss between about 180 and 780 ° C (as described in the above test) and the second stage of thermal weight loss, the dechlorination and dehydrogenation of polyvinyl chloride. According to the detection data, at this time, the hydrogen chloride in the polyvinyl chloride is volatilized, and the weight loss rate of the two-stage thermal weight loss can reach about 60%, and the total weight loss rate of the first stage alone reaches about 36.7%. The remaining polymer undergoes the second step of deoxygenation decomposition. Under higher temperature conditions, when the oxygen content is sufficient, polyvinyl chloride may even produce oxidative combustion that cannot be self-extinguished. At this time, the total weight loss rate is greater than 85 %, the vinyl chloride material prepared by the present invention forms a unique folded chain and micellar crystal structure through the modification operation of bio-based resin and staged curing, which significantly improves the fracture toughness and strength of the material. At the same time, during the combustion process, the components inside the material form a honeycomb structure at high temperature, which improves thermal stability, crosslinking density and carbonization ability, and enhances flame retardant properties. The macroscopic manifestation is that the temperature at which deoxidation begins is increased, which can reflect that the thermal stability of the material is stronger.

Claims

1. A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material, It is characterized in that The method comprises: (1) Mixing rosin derivatives, polymer monomers, cyclic hydrocarbons and organic ammonium salts in proportion to prepare a bio-based resin solution; (2) uniformly mixing a polyvinyl chloride based polymer, a bio-based resin liquid and a curing agent in proportion to prepare a modified resin; (3) adding the modified resin into a twin-screw extruder for melt blending and granulation to obtain a modified polyvinyl chloride material; The rosin derivative in step (1) is hydrogenated abietic alcohol; The polymerization monomer in step (1) is furan dicarboxylic acid chloride; The cyclic hydrocarbon in step (1) is epichlorohydrin; The organic ammonium salt in step (1) is tetrabutylammonium bromide; The curing agent in step (2) is bisphenol A containing a β-amino alcohol structure.

2. A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material according to claim 1, It is characterized in that In step (1), the rosin derivative, polymerization monomer, cyclic hydrocarbon and organic ammonium salt are uniformly mixed in a mass ratio of (3-7):15:(3-5):

1.

3. A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material according to claim 1 or 2, It is characterized in that The prepared bio-based resin liquid in step (1) is stirred for 8 to 12 hours under a nitrogen atmosphere at a temperature of -5 to 10°C and a rotation speed of 1000 to 1500 r / min.

4. The method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material according to claim 1, It is characterized in that The polyvinyl chloride-based polymer in step (2) is SG-5 type polyvinyl chloride resin.

5. The method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material according to claim 4, It is characterized in that In step (2), the polyvinyl chloride based polymer, bio-based resin liquid and curing agent are uniformly mixed in a mass ratio of (3-4): (1.8-2.2):

1.

6. A method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material according to claim 1 or 5, It is characterized in that The specific operation of preparing the modified resin in step (2) is: first, drying in a vacuum environment at a temperature of 30 to 40 °C for 4 to 6 hours, then pre-curing in an environment at a temperature of 60 to 70 °C for 2 to 3 hours, and then heating and curing at a heating rate of 10 °C / h for 8 to 12 hours.

7. The method for preparing a highly flame-retardant and heat-stable modified polyvinyl chloride material according to claim 1, It is characterized in that The operating parameters of the twin-screw extruder in step (3) are as follows: the screw zone temperatures are 140-160°C in zone 1, 140-160°C in zone 2, 135-155°C in zone 3, 130-150°C in zone 4, and 130-150°C in zone 5.

8. A highly flame-retardant and heat-stable modified polyvinyl chloride material prepared by the method of any one of claims 1 to 7.

Citation Information

Cited By

  • Flame-retardant modified PVC (polyvinyl chloride) composite material based on graphene-coated hydroxyl magnesium-aluminum hydrotalcite LDHs (layered double hydroxides) and preparation method of flame-retardant modified PVC composite material

    CN119286165A

  • A flame retardant modified PVC composite material based on graphene-coated hydroxy magnesium aluminum hydrotalcite LDHs and preparation method thereof

    CN119286165B