Acrylic plate surface coating material and surface treatment process

By coating an acrylic plate with a coating containing synergistically modified SiO2 nanoparticles and antioxidant synergists, the problem of insufficient anti-ultraviolet and anti-oxidation properties in the existing technology is solved, achieving longer-lasting protection and wear resistance. Scratch resistance, while avoiding the risk of strong oxidizing free radicals, extending the service life of the acrylic plate.

CN118389034BActive Publication Date: 2024-10-15FENIMEIJIA (JIANGSU) NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410407359.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-15
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

Existing acrylic plate surface treatment technology cannot effectively improve its anti-ultraviolet and anti-oxidation properties, resulting in shortened service life.

Method used

A coating material including a host resin, an active monomer, a photoinitiator and an anti-UV antioxidant synergist is used to prepare synergistically modified SiO2 nanoparticles and graft polymers on them to form a coating with anti-UV and anti-UV properties. The coating has anti-oxidation properties and is cured by an excimer lamp to form a coating with a thickness of 12-40μm.

Benefits of technology

Significantly improves the wear resistance, UV resistance and oxidation resistance of the coating, prolongs the service life of the acrylic plate, and produces a matte effect through the diffuse reflection of nanoparticles, avoiding the use of traditional nano-ZnO particles in the coating system. Strong risk of oxidative free radicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389034B_ABST
    Figure CN118389034B_ABST
Patent Text Reader

Abstract

The present invention discloses an acrylic plate surface coating material and a surface treatment process, wherein the coating material comprises the following components by weight: 23-75 parts of a main resin; 6-24 parts of an active monomer; 0.5-3.8 parts of a photoinitiator; 1.2-6 parts of an auxiliary agent; and 1.8-8.5 parts of an anti-ultraviolet antioxidant synergist. In the coating material of the present invention, by adding an anti-ultraviolet antioxidant synergist, the wear resistance, anti-ultraviolet performance and antioxidant performance of the formed coating can be improved at the same time, so that the coating can provide a longer-lasting protection for the acrylic plate, making it have better wear resistance and scratch resistance and surface resistance than traditional acrylic plates; and the effect of nanoparticles in the anti-ultraviolet antioxidant synergist can form a surface with concave-convex particles, and through the diffuse reflection effect of the concave-convex particles, the coating surface can produce a matte effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of acrylic plate materials, and in particular to an acrylic plate surface coating material and a surface treatment process. Background Art

[0002] Acrylic, also known as PMMA or organic glass, is mainly made of polymethyl methacrylate, which is polymerized from methyl methacrylate monomers. Acrylic sheets have the advantages of light weight, low price, good light transmittance, easy molding, high recyclability, etc., and are widely used.

[0003] As acrylic sheets are used in various industries, the requirements for their performance are getting higher and higher, such as friction resistance, UV resistance, oxidation resistance, etc. Ultraviolet light irradiation or oxidizing substance attack can easily accelerate the degradation of organic matter in the sheet, resulting in a shortened service life.

[0004] By performing surface treatment on acrylic sheets, such as surface coating treatment, its performance can be improved, which is conducive to extending its service life and improving its use effect. For example, patent CN107216744A discloses a new type of UV nano-coated acrylic sheet technology, which can extend its indoor and outdoor service life by spraying UV nano-coating. However, the coating in this patent does not have good anti-ultraviolet or anti-oxidation properties, and the improvement effect on acrylic sheets is limited.

[0005] In view of this, it is now necessary to improve the existing technology to provide a more reliable solution. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide an acrylic plate surface coating material and a surface treatment process in view of the deficiencies in the above-mentioned prior art.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: an acrylic plate surface coating material, comprising the following components in parts by weight:

[0008] Main resin 23-75 parts;

[0009] 6-24 parts of active monomer;

[0010] Photoinitiator 0.5-3.8 parts;

[0011] 1.2-6 parts of additives;

[0012] 1.8-8.5 parts of anti-ultraviolet antioxidant synergist.

[0013] Preferably, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0014] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0015] S1-1, adding nano-SiO2 to deionized water, ultrasonically dispersing, then adding zinc chloride solution, and then adding hydrochloric acid, ultrasonically dispersing to obtain precursor solution 1;

[0016] S1-2, adding glucose, thioacetamide and L-proline to an ethanol aqueous solution, stirring, adding the obtained mixture to the precursor solution 1, and ultrasonically dispersing to obtain a precursor solution 2;

[0017] S1-3, transferring the precursor solution 2 to a polytetrafluoroethylene-lined reactor, reacting under heating, cooling to room temperature after the reaction, filtering, and vacuum drying the obtained solid to obtain synergistically modified SiO2 nanoparticles;

[0018] S2, grafting a polymer onto the synergistically modified SiO2 nanoparticles to obtain the anti-ultraviolet antioxidant synergist:

[0019] S2-1, adding vinyl triethoxysilane and methyl methacrylate to ethanol, stirring to obtain a mixture 1;

[0020] S2-2. Add the initiator and the synergistically modified SiO2 nanoparticles prepared in step S1 into ethanol, disperse them ultrasonically, add the obtained dispersion into mixture 1 under stirring, heat to reflux, filter after the reaction is completed, and wash the solid product with deionized water and ethanol in sequence to obtain the anti-UV antioxidant synergistic additive.

[0021] Preferably, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0022] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0023] S1-1, add 50-200 mg of nano-SiO2 into 50-200 mL of deionized water, ultrasonically disperse for 5-15 min, then add 5-20 mL of 2 mg / mL zinc chloride solution, then add 2-10 mL of 5% hydrochloric acid, ultrasonically disperse for 10-30 min, to obtain precursor solution 1;

[0024] S1-2, adding 18-72 mg of glucose, 5.6-22.4 mg of thioacetamide, and 11.5-46 mg of L-proline to 50-200 mL of ethanol aqueous solution, stirring for 2-15 min, adding the obtained mixture to the precursor solution 1, and ultrasonically dispersing for 15-60 min to obtain precursor solution 2;

[0025] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 175-195°C for 6-24h, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 50-70°C for 4-12h to obtain synergistically modified SiO2 nanoparticles;

[0026] S2, grafting a polymer onto the synergistically modified SiO2 nanoparticles to obtain the anti-ultraviolet antioxidant synergist:

[0027] S2-1, adding 1.25-5 mg of vinyl triethoxysilane and 8-32 mg of methyl methacrylate to 25-100 mL of ethanol, stirring for 5-30 min, to obtain a mixture 1;

[0028] S2-2. Add 0.015-0.06 mg of benzoyl peroxide and 2.5-10 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 10-40 mL of ethanol, and disperse them ultrasonically for 5-30 min. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 65-78°C for 3-12 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain the anti-UV antioxidant synergistic aid.

[0029] Preferably, the ethanol aqueous solution in step S1-2 is obtained by mixing deionized water and ethanol in a volume ratio of 1:2 to 3:1.

[0030] Preferably, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0031] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0032] S1-1, add 100 mg of nano-SiO2 into 100 mL of deionized water, ultrasonically disperse for 10 min, then add 10 mL of 2 mg / mL zinc chloride solution, then add 5 mL of 5% hydrochloric acid, ultrasonically disperse for 20 min, to obtain precursor solution 1;

[0033] S1-2, adding 36 mg of glucose, 11.2 mg of thioacetamide, and 23 mg of L-proline to 100 mL of ethanol aqueous solution, stirring for 5 min, adding the resulting mixture to the precursor solution 1, and ultrasonically dispersing for 30 min to obtain a precursor solution 2;

[0034] The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 2:3;

[0035] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 185°C for 12 hours, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 60°C for 8 hours to obtain synergistically modified SiO2 nanoparticles;

[0036] S2, grafting a polymer onto the synergistically modified SiO2 nanoparticles to obtain the anti-ultraviolet antioxidant synergist:

[0037] S2-1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1;

[0038] S2-2. Add 0.03 mg of benzoyl peroxide and 5 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 20 mL of ethanol, and ultrasonically disperse for 15 minutes. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 75°C for 6 hours, filter, and wash the solid product with deionized water and ethanol in turn to obtain the anti-UV antioxidant synergistic aid.

[0039] Preferably, the auxiliary agent includes one or more of a leveling agent, a dispersant, and a defoaming agent.

[0040] Preferably, the main resin is a mixture of one or both of polyurethane acrylic resin and epoxy acrylic resin and acrylic resin.

[0041] Preferably, the active monomer is at least one of dipropylene glycol diacrylate, tripropylene glycol diacrylate and pentaerythritol triacrylate.

[0042] Preferably, the acrylic plate surface coating material is prepared by the following method: by weight, 23-75 parts of the main resin, 1.8-8.5 parts of the anti-ultraviolet antioxidant synergist, 6-24 parts of the active monomer, 0.5-3.8 parts of the photoinitiator, and 1.2-6 parts of the auxiliary agent are mixed evenly to obtain the acrylic plate surface coating material.

[0043] The present invention also provides an acrylic plate surface treatment process, comprising the following steps: the acrylic plate to be treated is cleaned with ethanol, blown dry, the acrylic plate surface coating material as described above is evenly coated on the surface of the acrylic plate in a nitrogen atmosphere, and then irradiated and cured with a 172nm excimer lamp to form a coating with a thickness of 12-40μm, thereby completing the surface treatment.

[0044] The beneficial effects of the present invention are:

[0045] The present invention provides an acrylic plate surface coating material and an acrylic plate surface treatment process based on the material. In the coating material of the present invention, by adding an anti-ultraviolet antioxidant synergist, the wear resistance, anti-ultraviolet performance and anti-oxidation performance of the formed coating can be improved at the same time, so that the coating can provide longer-lasting protection for the acrylic plate, making it have better wear resistance and scratch resistance and surface resistance than traditional acrylic plates; and the effect of nanoparticles in the anti-ultraviolet antioxidant synergist can form a surface with concave-convex particles, and the coating surface can produce a matte effect through the diffuse reflection effect of the concave-convex particles;

[0046] The carbon dots in the anti-ultraviolet antioxidant synergist of the present invention can provide good antioxidant performance; on the other hand, the carbon dots have a good absorption effect on light in the ultraviolet band, thereby giving the anti-ultraviolet antioxidant synergist good anti-ultraviolet performance; Zn 2+ In the carbon dot modification stage, it can play a bridging role, so that the carbon dots are uniformly and massively grafted to the SiO2 surface, and the nano ZnO particles finally formed can further enhance the anti-ultraviolet performance of the anti-ultraviolet antioxidant synergist; and in the present invention, by combining the carbon dots with reducing properties with the nano ZnO particles and by the scavenging effect of the carbon dots on free radicals, it can overcome the defect of ZnO particles in traditional application schemes that potential risks are caused by the easy generation of strong oxidizing free radicals, so that the nano ZnO particles can provide good ultraviolet shielding effect in the coating system without worrying about the risks brought to the coating system by the strong oxidizing free radicals generated by them. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is the UV-visible absorption spectrum of the anti-UV antioxidant synergist prepared in Example 1;

[0048] Figure 2 This is the antioxidant performance test result of the present invention. DETAILED DESCRIPTION

[0049] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0050] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0051] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0052] The present invention provides an acrylic plate surface coating material, comprising the following components in parts by weight:

[0053] Main resin 23-75 parts;

[0054] 6-24 parts of active monomer;

[0055] Photoinitiator 0.5-3.8 parts;

[0056] 1.2-6 parts of additives;

[0057] 1.8-8.5 parts of anti-ultraviolet antioxidant synergist.

[0058] In a preferred embodiment, the main resin is a mixture of one or both of polyurethane acrylic resin and epoxy acrylic resin and acrylic resin.

[0059] In a preferred embodiment, the active monomer is at least one of dipropylene glycol diacrylate, tripropylene glycol diacrylate, and pentaerythritol triacrylate.

[0060] In a preferred embodiment, the photoinitiator is one or more of TPO, 819, 1173, 184, ITX, and 907.

[0061] In a preferred embodiment, the auxiliary agent includes one or more of a leveling agent, a dispersant, and a defoaming agent.

[0062] Furthermore, the leveling agent is one or more of TEGO432, TEGO410, BYK378, Digo 435, and Aifka 3883; further, the dispersant is one or more of Deqian DP983, BYK168, and Digo 710; further, the defoaming agent is one or more of Deqian 5300, Digo 815N, TEGO920, and BYK055.

[0063] In the present invention, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0064] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0065] S1-1, add 50-200 mg of nano-SiO2 into 50-200 mL of deionized water, ultrasonically disperse for 5-15 min, then add 5-20 mL of 2 mg / mL zinc chloride solution, then add 2-10 mL of 5% hydrochloric acid, ultrasonically disperse for 10-30 min, to obtain precursor solution 1;

[0066] S1-2, add 18-72 mg glucose, 5.6-22.4 mg thioacetamide, and 11.5-46 mg L-proline to 50-200 mL ethanol aqueous solution, stir for 2-15 min, add the obtained mixture to precursor solution 1, and disperse by ultrasonic for 15-60 min to obtain precursor solution 2;

[0067] The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 1:2 to 3:1;

[0068] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 175-195°C for 6-24h, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 50-70°C for 4-12h to obtain synergistically modified SiO2 nanoparticles;

[0069] S2. Grafting polymer onto synergistically modified SiO2 nanoparticles to obtain an anti-ultraviolet antioxidant synergist:

[0070] S2-1, adding 1.25-5 mg of vinyl triethoxysilane and 8-32 mg of methyl methacrylate to 25-100 mL of ethanol, stirring for 5-30 min, to obtain a mixture 1;

[0071] S2-2. Add 0.015-0.06 mg of benzoyl peroxide and 2.5-10 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 10-40 mL of ethanol, and ultrasonically disperse for 5-30 min. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 65-78°C for 3-12 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain an anti-UV antioxidant synergistic additive.

[0072] The acrylic plate surface coating material is prepared by the following method: by weight, 23-75 parts of a main resin, 1.8-8.5 parts of an anti-ultraviolet antioxidant synergist, 6-24 parts of an active monomer, 0.5-3.8 parts of a photoinitiator, and 1.2-6 parts of an auxiliary agent are uniformly mixed to obtain the acrylic plate surface coating material.

[0073] The present invention also provides an acrylic plate surface treatment process, comprising the following steps: the acrylic plate to be treated is cleaned with ethanol, blown dry, the above acrylic plate surface coating material is evenly coated on the surface of the acrylic plate under a nitrogen atmosphere, and then irradiated and cured with a 172nm excimer lamp to form a coating with a thickness of 12-40μm, thereby completing the surface treatment.

[0074] In the present invention, by adding an anti-ultraviolet antioxidant synergist, the wear resistance, anti-ultraviolet performance and anti-oxidation performance of the formed coating can be improved at the same time, so that the coating can provide longer-term protection for the acrylic plate, making it have better wear resistance, scratch resistance and surface resistance than traditional acrylic plates; and the effect of nanoparticles in the anti-ultraviolet antioxidant synergist can form a surface with concave-convex particles, and the diffuse reflection effect of the concave-convex particles can make the coating surface produce a matte effect. The principle of the anti-ultraviolet antioxidant synergist is described in detail below to facilitate the understanding of the present invention.

[0075] The present invention firstly mixes nano-SiO2 with zinc chloride, and then reacts with the silanol group on the surface of SiO2 with Zn 2+ The electrostatic adsorption and / or complexation of SiO2 surface can modify a large amount of Zn 2+ Then, glucose, thioacetamide, and L-proline were used as the main raw materials to synthesize a large number of carbon dots in situ on the SiO2 surface by hydrothermal method. The surface of the carbon dots has abundant functional groups such as hydroxyl, amino, and carboxyl groups, which can react with Zn 2+ Combination, so that carbon dots can be grafted onto the SiO2 surface in large quantities and evenly, and under high temperature, Zn 2+ Nano-ZnO particles will be further formed, and finally a composite system with nano-SiO2 as the carrier and loaded with nano-ZnO particles and carbon dots will be obtained: synergistically modified SiO2 nanoparticles (SiO2-ZnO-CDs); finally, a polymethacrylate polymer film layer modified with vinyltriethoxysilane is coated on the surface of SiO2-ZnO-CDs by in-situ polymerization to obtain an anti-UV antioxidant synergist.

[0076] Among them, the in situ synthesized carbon dots inherit the reducing properties of thioacetamide and L-proline very well, so that the carbon dots can provide good antioxidant properties for anti-UV antioxidant synergists; on the other hand, the carbon dots have a good absorption effect on light in the ultraviolet band through the interaction between photons and their energy bands, thereby giving the anti-UV antioxidant synergists better anti-UV properties.

[0077] Among them, Zn 2+In the carbon point modification stage, it can play a bridging role, so that the carbon points are uniformly and massively grafted to the SiO2 surface, and the nano ZnO particles formed at last can further enhance the anti-ultraviolet performance of the anti-ultraviolet antioxidant synergist: zinc oxide belongs to an N-type semiconductor, and the electrons on the valence band can accept the energy in the ultraviolet rays to make transitions, so that it has good ultraviolet absorption ability. However, nano ZnO particles are prone to release free radicals with strong oxidizing properties in the process of absorbing ultraviolet rays, and some potential risks are generated, which is an important factor limiting the use of nano ZnO particles as ultraviolet shielding agents; for example, when applied in organic materials (such as the organic coating system of the present invention), the free radicals with strong oxidizing properties will accelerate the degradation of organic matter, resulting in a shortened life of the organic material. In the present invention, by combining carbon points with reducing properties with nano ZnO particles, the above-mentioned defects of ZnO particles can be overcome, and the free radicals generated by them can be quickly removed by carbon points, so that nano ZnO particles provide good ultraviolet shielding in the coating system, and there is no need to worry about the risks brought to the coating system by the strong oxidizing free radicals generated by them.

[0078] Among them, SiO2 nanoparticles can, on the one hand, act as carriers to load carbon dots and ZnO particles to reduce their agglomeration; on the other hand, SiO2 nanoparticles themselves can significantly improve the friction resistance and surface hardness of the coating, and can also make the coating present a matte effect by forming a concave-convex structure on the surface.

[0079] Among them, the coating of SiO2-ZnO-CDs by polymethacrylate polymer modified by vinyltriethoxysilane can significantly improve the dispersion effect of inorganic material nanoparticles SiO2-ZnO-CD in the organic resin system, and the double bonds in vinyltriethoxysilane can participate in the polymerization process in the coating system, further enabling the anti-UV antioxidant synergist to be better dispersed in the coating system.

[0080] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.

[0081] In the following examples and comparative examples, the main raw materials and their sources are as follows:

[0082] Polyurethane acrylic resin, brand AgiSyn 271, purchased from Youming (Shanghai) Chemical Co., Ltd.;

[0083] Epoxy acrylic resin, brand name iForm 88821, purchased from Guangzhou Yousu 3D Technology Co., Ltd.;

[0084] Polyester acrylate, brand name iForm 88606, purchased from Guangzhou Yousu 3D Technology Co., Ltd.;

[0085] The active monomer is pentaerythritol triacrylate, brand M340, purchased from Youming (Shanghai) Chemical Co., Ltd.;

[0086] The photoinitiator is a mixture of BASF's IRGACURE 184 and BASF's TPO, with a mass ratio of 1:1; the defoamer is Deqian 5300, and the dispersant is Deqian DP983;

[0087] Nano-SiO2, with an average particle size of 40 nm and a brand name of TSP-L12, was purchased from Jiangsu Tianxing New Materials Co., Ltd.

[0088] Example 1

[0089] An acrylic plate surface coating material comprises the following components in parts by weight:

[0090] Main resin 62 parts;

[0091] 17 parts of active monomer;

[0092] 2.1 parts of photoinitiator;

[0093] 0.4 parts of leveling agent;

[0094] Dispersant 0.7 parts;

[0095] 0.5 parts of defoaming agent;

[0096] 4.5 parts of anti-ultraviolet antioxidant synergist.

[0097] The main resin includes 32 parts of polyester acrylate, 15 parts of polyurethane acrylate resin and 15 parts of epoxy acrylate resin.

[0098] The acrylic plate surface coating material is prepared by the following method: a main resin, an anti-ultraviolet antioxidant synergist, an active monomer, a photoinitiator, a leveling agent, a dispersant, and a defoamer are uniformly mixed according to a weight ratio to obtain the acrylic plate surface coating material.

[0099] Wherein, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0100] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0101] S1-1, add 100 mg of nano-SiO2 into 100 mL of deionized water, ultrasonically disperse for 10 min, then add 10 mL of 2 mg / mL zinc chloride solution, then add 5 mL of 5% hydrochloric acid, ultrasonically disperse for 20 min, to obtain precursor solution 1;

[0102] S1-2, 36 mg of glucose, 11.2 mg of thioacetamide, and 23 mg of L-proline were added to 100 mL of ethanol aqueous solution, stirred for 5 min, and the resulting mixture was added to precursor solution 1, and ultrasonically dispersed for 30 min to obtain precursor solution 2;

[0103] The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 2:3;

[0104] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 185°C for 12 hours, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 60°C for 8 hours to obtain synergistically modified SiO2 nanoparticles;

[0105] S2. Grafting polymer onto synergistically modified SiO2 nanoparticles to obtain an anti-ultraviolet antioxidant synergist:

[0106] S2-1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1;

[0107] S2-2. Add 0.03 mg of benzoyl peroxide and 5 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 20 mL of ethanol, and ultrasonically disperse for 15 min. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 75°C for 6 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain an anti-UV antioxidant synergistic additive.

[0108] Example 2

[0109] An acrylic plate surface coating material comprises the following components in parts by weight:

[0110] Main resin 62 parts;

[0111] 17 parts of active monomer;

[0112] 2.1 parts of photoinitiator;

[0113] 0.4 parts of leveling agent;

[0114] Dispersant 0.7 parts;

[0115] 0.5 parts of defoaming agent;

[0116] 4.0 parts of anti-ultraviolet antioxidant synergist.

[0117] The main resin includes 36 parts of polyester acrylate, 13 parts of polyurethane acrylic resin and 13 parts of epoxy acrylic resin.

[0118] The acrylic plate surface coating material is prepared by the following method: a main resin, an anti-ultraviolet antioxidant synergist, an active monomer, a photoinitiator, a leveling agent, a dispersant, and a defoamer are uniformly mixed according to a weight ratio to obtain the acrylic plate surface coating material.

[0119] Wherein, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0120] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0121] S1-1, add 100 mg of nano-SiO2 into 100 mL of deionized water, ultrasonically disperse for 10 min, then add 10 mL of 2 mg / mL zinc chloride solution, then add 5 mL of 5% hydrochloric acid, ultrasonically disperse for 20 min, to obtain precursor solution 1;

[0122] S1-2, 36 mg of glucose, 11.2 mg of thioacetamide, and 23 mg of L-proline were added to 100 mL of ethanol aqueous solution, stirred for 5 min, and the resulting mixture was added to precursor solution 1, and ultrasonically dispersed for 30 min to obtain precursor solution 2;

[0123] The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 2:3;

[0124] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 185°C for 12 hours, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 60°C for 8 hours to obtain synergistically modified SiO2 nanoparticles;

[0125] S2. Grafting polymer onto synergistically modified SiO2 nanoparticles to obtain an anti-ultraviolet antioxidant synergist:

[0126] S2-1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1;

[0127] S2-2. Add 0.03 mg of benzoyl peroxide and 5 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 20 mL of ethanol, and ultrasonically disperse for 15 min. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 75°C for 6 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain an anti-UV antioxidant synergistic additive.

[0128] Example 3

[0129] An acrylic plate surface coating material comprises the following components in parts by weight:

[0130] Main resin 62 parts;

[0131] 17 parts of active monomer;

[0132] 2.1 parts of photoinitiator;

[0133] 0.4 parts of leveling agent;

[0134] Dispersant 0.7 parts;

[0135] 0.5 parts of defoaming agent;

[0136] 5.0 parts of anti-ultraviolet antioxidant synergist.

[0137] The main resin includes 30 parts of polyester acrylate, 16 parts of polyurethane acrylic resin and 16 parts of epoxy acrylic resin.

[0138] The acrylic plate surface coating material is prepared by the following method: a main resin, an anti-ultraviolet antioxidant synergist, an active monomer, a photoinitiator, a leveling agent, a dispersant, and a defoamer are uniformly mixed according to a weight ratio to obtain the acrylic plate surface coating material.

[0139] Wherein, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0140] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0141] S1-1, add 100 mg of nano-SiO2 into 100 mL of deionized water, ultrasonically disperse for 10 min, then add 10 mL of 2 mg / mL zinc chloride solution, then add 5 mL of 5% hydrochloric acid, ultrasonically disperse for 20 min, to obtain precursor solution 1;

[0142] S1-2, 36 mg of glucose, 11.2 mg of thioacetamide, and 23 mg of L-proline were added to 100 mL of ethanol aqueous solution, stirred for 5 min, and the resulting mixture was added to precursor solution 1, and ultrasonically dispersed for 30 min to obtain precursor solution 2;

[0143] The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 2:3;

[0144] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 185°C for 12 hours, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 60°C for 8 hours to obtain synergistically modified SiO2 nanoparticles;

[0145] S2. Grafting polymer onto synergistically modified SiO2 nanoparticles to obtain an anti-ultraviolet antioxidant synergist:

[0146] S2-1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1;

[0147] S2-2. Add 0.03 mg of benzoyl peroxide and 4.5 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 20 mL of ethanol, and ultrasonically disperse for 15 minutes. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 75°C for 6 hours, filter, and wash the solid product with deionized water and ethanol in turn to obtain an anti-UV antioxidant synergistic additive.

[0148] Comparative Example 1

[0149] The only difference between this example and Example 1 is that the raw material components do not contain an anti-ultraviolet antioxidant synergist.

[0150] Comparative Example 2

[0151] The only difference between this example and Example 1 is that the preparation method of the anti-ultraviolet antioxidant synergist is different. In this example, step S2 is not included, that is, in this example, the synergistically modified SiO2 nanoparticles prepared in step S1 of Example 1 are used as the anti-ultraviolet antioxidant synergist.

[0152] Comparative Example 3

[0153] The difference between this example and Example 1 is that the preparation method of the anti-ultraviolet antioxidant synergist is different. In this example, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0154] S1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1;

[0155] S2. Add 0.03 mg of benzoyl peroxide and 5 mg of nano-SiO2 into 20 mL of ethanol, and perform ultrasonic dispersion for 15 min. Add the obtained dispersion into mixture 1 under stirring, heat under reflux at 75° C. for 6 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain an anti-UV antioxidant synergistic additive.

[0156] Comparative Example 4

[0157] The difference between this example and Example 1 is that the preparation method of the anti-ultraviolet antioxidant synergist is different. In this example, the anti-ultraviolet antioxidant synergist is prepared by the following steps:

[0158] S1. Preparation of synergistically modified SiO2 nanoparticles:

[0159] S1-1, add 100 mg of nano-SiO2 into 100 mL of deionized water, ultrasonically disperse for 10 min, then add 5 mL of 5% hydrochloric acid, ultrasonically disperse for 20 min, to obtain precursor solution 1;

[0160] S1-2, 36 mg of glucose, 11.2 mg of thioacetamide, and 23 mg of L-proline were added to 100 mL of ethanol aqueous solution, stirred for 5 min, and the resulting mixture was added to precursor solution 1, and ultrasonically dispersed for 30 min to obtain precursor solution 2;

[0161] The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 2:3;

[0162] S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 185°C for 12 hours, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 60°C for 8 hours to obtain synergistically modified SiO2 nanoparticles;

[0163] S2. Grafting polymer onto synergistically modified SiO2 nanoparticles to obtain an anti-ultraviolet antioxidant synergist:

[0164] S2-1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1;

[0165] S2-2. Add 0.03 mg of benzoyl peroxide and 5 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 20 mL of ethanol, and ultrasonically disperse for 15 min. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 75°C for 6 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain an anti-UV antioxidant synergistic additive.

[0166] 1. Performance characterization of anti-ultraviolet and anti-oxidant synergistic agents:

[0167] 1. Reference Figure 1 , is the UV-visible absorption spectrum of the anti-UV antioxidant synergistic aid prepared in Example 1. It can be seen that it has absorption in the range of 150-450nm.

[0168] 2. Antioxidant performance test

[0169] 10 mg of the anti-ultraviolet antioxidant synergistic aid prepared in Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 were respectively added to 15 mL of ethanol, ultrasonically dispersed for 10 minutes, and allowed to stand; a blank ethanol solution was used as a control example; then a DPPH kit (Isejiu (Jiangsu Lianyungang) Biotechnology Co., Ltd.) was used to test the absorption intensity of the supernatant at 515 nm at different standing times (1 h, 2.5 h, 5 h) to characterize the antioxidant content in the supernatant. As the concentration of the antioxidant increased, the absorption intensity of DPPH at 515 nm decreased.

[0170] according to Figure 2 The test results shown in the figure show that during the standing period of 1h, 2.5h and 5h, the absorbance of Example 1, Comparative Example 2 and Comparative Example 4 gradually decreased, indicating that the concentration of the antioxidant was gradually increasing, and that Example 1 had the strongest antioxidant capacity, while Comparative Example 3 had no antioxidant capacity.

[0171] 2. Application Testing

[0172] The acrylic plate was surface treated using the coating materials prepared in the examples and comparative examples:

[0173] After the acrylic plate was cleaned with ethanol and dried, the acrylic plate surface coating material prepared in each example was evenly coated on the surface of the acrylic plate under a nitrogen atmosphere, and then irradiated and cured with a 172nm excimer lamp (energy of 750mJ / cm 2 ) forms a coating with a thickness of 25 μm to complete the surface treatment.

[0174] Then the performance of the coating on the surface of the acrylic plate was tested, and the test results are shown in Table 1 below:

[0175] Table 1

[0176]

[0177] in:

[0178] Pencil hardness: Tested in accordance with GB / T 6739-2006.

[0179] The adhesion test adopts the hundred-grid method, and the reference standard is GB / T 9286-1998, among which grade 0 is the best;

[0180] The RCA wear test uses an RCA wear tester with a pressure of 175g applied to the sample. The number of frictions when the coating is fully penetrated is used as the evaluation standard. For example, 600 means that the coating is fully penetrated after 600 frictions.

[0181] The coating on the surface of the acrylic plate was irradiated with an ultraviolet lamp with a wavelength of 350nm and a power of 30W for 20 days, and then the adhesion and wear resistance of the coating were tested according to the above test method to evaluate the anti-ultraviolet performance of the coating. The test results are shown in Table 2 below:

[0182] Table 2

[0183]

[0184] It can be seen from the test results in Table 1 that the coatings prepared in Examples 1-3 have excellent friction resistance, high surface hardness and good adhesion; the wear resistance and surface hardness of Comparative Example 1 are significantly reduced, which is attributed to the fact that no SiO2 nanoparticles are added; the wear resistance and surface hardness of Comparative Example 2 also show a certain degree of decline, which is mainly attributed to the fact that no polymer is grafted onto the synergistically modified SiO2 nanoparticles, which affects its dispersion performance in the coating system.

[0185] Combining the test results of Table 1 and Table 2, it can be seen that the adhesion and friction resistance of the coatings of Examples 1-3 remain basically unchanged after ultraviolet irradiation, indicating that they have excellent resistance to ultraviolet oxidation; in Comparative Example 1, since no anti-ultraviolet antioxidant synergist is added, its anti-ultraviolet oxidation ability is the worst; in Comparative Example 2, due to the poor dispersion effect of the anti-ultraviolet antioxidant synergist in the coating, the effect of SiO2 nanoparticles on improving the wear resistance is weakened, and the effect of the active ingredients with ultraviolet shielding effect is also negatively affected, resulting in a decrease in its adhesion and friction resistance; in Comparative Example 3, due to the lack of carbon dots that absorb ultraviolet rays, the anti-ultraviolet oxidation performance is significantly reduced, showing a decrease in adhesion and friction resistance; the reason for the decrease in anti-ultraviolet oxidation performance in Comparative Example 4 is the lack of the ultraviolet shielding effect provided by zinc oxide.

[0186] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. An acrylic plate surface coating material, characterized in that: The composition comprises the following components in parts by weight: Main resin 23-75 parts; 6-24 parts of active monomer; Photoinitiator 0.5-3.8 parts; 1.2-6 parts of additives; 1.8-8.5 parts of anti-ultraviolet antioxidant synergist; The anti-ultraviolet antioxidant synergist is prepared by the following steps: S1. Preparation of synergistically modified SiO2 nanoparticles: S1-1, adding nano-SiO2 to deionized water, ultrasonically dispersing, then adding zinc chloride solution, and then adding hydrochloric acid, ultrasonically dispersing to obtain precursor solution 1; S1-2, adding glucose, thioacetamide and L-proline to an ethanol aqueous solution, stirring, adding the obtained mixture to the precursor solution 1, and ultrasonically dispersing to obtain a precursor solution 2; S1-3, transferring the precursor solution 2 to a polytetrafluoroethylene-lined reactor, reacting under heating, cooling to room temperature after the reaction, filtering, and vacuum drying the obtained solid to obtain synergistically modified SiO2 nanoparticles; S2, grafting a polymer onto the synergistically modified SiO2 nanoparticles to obtain the anti-ultraviolet antioxidant synergist: S2-1, adding vinyl triethoxysilane and methyl methacrylate into ethanol, stirring to obtain a mixture 1; S2-2. Add the initiator and the synergistically modified SiO2 nanoparticles prepared in step S1 into ethanol, disperse them ultrasonically, add the obtained dispersion into mixture 1 under stirring, heat to reflux, filter after the reaction is completed, and wash the solid product with deionized water and ethanol in sequence to obtain the anti-UV antioxidant synergistic additive.

2. The acrylic plate surface coating material according to claim 1, characterized in that: The anti-ultraviolet antioxidant synergist is prepared by the following steps: S1. Preparation of synergistically modified SiO2 nanoparticles: S1-1, add 50-200 mg of nano-SiO2 into 50-200 mL of deionized water, ultrasonically disperse for 5-15 min, then add 5-20 mL of 2 mg / mL zinc chloride solution, then add 2-10 mL of 5% hydrochloric acid, ultrasonically disperse for 10-30 min, to obtain precursor solution 1; S1-2, adding 18-72 mg of glucose, 5.6-22.4 mg of thioacetamide, and 11.5-46 mg of L-proline to 50-200 mL of ethanol aqueous solution, stirring for 2-15 min, adding the obtained mixture to the precursor solution 1, and ultrasonically dispersing for 15-60 min to obtain precursor solution 2; S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 175-195°C for 6-24h, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 50-70°C for 4-12h to obtain synergistically modified SiO2 nanoparticles; S2, grafting a polymer onto the synergistically modified SiO2 nanoparticles to obtain the anti-ultraviolet antioxidant synergist: S2-1, adding 1.25-5 mg of vinyl triethoxysilane and 8-32 mg of methyl methacrylate to 25-100 mL of ethanol, stirring for 5-30 min, to obtain a mixture 1; S2-2. Add 0.015-0.06 mg of benzoyl peroxide and 2.5-10 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 10-40 mL of ethanol, and disperse them ultrasonically for 5-30 min. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 65-78°C for 3-12 h, filter, and wash the solid product with deionized water and ethanol in turn to obtain the anti-UV antioxidant synergistic aid.

3. The acrylic plate surface coating material according to claim 2, characterized in that: in, The ethanol aqueous solution in step S1-2 is obtained by mixing deionized water and ethanol in a volume ratio of 1:2 to 3:

1.

4. The acrylic plate surface coating material according to claim 2, characterized in that: The anti-ultraviolet antioxidant synergist is prepared by the following steps: S1. Preparation of synergistically modified SiO2 nanoparticles: S1-1, add 100 mg of nano-SiO2 into 100 mL of deionized water, ultrasonically disperse for 10 min, then add 10 mL of 2 mg / mL zinc chloride solution, then add 5 mL of 5% hydrochloric acid, ultrasonically disperse for 20 min, to obtain precursor solution 1; S1-2, adding 36 mg of glucose, 11.2 mg of thioacetamide, and 23 mg of L-proline to 100 mL of ethanol aqueous solution, stirring for 5 min, adding the resulting mixture to the precursor solution 1, and ultrasonically dispersing for 30 min to obtain a precursor solution 2; The ethanol aqueous solution is obtained by mixing deionized water and ethanol in a volume ratio of 2:3; S1-3, transfer the precursor solution 2 to a polytetrafluoroethylene-lined reactor, react at 185°C for 12 hours, cool to room temperature after the reaction, filter, and vacuum dry the obtained solid at 60°C for 8 hours to obtain synergistically modified SiO2 nanoparticles; S2, grafting a polymer onto the synergistically modified SiO2 nanoparticles to obtain the anti-ultraviolet antioxidant synergist: S2-1, adding 2.5 mg of vinyl triethoxysilane and 16 mg of methyl methacrylate to 50 mL of ethanol, stirring for 10 min, to obtain a mixture 1; S2-2. Add 0.03 mg of benzoyl peroxide and 5 mg of the synergistically modified SiO2 nanoparticles prepared in step S1 to 20 mL of ethanol, and ultrasonically disperse for 15 minutes. Add the resulting dispersion to mixture 1 under stirring, heat under reflux at 75°C for 6 hours, filter, and wash the solid product with deionized water and ethanol in turn to obtain the anti-UV antioxidant synergistic aid.

5. The acrylic plate surface coating material according to claim 1, characterized in that: The additives include one or more of leveling agents, dispersants, and defoamers.

6. The acrylic plate surface coating material according to claim 1, characterized in that: The main resin is a mixture of one or two of polyurethane acrylic resin and epoxy acrylic resin and acrylic resin.

7. The acrylic plate surface coating material according to claim 1, characterized in that: The active monomer is at least one of dipropylene glycol diacrylate, tripropylene glycol diacrylate and pentaerythritol triacrylate.

8. The acrylic plate surface coating material according to claim 1, characterized in that: The acrylic plate surface coating material is prepared by the following method: by weight, 23-75 parts of main resin, 1.8-8.5 parts of anti-ultraviolet antioxidant synergist, 6-24 parts of active monomer, 0.5-3.8 parts of photoinitiator and 1.2-6 parts of auxiliary agent are mixed evenly to obtain the acrylic plate surface coating material.

9. A surface treatment process for acrylic plate, characterized in that: The following steps are involved: The acrylic plate to be treated is cleaned with ethanol and blown dry, and the acrylic plate surface coating material as described in any one of claims 1 to 8 is evenly coated on the surface of the acrylic plate under a nitrogen atmosphere, and then irradiated and cured with a 172nm excimer lamp to form a coating with a thickness of 12-40μm to complete the surface treatment.