Ion balance layer for electrochromic device and preparation method thereof, electrochromic device and application thereof
By using hydrated vanadium pentoxide and a C-O-C bond organic additive network in electrochromic devices, a continuous V-O structure is formed, which solves the color change problem and film void problem caused by redox reactions in traditional technology, and improves electrochromic performance. Speed and color saturation improve the overall performance of electrochromic devices.
Patent Information
- Application Number
- CN202410845103.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The ion storage layer of existing electrochromic devices has obvious color changes during the redox reaction, which affects the color purity and contrast. In addition, there are nanoscale gaps in the film when forming the film using traditional nanoparticle coatings or physical coating methods, which affects the utilization efficiency of vanadium. .
Using hydrated vanadium pentoxide and an organic additive network containing C-O-C bonds as the main body, a continuous V-O network structure is formed through hydrogen bond interaction, which alleviates the problem of nanoscale voids in the film, improves the utilization efficiency of vanadium, and optimizes the concentration of active ions. The migration rate and charge per unit area improve the electrochromic speed and ion balance capacity.
It effectively improves the electrochemical and optical properties of electrochromism, increases the speed and color saturation of electrochromism, enhances the sensitivity and ion balance capacity of electrochromic devices, reduces color interference, and improves the overall performance of the device .
Smart Images

Figure CN118393789B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of material technology, and in particular to an ion balance layer for an electrochromic device and a preparation method thereof, an electrochromic device and applications thereof. Background Art
[0002] In the related art, the ion storage layer material needs to have an oxidation-reduction reaction to achieve charge balance, thereby stabilizing the life of the device. In addition, the ion storage layer also requires that the oxidation-reduction process should not have obvious color changes, thereby ensuring the purity and contrast of the color change, that is, it needs to have a smaller coloring efficiency. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one object of the present invention is to provide an ion balance layer for an electrochromic device, wherein the color of hydrated vanadium pentoxide has little effect on the color change of the device and the color change saturation of the device is high.
[0004] Another object of the present invention is to provide a method for preparing an ion balance layer for an electrochromic device.
[0005] Another object of the present invention is to provide an electrochromic device.
[0006] Another object of the present invention is to provide an application of an electrochromic device.
[0007] According to an embodiment of the first aspect of the present invention, the present invention provides an ion balance layer for an electrochromic device, comprising, by mass percentage: 98% to 99.9% of hydrated vanadium pentoxide and 0.1% to 2% of an organic additive with a COC bond as the main network,
[0008] When the voltage is 1.0V to 3.5V, the migration rate of active ions in the ion balance layer is v, wherein v satisfies: v>1x10 -11 cm 2 / s, the charge per unit area in the ion balance layer is C, wherein C satisfies: C>8mC / cm 2 .
[0009] According to the ion balance layer for electrochromic devices of the present invention, the hydrated vanadium pentoxide and the network of the main chain additive containing COC bonds have hydrogen bond interactions, resulting in the growth process of the vanadium oxide film using the polymer segment as a template to form a continuous VO network structure, which effectively alleviates the nano-scale gaps in the film caused by the traditional nanoparticle coating or physical plating method, and improves the utilization efficiency of vanadium. Compared with traditional anhydrous vanadium pentoxide, the hydrated vanadium pentoxide used in the present invention can effectively improve the electrochemical and optical properties of electrochromism, and the entry of water increases the VO bond space gap, thereby prompting vanadium oxide to expose more active sites, shortening the diffusion path of active ions in the VO structure, thereby promoting the improvement of electrochromic speed and ion balance capacity, and thus having excellent electrochromic ion balance performance.
[0010] According to some embodiments of the present invention, when the voltage is 1.0V to 3.5V, the migration rate of active ions in the ion balance layer is v, wherein v satisfies: 2x10 -10 cm 2 / s≥v>1x10 -11 cm 2 / s,
[0011] The charge per unit area in the ion balance layer is C, where C satisfies: 10 mC / cm 2 ≥C>8mC / cm 2 .
[0012] According to some embodiments of the present invention, the molecular formula of the hydrated vanadium pentoxide is V2O5·xH2O, wherein x satisfies: 2.5≥x>0.1.
[0013] According to some embodiments of the present invention, the organic auxiliary agent is an organic polymer mixture containing a large number of chain ether bonds.
[0014] According to some embodiments of the present invention, the organic polymer mixture includes an aqueous acrylic emulsion and / or an aqueous polyurethane emulsion.
[0015] According to some embodiments of the present invention, the roughness of the surface of the ion balance layer is Ra, wherein the Ra satisfies: Ra≤20 nm.
[0016] According to some embodiments of the present invention, the thickness of the ion balance layer is d1, wherein d1 satisfies: 30 nm≤d1≤90 nm.
[0017] According to an embodiment of the second aspect of the present invention, the present invention provides a method for preparing an ion balance layer for an electrochromic device according to an embodiment of the first aspect of the present invention, comprising the following steps:
[0018] Preparation of hydrated vanadium pentoxide sol: dissolving a vanadium-containing compound in a hydrogen peroxide solution, reacting to obtain a sol containing hydrated vanadium pentoxide, and diluting to obtain a sol dispersion for later use;
[0019] An organic auxiliary agent with a COC bond as the main network is prepared, and the precursors of the organic auxiliary agent are mixed, prepolymerized, and emulsified to obtain the organic auxiliary agent with a COC bond as the main network, wherein the organic auxiliary agent with a COC bond as the main network is an aqueous acrylic emulsion or an aqueous polyurethane emulsion;
[0020] Mixing, adding the organic additive to the sol dispersion, reacting to obtain an ion balance layer slurry;
[0021] Film forming: coating the ion balance material to form a film, and baking to obtain an ion balance layer.
[0022] According to some embodiments of the present invention, the vanadium-containing compound includes at least one of vanadium pentoxide, vanadyl sulfate, ammonium vanadate and ammonium metavanadate.
[0023] According to some embodiments of the present invention, the precursor of the organic auxiliary agent includes: at least one of methyl methacrylate, methyl acrylate, styrene, acrylonitrile, hydroxypropyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, itaconic acid, acrylamide, polyethylene glycol methacrylate, polymethyl methacrylate, polydioxolane, polymethyl methacrylate, polyethyl methacrylate, and isobornyl methacrylate;
[0024] Or at least one of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate and polyether polyol, polyether diol, polyethylene glycol, polytetramethylene ether, 1,4-butanediol, polyethylene adipate, polyoxypropylene ether diol, polytetramethylene ether glycol and polyester polyol.
[0025] According to an embodiment of the third aspect of the present invention, the present invention provides an electrochromic device, comprising:
[0026] The electrochromic layer, ion conduction layer, ion balance layer and transparent conductive film are stacked in sequence.
[0027] The ion balance layer is attached to the transparent conductive film, and the ion balance layer is the ion balance layer described in the embodiment of the first aspect of the present invention, or the ion balance layer prepared by the preparation method described in the embodiment of the first aspect of the present invention.
[0028] According to some embodiments of the present invention, the adhesion force between the ion balance layer and the transparent conductive film is F, and F satisfies: F≥4B.
[0029] According to some embodiments of the present invention, the electrochromic layer includes at least one of viologen and its derivatives, polythiophene, polypyrrole, polyaniline and its derivatives, tungsten oxide, nickel oxide and vanadium oxide.
[0030] According to some embodiments of the present invention, the ion conducting layer comprises at least one of PEO, PVDF, PMMA and PANI systems.
[0031] According to an embodiment of the fourth aspect of the present invention, the present invention provides an application of the electrochromic device according to an embodiment of the fourth aspect of the present invention, wherein the electrochromic device is used for electronic and electrical components, automobile windows, rearview mirrors and architectural glass windows.
[0032] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is the interaction process between the polyurethane-based additive and the vanadium oxide polyhedron according to a specific embodiment of the present invention;
[0034] Figure 2 This is the coordination and decoordination process between the vanadium ion and the ether bond according to a specific embodiment of the present invention. DETAILED DESCRIPTION
[0035] The ion balance layer for an electrochromic device according to the first aspect of the present invention is described in detail below.
[0036] According to the first aspect of the present invention, the ion balance layer for the electrochromic device includes an organic auxiliary agent with a COC bond as the main network of hydrated vanadium pentoxide. The hydrated vanadium pentoxide and the chain-like main auxiliary agent network containing COC bonds have hydrogen bond interactions, resulting in the growth process of the vanadium oxide film using the polymer segment as a template to form a continuous VO network structure, which effectively alleviates the nanoscale gaps in the film caused by the traditional nanoparticle coating or physical plating method, and improves the utilization efficiency of vanadium. Compared with traditional anhydrous vanadium pentoxide, the present invention uses hydrated vanadium pentoxide to effectively improve the electrochemical and optical properties of electrochromism. The entry of water increases the VO bond space gap, which can promote vanadium oxide to expose more active sites and shorten the diffusion path of active ions in the VO structure, thereby promoting the improvement of electrochromic speed and ion balance capacity. Here, the hydrated vanadium pentoxide is a hydrated amorphous vanadium pentoxide, most of the molecules are arranged in a disordered manner, and less than 20% of the crystal structure is allowed to exist in the molecular structure.
[0037] The content of the organic additive with COC bond as the main network is 0.1% to 2% by mass, and the balance is hydrated vanadium pentoxide. In this way, a small amount of the organic additive with COC bond as the main network is mixed into a large amount of hydrated vanadium pentoxide.
[0038] When the voltage is 1.0V to 3.5V, the migration rate of active ions in the ion balance layer is v, where v satisfies: v>1x10 -11 cm 2 / s. With this setting, if v is less than 1.0x10 -11 cm 2 / s, the migration rate of active ions in the ion balance layer is small, the migration rate of active ions is slow, the electrochromic speed is slow, and the sensitivity of the electrochromic device is poor. By setting, v satisfies v>1x10 -11 cm 2 / s, then under the normal operating voltage of the electrochromic device, the migration rate of the active ions in the ion balance layer is faster, thereby promoting a faster electrochromic speed and a stronger sensitivity of the electrochromic device.
[0039] The charge per unit area in the ion balance layer is C, where C satisfies: C>8mC / cm 2 If C is less than 8mC / cm 2 , then the charge per unit area in the ion balance layer is small, the ion balance capacity in the ion balance layer is small, and the ion balance ability may be poor. By setting, C satisfies: C>8mC / cm 2 , under the normal operating voltage of the electrochromic device, the ion balance capacity in the ion balance layer is large, thereby promoting a large ion balance capacity.
[0040] According to the ion balance layer for electrochromic devices of a specific embodiment of the present invention, the hydrated vanadium pentoxide and the network of the main chain additive containing COC bonds have hydrogen bond interactions, resulting in the growth process of the vanadium oxide film using the polymer segment as a template to form a continuous VO network structure, which effectively alleviates the nano-scale voids in the film caused by the traditional nanoparticle coating or physical plating method, and improves the utilization efficiency of vanadium. Compared with traditional anhydrous vanadium pentoxide, the present invention uses hydrated vanadium pentoxide to effectively improve the electrochemical and optical properties of electrochromism. The entry of water increases the VO bond space gap, thereby causing the vanadium oxide to expose more active sites, shortening the diffusion path of active ions in the VO structure, thereby promoting the improvement of the electrochromic speed and ion balance capacity, and thus having excellent electrochromic ion balance performance.
[0041] According to some embodiments of the present invention, when the voltage is 1.0V to 3.5V, the migration rate of active ions in the ion balance layer is v, where v satisfies: 2x10 -10 cm 2 / s≥v>1x10 -11 cm 2 / s. With this setting, if v is less than 1.0x10 - 11 cm 2 / s, the migration rate of active ions in the ion balance layer is small, the migration rate of active ions is slow, the electrochromic speed is slow, and the sensitivity of the electrochromic device is poor; if v is greater than 2x10 -10 cm 2 / s, the migration rate of active ions in the ion balance layer is faster, which may make the high temperature stability of the color-changing material poor. By setting, v satisfies 2x10 - 10 cm 2 / s≥v>1x10 -11 cm 2 / s, then under the normal operating voltage of the electrochromic device, the migration rate of the active ions in the ion balance layer is appropriate, thereby promoting a faster electrochromic speed, a stronger sensitivity of the electrochromic device, and a higher color saturation of the color-changing material.
[0042] According to some embodiments of the present invention, the charge per unit area in the ion balance layer is C, where C satisfies: 10 mC / cm 2 ≥C>8mC / cm 2 If C is less than 8mC / cm 2 , the charge per unit area in the ion balance layer is small, the ion balance capacity in the ion balance layer is small, and the ion balance ability may be poor; if C is greater than 10mC / cm 2 , then the charge per unit area in the ion balance layer is large, the vanadium layer thickness may have a greater impact on the color, and the color saturation may be poor. By setting, C satisfies: 10mC / cm 2 ≥C>8mC / cm 2 , under the normal operating voltage of the electrochromic device, the ion balance capacity in the ion balance layer is appropriate, thereby promoting a large ion balance capacity.
[0043] According to some embodiments of the present invention, the molecular formula of hydrated vanadium pentoxide is V2O5·xH2O, wherein x satisfies: 2.5≥x>0.1. In this way, when x is less than 0.1, the water content in the hydrated vanadium pentoxide molecule is less, which may result in fewer active sites of vanadium oxide, smaller VO bond space gap, and the diffusion path of active ions in the VO structure may become longer, thereby affecting the electrochromic speed and ion balance capacity of the ion balance layer; when x is greater than 2.5, the water content in the hydrated vanadium pentoxide molecule is more, which reduces the vanadium pentoxide content in the hydrated vanadium pentoxide molecule, thereby affecting the electrochromic speed and ion balance capacity of the ion balance layer. By setting x to satisfy 2.5≥x>0.1, the water content in the hydrated vanadium pentoxide molecule is sufficient, and the VO bond space gap is increased, so that the vanadium oxide can be prompted to expose more active sites, shorten the diffusion path of active ions in the VO structure, thereby promoting the improvement of electrochromic speed and ion balance capacity.
[0044] According to some embodiments of the present invention, the organic additive is an organic polymer mixture containing a large number of chain ether bonds. In this way, the organic polymer mixture containing a large number of chain ether bonds may also contain other functional groups, such as hydroxyl groups. In this way, the COC bond is a chain-like main body additive network with hydrogen bond interactions, resulting in the growth process of the vanadium oxide film using the polymer segment as a template to form a continuous VO network structure, which effectively alleviates the presence of nano-scale voids in the film caused by traditional nanoparticle coatings or physical plating methods, improves the utilization efficiency of vanadium, and other functional groups such as hydroxyl groups form auxiliary hydrogen bonds, etc., to promote the stable combination of the vanadium oxide film and the polymer segment template.
[0045] According to some embodiments of the present invention, the organic polymer mixture includes an aqueous acrylic emulsion and / or an aqueous polyurethane emulsion. In this way, the aqueous acrylic emulsion and / or the aqueous polyurethane emulsion have good compatibility with hydrated vanadium pentoxide, which is conducive to forming a uniform ion balance layer of the electrochromic device. In addition, the aqueous acrylic emulsion and / or the aqueous polyurethane emulsion include a large number of chain ether bonds and neutral polar functional groups (such as -OH, -COO-, -CN) that can interact with the hydrated vanadium oxide polyhedron, and the main interaction mode is hydrogen bonds between molecules, such as Figure 1 As shown. Therefore, the organic polymer network is used as a template to form a continuous hydrated vanadium pentoxide film, improve the utilization rate of vanadium oxide, reduce the film thickness by 20%-50%, and thus reduce the effect of the color of vanadium pentoxide on the color change of the device and improve the color change saturation of the device. In addition, the selection of a polymer network containing ether bonds can balance the coordination and decoordination capabilities of lithium ions. Figure 2 , increasing the electrochemical reaction rate of the vanadium oxide film layer, combined with the reduction of film thickness, can shorten the color change time by more than 20%.
[0046] According to some embodiments of the present invention, the roughness of the surface of the ion balance layer is Ra, wherein Ra satisfies: Ra≤20nm. In this way, if Ra is greater than 20nm, the roughness of the surface of the ion balance layer is large, and the flatness of the ion balance layer is poor, so that the charge per unit area in the ion balance layer fluctuates greatly, which may bring the risk of uneven discoloration. By setting so that Ra satisfies Ra≤20nm, the roughness of the surface of the ion balance layer is appropriate, the ion balance capacity of the balance membrane is large, and the formed electrochromic device is reliable. Optionally, Ra is 2nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm or 20nm, but is not limited thereto.
[0047] According to some embodiments of the present invention, the thickness of the ion balance layer is d1, wherein d1 satisfies: 30nm≤d1≤90nm. In this way, if d1 is less than 30nm, the thickness of the ion balance layer is small, the ions and electricity in the ion balance layer are small, and the electrochromic electrochemical and optical properties of the ion balance layer may be poor; if d1 is greater than 90nm, the thickness of the ion balance layer is large, and the hydrated vanadium pentoxide has a greater impact on the color of the electrochromic device, thereby making the saturation lower. By setting d1 to satisfy 30nm≤d1≤90nm, the thickness of the surface of the ion balance layer is appropriate, the electrochromic electrochemical and optical properties of the ion balance layer are excellent, and the cost of the formed electrochromic device is low. Optionally, d1 is 35nm, 45nm, 57nm, 65nm, 70nm, 75nm, 80nm, 85nm or 90nm, but is not limited thereto.
[0048] According to an embodiment of the second aspect of the present invention, the present invention provides a method for preparing an ion balance layer for an electrochromic device according to an embodiment of the first aspect of the present invention, comprising the following steps:
[0049] To prepare the hydrated vanadium pentoxide sol, a vanadium-containing compound is dissolved in a hydrogen peroxide solution, reacted, and a sol containing hydrated vanadium pentoxide is obtained, which is diluted to obtain a sol dispersion for standby use. In this arrangement, the vanadium-containing compound is first formed into a sol dispersion for easy mixing with an aqueous acrylic emulsion or an aqueous polyurethane emulsion.
[0050] An organic additive with COC bonds as the main network is prepared, and the precursors of the organic additive are mixed, prepolymerized, and emulsified to obtain the organic additive with COC bonds as the main network, and the organic additive with COC bonds as the main network is a water-based acrylic emulsion or a water-based polyurethane emulsion;
[0051] Mixing, adding an organic additive to the sol dispersion, and reacting to obtain an ion balance layer slurry;
[0052] Film forming: coating the ion balance material to form a film, and baking to obtain the ion balance layer.
[0053] According to a method for preparing an ion balance layer for an electrochromic device according to a specific embodiment of the present invention, a vanadium-containing compound is first formed into a sol dispersion, the sol dispersion is conveniently mixed with an aqueous acrylic emulsion or an aqueous polyurethane emulsion to form an ion balance layer slurry, and the slurry is coated to form a uniform ion balance layer. Optionally, the ion balance material is coated on an ITO (indium tin oxide) film.
[0054] According to some embodiments of the present invention, the vanadium-containing compound includes at least one of vanadium pentoxide, vanadium sulfate, ammonium vanadate and ammonium metavanadate. Here, the valence state of vanadium in the hydrated vanadium oxide precursor solution is a mixture of 4+ and 5+. It is convenient for the formation of sol. In this way, the source of vanadium-containing compounds is wide, cheap and easy to obtain, which is convenient for the promotion and use of the preparation method of the ion balance layer for electrochromic devices of the present invention.
[0055] According to some embodiments of the present invention, the precursor of the organic auxiliary agent includes at least one of methyl methacrylate, methyl acrylate, styrene, acrylonitrile, hydroxypropyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, itaconic acid, acrylamide, polyethylene glycol methacrylate, polymethyl methacrylate, polydioxolane, polymethyl methacrylate, polyethyl methacrylate, and isobornyl methacrylate. In this way, the precursor of the organic auxiliary agent is prepolymerized and polycondensed to obtain an aqueous acrylic emulsion.
[0056] According to other embodiments of the present invention, the precursor of the organic auxiliary agent includes at least one of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate and polyether polyol, polyether diol, polyethylene glycol, polytetramethylene ether, 1,4-butanediol, polyethylene adipate glycol, polyoxypropylene ether diol, polytetramethylene ether glycol and polyester polyol. In this way, the precursor of the organic auxiliary agent is prepolymerized and polycondensed to obtain an aqueous polyurethane emulsion.
[0057] According to an embodiment of the third aspect of the present invention, the present invention provides an electrochromic device, comprising: an electrochromic layer, an ion conduction layer, an ion balance layer and a transparent conductive film stacked in sequence, wherein the ion balance layer is attached to the transparent conductive film, and the ion balance layer is the ion balance layer according to the embodiment of the first aspect of the present invention, or the ion balance layer prepared by the preparation method according to the embodiment of the second aspect of the present invention.
[0058] According to the electrochromic device of the specific embodiment of the present invention, the electrochromic ion balance performance of the ion balance layer is excellent. The intrinsic color of vanadium oxide has little effect on the color changing performance of the device, which is conducive to the color changing material of the device to exert a high saturation color changing effect. Here, the transparent conductive film can be an ITO (indium tin oxide) film.
[0059] According to some embodiments of the present invention, the adhesion between the ion balance layer and the transparent conductive film is F, and F satisfies: F ≥ 4 B. In this way, the adhesion between the ion balance layer and the transparent conductive film is large, and the formed ion balance layer structure for the electrochromic device is reliable.
[0060] According to some other embodiments of the present invention, after standing at room temperature of 25° C. for 48 hours, the adhesion F between the ion balance layer and the transparent conductive film satisfies: F ≥ 4B. That is, after being placed at room temperature for a long time, the adhesion between the ion balance layer and the transparent conductive film remains substantially unchanged. This ensures that the ion balance layer has storage stability.
[0061] According to some embodiments of the present invention, the electrochromic layer includes at least one of viologen and its derivatives, polythiophene, polypyrrole, polyaniline and its derivatives, tungsten oxide, nickel oxide and vanadium oxide. In this way, the electrochromic layer has a wide range of color-changing raw materials and has a variety of colors.
[0062] According to some embodiments of the present invention, the ion conducting layer includes: at least one of PEO, PVDF, PMMA and PANI systems. In the PEO, PVDF, PMMA and PANI systems, at least one of PEO, PVDF, PMMA and PANI and their derivatives as a network framework, organic small molecules (propylene carbonate, ethylene carbonate, acetonitrile, vinyl ethylene carbonate, vinylene carbonate, N,N-dimethylformamide, dimethyl carbonate, methyl ethyl carbonate, butanediol, propylene glycol, dimethyl propanediol, hexadecene and diols), lithium salts (1-butyl-3-methylimidazolium lithium hexafluorophosphate, 1-butyl-3-methylimidazolium bis (trifluoromethylsulfonyl) imide lithium, 1-butyl-3-methylimidazolium lithium toluenesulfonate, 1 -ethyl-2,3-dimethylimidazole lithium hexafluorophosphate, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, bisfluorosulfonyl imide lithium salt, lithium tetrafluoroborate and lithium perchlorate) and an initiator (at least one of 2-hydroxy-2-methyl-1-phenylacetone, 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and ethyl 2,4,6-trimethylbenzoylphenylphosphonate) among which PEO (polyethylene, oxidized), PVDF (polyvinylidene difluoride), PMMA (polymethyl methacrylate) and PANI (polyaniline (emeraldine base)).
[0063] According to an embodiment of the fifth aspect of the present invention, the present invention provides an application of an electrochromic device according to an embodiment of the fourth aspect of the present invention, wherein the electrochromic device is used in electronic and electrical components, automobile windows, rearview mirrors, and architectural glass windows. Here, the automobile windows may include skylights.
[0064] The electrochromic device according to the specific embodiment of the present invention has a wide range of applications. When the electrochromic device is used in electronic and electrical components, it can be used in the back cover of a mobile phone, AR glasses, etc.
[0065] The ion balance layer for an electrochromic device of the present invention is further described below through specific exemplary embodiments and comparative examples and performance tests of the obtained ion balance layer for an electrochromic device.
[0066] Example 1
[0067] The first step is to prepare a hydrated amorphous vanadium pentoxide sol, dissolve 5g of vanadyl sulfate in 50g of a 30% hydrogen peroxide solution, control the temperature to 0°C, and react for 240 minutes; continue to add 50g of a 30% hydrogen peroxide solution, continue to keep the solution system temperature at 0°C, and react for 60 minutes to obtain a vanadium oxide sol precursor dispersion, and dilute the above-obtained dispersion 10 times with a mixture of deionized water and ethanol for later use;
[0068] In the second step, an organic auxiliary agent with a COC bond as the main network is prepared, and a polymerization reaction is carried out in a 500mL four-necked flask equipped with a thermometer, mechanical stirring, a condenser and a nitrogen protection device. The polyester polyol is heated at 110°C and maintained under vacuum conditions for 2 hours to remove moisture from the polyester polyol, and then cooled to 75°C, and a measured amount of isophorone diisocyanate is added, and the temperature is raised to about 90°C for reaction for 3 hours, and then cooled to 80°C, and an appropriate amount of acetone solvent, chain extender 1,4-butanediol and catalyst are added, and the temperature is raised to about 70°C for reaction for 5 hours. During the reaction, an appropriate amount of acetone is added according to the viscosity of the reaction system to adjust the viscosity of the prepolymer. Finally, the prepolymer is transferred to an emulsification barrel, cooled to 40°C, and deionized water is added to emulsify at a speed of 2000rmp for shearing. After the emulsion is formed, a 10wt% ethylenediamine aqueous solution is slowly added, and the speed is maintained at 3000rmp for 30 minutes to obtain a polyurethane acrylic emulsion. The solvent acetone in the emulsion is removed by reduced pressure distillation, and the solid content of the emulsion is controlled at 45wt%, and a stable additive can be obtained.
[0069] The third step is mixing. Take 80 μL of organic polymer stabilizer and add it to 50 mL of diluted vanadium sol precursor dispersion. Continue stirring at 500 rpm for 30 min to obtain a stable ion balance layer slurry. After film formation and curing, the molecular additive content is about 0.25wt%;
[0070] The fourth step is film formation. The obtained ion balance material is coated on the conductive substrate ITO using a small slit coater and dried in an oven to obtain a stable ion balance layer membrane. The effective thickness of the ion balance layer is 50nm.
[0071] The fifth step is to characterize the performance, testing the stability of color difference, adhesion, diffusion coefficient, and color change performance of the device.
[0072] Example 2
[0073] The difference from Example 1 is as follows: 240 μL of organic polymer stabilizing agent is added to 50 mL of diluted vanadium sol precursor dispersion, and stirring is continued at 500 rpm for 30 min to obtain a stable ion balance layer slurry. After film formation and curing, the molecular agent content is about 0.75 wt%.
[0074] Example 3
[0075] The difference from Example 1 is as follows: 480 μL of organic polymer stabilizing agent is added to 50 mL of diluted vanadium sol precursor dispersion, and stirring is continued at 500 rpm for 30 min to obtain a stable ion balance layer slurry. After film formation and curing, the molecular agent content is about 1.5 wt%.
[0076] Example 4
[0077] The difference from Example 1 is as follows: 640 μL of organic polymer stabilizing agent is added to 50 mL of diluted vanadium sol precursor dispersion, and stirring is continued at 500 rpm for 30 min to obtain a stable ion balance layer slurry. After film formation and curing, the molecular agent content is about 2 wt%.
[0078] Example 5
[0079] The first step is to prepare a vanadium oxide sol precursor solution, which is the same as Example 1.
[0080] The second step is to prepare the acrylic acid system polymer additive. Methyl methacrylate, ethyl acrylate, hydroxyethyl acrylate, emulsifier nonylphenol polyoxyethylene ether, and water are added to the pre-emulsification reactor, emulsified for 30 minutes, and then an appropriate amount of water and buffer sodium bicarbonate are added. The temperature is raised to 75°C, and then an initiator is added to react for 30 minutes. The temperature is then raised to 90°C and reacted for 120 minutes. The temperature is naturally lowered to 50°C, and the pH is adjusted to between 6 and 7 to obtain a polymer stabilizing additive for the acrylic emulsion system, and finally an emulsion with a solid content of 45wt% is obtained.
[0081] The third step is mixing. Take 80 μL of organic polymer stabilizing agent and add it to 50 mL of diluted vanadium sol precursor dispersion. Continue stirring at 500 rpm for 30 min to obtain a stable ion balance layer slurry. After film formation and curing, the molecular additive content is about 0.25 wt%.
[0082] The fourth step is film formation. The obtained ion balance material is coated on the conductive substrate ITO using a small slit coater and then dried in an oven to obtain a stable ion balance layer membrane. The effective thickness of the ion balance layer is 50nm.
[0083] Example 6
[0084] The difference from Example 5 is as follows: 480 μL of organic polymer stabilizing agent is added to 50 mL of diluted vanadium sol precursor dispersion, and stirring is continued at 500 rpm for 30 min to obtain a stable ion balance layer slurry. After film formation and curing, the molecular agent content is about 1.5 wt%.
[0085] Comparative Example 1
[0086] The first step: preparing a vanadium oxide sol precursor solution, the same as in Example 1.
[0087] Step 2: Preparation of silicone emulsion. First, PPG1000 and DMPA were vacuum dried at 110℃ for 3h to remove moisture. PPG10000 and IPDI were added to a three-necked flask and stirred evenly. After heating, DMPA and PEG1000 were added to react, and then a catalyst was added to continue the reaction. After cooling, silane was added dropwise, and finally deionized water was added for emulsification. Acetone, butanone and other solvents were removed in vacuum. A silicone emulsion with a solid content of about 45% was prepared using silane: polyurethane = 3:1.
[0088] Step 3: Take 480 μL of organic polymer stabilizing agent and add it to 50 mL of diluted vanadium sol precursor dispersion, and continue stirring at 500 rpm for 30 min to obtain a stable ion balance layer slurry with a molecular additive content of about 1.5wt%.
[0089] Comparative Example 2
[0090] The first step: preparing a vanadium oxide sol precursor solution, the same as in Example 1.
[0091] Step 2: Dissolve PVDF in NMP solvent and prepare a 10wt% solution to serve as a polymer additive without ether bonds.
[0092] Step 3: Add an appropriate amount of organic polymer stabilizing agent to 50 mL of the diluted vanadium sol precursor dispersion, and continue stirring at 500 rpm for 30 minutes to obtain a stable ion balance layer slurry. After film formation and curing, the molecular additive content is about 1.5wt%.
[0093] Comparative Example 3
[0094] The difference from Example 1 is as follows: 1600 μL of organic polymer stabilizing agent is added to 50 mL of the diluted vanadium sol precursor dispersion, and stirring is continued at 500 rpm for 30 min to obtain a stable ion balance layer slurry, and the molecular agent content is about 5 wt%.
[0095] Comparative Example 4
[0096] The difference from Example 1 is as follows: no polymer stabilizing agent is added, and the vanadium sol precursor dispersion is directly used for coating to prepare an ion balance layer with a thickness of 50 nm.
[0097] Comparative Example 5
[0098] The difference from Example 7 is as follows: no polymer stabilizing agent is added, and the vanadium sol precursor dispersion is directly used for coating, followed by heat treatment to remove water molecules in the hydrated vanadium oxide and prepare an ion balance layer with a thickness of 50 nm.
[0099] Comparative Example 6
[0100] The difference from Example 1 is as follows: vanadium pentoxide is prepared by PVD coating with a thickness of 50 nm.
[0101] Comparative Example 7
[0102] The difference from Example 1 is as follows: commercial anhydrous vanadium pentoxide powder is used as the vanadium source to prepare the slurry. Because commercial powder is difficult to ball-mill into powder below 50 nm, we finally use the polymer additive in Example 3 to coat and prepare the vanadium pentoxide ion balance layer with a thickness of about 200 nm.
[0103] Surface roughness testing
[0104] The surface roughness of the ion storage layer was tested using an atomic force microscope. The test area was 50 μm*50 μm, and the parameter Ra data was recorded.
[0105] Adhesion test
[0106] The prepared ion balance layer membrane was directly exposed to room temperature (temperature 25℃±2, humidity 40-80%), left to stand for 48 hours, and its adhesion was tested using a hundred-grid tester.
[0107] Ion diffusion rate test
[0108] The ion diffusion rate was calculated using an electrochemical workstation (biologic SP200) and the GITT test method with reference to the following formula.
[0109] ;
[0110] Where: r is the radius of the positive and negative active material particles; t is the duration of the pulse current; ΔEs is the change in equilibrium voltage during the current pulse; ΔEt is the total voltage change after subtracting the ohmic voltage drop during the current pulse.
[0111] Color change performance test
[0112] In order to ensure the consistency of the test conditions, in this experimental test, the color-changing layer uses PEDOT:PSS with the same properties as the color-changing material, uses in-situ cross-linked 1PC:1PEGDA:0.2M LiTFSI as the ion conduction layer, and the ion balance layer is prepared by the method in the embodiment. The effective color-changing area size of the device is 100*100 mm. The optical fiber spectrometer and electrochemical workstation are used to test the time required for the color fading of the center point of the device. The color-fading voltages are set to 1.2 V and 1.0 V respectively, and the color-fading time is 20 s. The color-changing time and cycle life are tested.
[0113] Test items Roughness Ra (nm) Room temperature adhesion <![CDATA[Ionic diffusivity (cm 2 / s)]]> Coloring time(s) Fading time(s) Cycle life Example 1 18 4B <![CDATA[2.4X10 -11 ]]> 6.2 4.9 9W Example 2 15 4B <![CDATA[6.1X10 -11 ]]> 5.8 4.4 10.1w Example 3 13 5B <![CDATA[1.7X10 -10 ]]> 3.1 2.9 13w Example 4 9 5B <![CDATA[3.4X10 -11 ]]> 4.8 4.7 12w Example 5 17 4B <![CDATA[4.1X10 -11 ]]> 7.1 6.9 8.5W Example 6 11 5B <![CDATA[6.7X10 -11 ]]> 4.4 .7 7.8W Comparative Example 1 13 3B <![CDATA[3.1X10 -13 ]]> 12.4 11.7 5.6W Comparative Example 2 12 4B <![CDATA[1.2X10 -15 ]]> 15.1 13.3 0.3W Comparative Example 3 8 5B <![CDATA[1.1X10 -13 ]]> 12.1 13.8 5.1W Comparative Example 4 24 3B <![CDATA[1.8X10 -12 ]]> 7.4 7.7 6.2W Comparative Example 5 29 3B <![CDATA[9.1X10 -13 ]]> 8.3 7.9 4.6W Comparative Example 6 32 4B <![CDATA[5.3X10 -12 ]]> 8.5 7.2 4.7W Comparative Example 7 51 4B <![CDATA[1.2X10 -13 ]]> 9.2 8.1 3.1W
[0114] Test Results
[0115] Examples 1-6 are examples of the present invention, used to illustrate the performance of the ion balance layer for electrochromic devices of the present invention. Comparative Examples 1-7 are used to illustrate the impact of different material proportions or preparation methods from the present invention on the technical solution.
[0116] Comprehensive evaluation and analysis show that the roughness of the polyurethane emulsion system is relatively low, among which the roughness in Example 3 can reach 13, and the conductivity and cycle life are optimal.
[0117] By comparing the test results of Examples 1-4, it can be seen that within the range of 0.5%-2%, as the additive content increases, the roughness of the ion balance layer gradually decreases; the ion diffusion rate of the ion balance layer is best at 1.5wt%. When the additive content is lower than 1.5% and greater than or equal to 0.5%, it may be due to the relatively small additive content that the conductive interface formed is insufficient, causing the ion diffusion rate to decrease, but it is also better than the ion diffusion rate of the ion balance layer of the comparative example; when the additive content is higher than 1.5% and less than or equal to 2%, the additive content may be relatively high, resulting in too much organic component and a decrease in the balance capacity, but it is also better than the ion diffusion rate of the ion balance layer of the comparative example.
[0118] As shown in Comparative Example 3, when the content reaches 5wt%, the cycle life is significantly reduced, so the polyurethane emulsion system is optimal at 1.5wt%.
[0119] Although acrylic emulsion can improve the discoloration time and cycle life of the device as shown in Examples 5 and 6, it is inferior to that of polyurethane emulsion. The main reason may be that polyurethane emulsion, in addition to containing ether bonds to lithium, has more CN bonds interacting with vanadium oxygen polyhedrons, resulting in better cycle stability, with a maximum cycle number of up to 13W times.
[0120] For Comparative Examples 1 and 2, as the ether bond content decreases, the conductivity decreases significantly, and even hinders the ion transmission characteristics. The ion diffusion rate is lower than that of Comparative Examples 4 and 5, so the polymer additive needs to contain a certain proportion of ether bonds. In addition, the vanadium pentoxide ion balance layer obtained by PVD and commercial powder has a poor cycle life. This may be mainly due to the fact that there are no water molecules in the vanadium molecular structure of PVD and commercial powder, and its crystal structure is unstable. As the number of cycles increases, its irreversible embedded ions increase, which ultimately leads to a relatively poor device life.
[0121] Therefore, in summary, the solution in Example 4 is the best solution, and Examples 1-3 and 5-6 are better solutions.
[0122] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0123] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. An ion balance layer for an electrochromic device, characterized in that: In terms of mass percentage, it includes: 98% to 99.9% of hydrated vanadium pentoxide and 0.1% to 2% of an organic additive with a COC bond as the main network. When the voltage is 1.0V to 3.5V, the migration rate of active ions in the ion balance layer is v, wherein v satisfies: v>1x10 -11 cm 2 / s, The charge per unit area in the ion balance layer is C, wherein C satisfies: C>8mC / cm 2 .
2. The ion balance layer for an electrochromic device according to claim 1, characterized in that: When the voltage is 1.0V to 3.5V, the migration rate of active ions in the ion balance layer is v, wherein v satisfies: 2x10 -10 cm 2 / s≥v>1x10 -11 cm 2 / s, The charge per unit area in the ion balance layer is C, where C satisfies: 10 mC / cm 2 ≥C>8mC / cm 2 .
3. The ion balance layer for an electrochromic device according to claim 1, characterized in that: The molecular formula of the hydrated vanadium pentoxide is V2O5·xH2O, wherein x satisfies: 2.5≥x>0.
1.
4. The ion balance layer for an electrochromic device according to claim 1, characterized in that: The organic auxiliary agent is an organic polymer mixture containing a large number of chain ether bonds.
5. The ion balance layer for an electrochromic device according to claim 4, characterized in that: The organic polymer mixture includes water-based acrylic emulsion and / or water-based polyurethane emulsion.
6. The ion balance layer for an electrochromic device according to claim 1, characterized in that: The roughness of the surface of the ion balance layer is Ra, wherein the Ra satisfies: Ra≤20nm.
7. The ion balance layer for an electrochromic device according to claim 1, characterized in that: The thickness of the ion balance layer is d1, wherein d1 satisfies: 30nm≤d1≤90nm.
8. The method for preparing an ion balance layer for an electrochromic device according to any one of claims 1 to 7, characterized in that: The steps include: Preparation of hydrated vanadium pentoxide sol: dissolving a vanadium-containing compound in a hydrogen peroxide solution, reacting to obtain a sol containing hydrated vanadium pentoxide, and diluting to obtain a sol dispersion for later use; An organic auxiliary agent with a COC bond as the main network is prepared, and the precursors of the organic auxiliary agent are mixed, prepolymerized, and emulsified to obtain the organic auxiliary agent with a COC bond as the main network, wherein the organic auxiliary agent with a COC bond as the main network is an aqueous acrylic emulsion or an aqueous polyurethane emulsion; Mixing, adding the organic additive to the sol dispersion, reacting to obtain an ion balance layer slurry; Film formation: coating the ion balance layer slurry to form a film, and baking to obtain the ion balance layer.
9. The preparation method according to claim 8, characterized in that: The vanadium-containing compound includes at least one of vanadium pentoxide, vanadyl sulfate, ammonium vanadate and ammonium metavanadate.
10. The preparation method according to claim 8, characterized in that: The precursor of the organic auxiliary agent includes at least one of methyl methacrylate, methyl acrylate, styrene, acrylonitrile, hydroxypropyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, itaconic acid, acrylamide, polyethylene glycol methacrylate, polymethyl methacrylate, polydioxolane, polyethyl methacrylate, and isobornyl methacrylate; Or at least one of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate and polyether polyol, polyether diol, polyethylene glycol, polytetramethylene ether, 1,4-butanediol, polyethylene adipate, polyoxypropylene ether diol, polytetramethylene ether glycol and polyester polyol.
11. An electrochromic device, characterized in that: include: The electrochromic layer, ion conduction layer, ion balance layer and transparent conductive film are stacked in sequence. Wherein, the ion balance layer is attached to the transparent conductive film, and the ion balance layer is the ion balance layer according to any one of claims 1-7, or the ion balance layer prepared by the preparation method according to any one of claims 8-10.
12. The electrochromic device according to claim 11, characterized in that: The adhesion force between the ion balance layer and the transparent conductive film is F, and F satisfies: F≥4B.
13. The electrochromic device according to claim 11 or 12, characterized in that: The electrochromic layer includes at least one of viologen and its derivatives, polythiophene, polypyrrole, polyaniline and its derivatives, tungsten oxide, nickel oxide and vanadium oxide.
14. The electrochromic device according to claim 11 or 12, characterized in that: The ion conducting layer comprises at least one of PEO, PVDF, PMMA and PANI systems.
15. Use of an electrochromic device according to any one of claims 11 to 14, characterized in that: The electrochromic device is used for electronic and electrical components, automobile windows, rearview mirrors and architectural glass windows.
Citation Information
Patent Citations
High-performance nano granular vanadium pentoxide lithium ion battery cathode material and preparation method thereof
CN103022457A
Vanadium oxide having VOX molecular formula for use as charge balancing material for electrochromic devices
CN114901596A
V2O5-based electrochromic material, preparation method thereof and electrochromic device
CN116514168A
VANADIUM OXIDE WITH A FORMULA OF VOx AS CHARGE BALANCING MATERIAL FOR ELECTROCHROMIC DEVICES
US20220066276A1