A method for mass production of pultrusion root bolt sleeve assembly for wind turbine blades
Through the pultrusion mass production preparation method, the problem of bonding strength and quality consistency of the bolt sleeve assembly at the root of the wind turbine blade has been solved, higher load strength and finished product quality have been achieved, and the problems of cavities and cracking in traditional methods have been avoided.
Patent Information
- Application Number
- CN202410892534.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-04
AI Technical Summary
In the traditional manufacturing method of wind turbine blade root bolt sleeve components, the bonding force between components is weak, which is prone to cracking and damage caused by cavity defects and stress concentration, and it is difficult to guarantee quality consistency.
The pultrusion mass production preparation method is adopted, including metal bolt sleeve pretreatment, mandrel production, fiber and fabric threading layout, dipping, preforming, heating and curing, cutting, beveling and milling. Through sandblasting, PET core Material connection, stud bolt series connection, resin glass transition temperature control and follow-up tooling positioning ensure uniform distribution and precise molding of fibers and fabrics.
It improves the bonding and load strength of the bolt sleeve assembly, reduces the production time, improves the quality of the finished product, avoids cracking damage of the pultruded wedge, and ensures the consistency and load-bearing capacity of the product.
Smart Images

Figure CN118404836B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material pultrusion molding, and in particular to a pultrusion mass production preparation method for a root bolt sleeve assembly for a wind turbine blade. Background Art
[0002] In the wind power industry, the root bolt sleeve assembly is one of the important components for connecting the blade and the hub. Its traditional manufacturing method is to use vacuum infusion process to form, and then lay each component one by one in the female mold during or before the blade production, and then use vacuum infusion process to solidify and form. Its components include: bolt sleeve, plug, sealing ring, core material, pultruded composite wedge, and related fiber yarns and multi-axial fabrics.
[0003] When the root bolt sleeve assembly is prepared by the traditional vacuum infusion process, the components are assembled during preparation, and it is difficult to ensure the consistency of the gaps and spacing between them. Therefore, the bonding force between the components is relatively weak, and it is very easy to form defects such as cavities, which further reduce the bonding force. In addition, when using yarn to fill the gaps between components, it is completely dependent on visual inspection and experience, and quality consistency is difficult to ensure. When the composite pultruded wedge between the bolt sleeves is solidified at the root assembly, the wedge body will also crack and break due to the instability of the operation due to the concentration of curing stress. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for mass production of pultrusion of root bolt sleeve assemblies for wind turbine blades, which effectively solves the problems in the background technology.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is: a method for mass production of a root bolt sleeve assembly for a wind turbine blade by pultrusion, comprising the following steps:
[0006] Step 1: Pretreatment of the metal bolt sleeve: First, sandblast the outer surface of the metal bolt sleeve, and then use a plug with a sealing ring to seal one end of the inner hole of the metal bolt sleeve;
[0007] Step 2: Mandrel production: Select two pre-treated metal bolt sleeves, and connect the ends with plugs to the two ends of the PET core material to form a mandrel;
[0008] Step 3: Start pultrusion: Use fibers and multi-axial fabrics to thread yarns on the mandrel, and connect two metal bolt sleeves between the mandrels through stud bolts to achieve series connection of multiple mandrels;
[0009] Step 4: Dipping in glue: Under the action of traction, the fibers and fabrics around the serially connected mandrels are dipped in glue;
[0010] Step 5, preforming: according to the center line of the preforming mold, the center line of the mandrel is positioned by using the mandrel holding follower tooling, so that it can smoothly enter the preforming tooling and the mold, and complete the preforming process together with the fibers and fabrics soaked with resin around it, and obtain a semi-finished product of the bolt sleeve assembly;
[0011] Step 6: Heating and curing: The semi-finished product of the bolt sleeve assembly is heated and cured through a pultrusion curing die to obtain a finished product of the bolt sleeve assembly;
[0012] Step 7, cutting: cutting the multiple sets of bolt sleeve assembly finished products after curing at the position of the stud bolts to obtain a single set of bolt sleeve assembly finished products;
[0013] Step 8: Bevel cutting: Bevel cutting the PET core material area of the finished single bolt sleeve assembly according to the drawing requirements to obtain two independent bolt sleeve assemblies with the same external dimensions;
[0014] Step 9: Milling of the bolt sleeve end: Milling of the solidified FRP composite material at the bolt sleeve end in the bolt sleeve assembly;
[0015] Step 10. Check and package: After milling, clean the dust from the bolt sleeve and remove the remaining bolts cut from the outer port. Use an endoscope or a go / no-go gauge to check whether there is resin glue on the inner thread of the bolt sleeve. If the inspection is qualified, it can be packaged.
[0016] Furthermore, in step 2, one end of the bolt sleeve with the plug is connected to the PET core material by a combination of mortise and tenon structure, latch structure, threaded structure or adhesive connection.
[0017] Furthermore, in step three, the pultrusion speed of the multiple sets of mandrels connected in series is 8-15 cm / min.
[0018] Furthermore, the pultrusion speed of the multiple sets of mandrels is 10-12 cm / min.
[0019] Furthermore, in step 4, the glass transition temperature Tg of the resin used for dipping is controlled between 95°C and 110°C.
[0020] Furthermore, in step five, when positioning the center line of a set of mandrels, the mandrel holding follower tooling moves to a release point at the entrance of the preforming mold, releases the clamping of the mandrel, and continues to support and position the center line of the next set of mandrels.
[0021] Furthermore, the mandrel holding follower tooling includes a guide rail bracket and at least two brackets arranged on the guide rail bracket;
[0022] The guide rail bracket is arranged at the entrance of the preforming mold or at the preforming bracket. The lower ends of the two brackets are installed with sliders or pulleys, and the upper ends of the brackets clamp the core shaft and move synchronously with the core shaft on the slide rail. By adjusting the height of the two brackets, the center line of the core shaft and the center line of the mold are always kept coincident.
[0023] Furthermore, the two brackets position the two metal bolt sleeves at both ends of the core shaft.
[0024] Furthermore, in step six, a first heating zone, a second heating zone and a third heating zone are provided in the pultrusion curing mold along the pultrusion direction, and the heating temperatures corresponding to the first heating zone, the second heating zone and the third heating zone are 100-120°C, 125-155°C and 125-145°C respectively.
[0025] Furthermore, the distance between the fiberglass reinforced plastic composite material and the end face of the bolt sleeve is 5 mm ± 0.5 mm.
[0026] The beneficial effects of the present invention are as follows: the present invention prefabricates the root bolt assembly through the pultrusion process, thereby reducing the time for installing and laying the bolt sleeve components during blade root production and improving work efficiency; the stress concentration and cavity defect problems caused by uneven fiber distribution are solved through precise distribution and control of fibers and fabrics; and the use of pultruded wedges is eliminated through the one-piece molding of the bolt sleeve, core material and yarn / fabric, thereby effectively improving the bonding of the components in the bolt sleeve assembly and effectively improving the bearing capacity of the blade root bolt assembly.
[0027] Compared with the traditional preparation process, continuous pultrusion is achieved, which greatly improves the finished product quality of the root bolt sleeve, effectively improves the load strength of the root bolt, and effectively solves the cracking damage problem of the traditional root wedge caused by uneven force. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 It is a schematic flow chart of a method for mass production of pultrusion of root bolt sleeve assemblies for wind turbine blades according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0031] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0033] like Figure 1 The method for mass production of the root bolt sleeve assembly for wind turbine blades by pultrusion comprises the following steps:
[0034] Step 1: Pretreatment of the metal bolt sleeve: First, sandblast the outer surface of the metal bolt sleeve, and then use a plug with a sealing ring to seal one end of the inner hole of the metal bolt sleeve; sandblasting increases the roughness of the metal surface and improves the bonding strength between the resin and the metal, and the setting of the plug ensures that the resin does not enter the inner thread of the screw sleeve during the pultrusion process;
[0035] Step 2: Mandrel production: Select two pre-treated metal bolt sleeves, and connect the ends with plugs to the two ends of the PET core material to form a mandrel;
[0036] In order to adapt to different working environments, in step 2, one end of the bolt sleeve with the plug and the PET core material adopt a combination of mortise and tenon structure, latch structure, thread structure or adhesive connection. Different connection methods can be selected according to material characteristics, mechanical properties and environmental conditions.
[0037] The pre-treated metal bolt sleeve is connected to the PET core material to form a mandrel for pultrusion, and the addition of the PET core material can improve the strength and stability of the final product.
[0038] Step 3: Start pultrusion: Use fibers and multi-axial fabrics to thread yarns on the mandrel, and connect two metal bolt sleeves between the mandrels through stud bolts to achieve series connection of multiple mandrels;
[0039] In step three, multiple sets of mandrels are connected in series through stud bolts, so that the pultrusion production of multiple bolt sleeve assemblies can be completed simultaneously, and the pultrusion speed of the multiple sets of mandrels after series connection is further controlled to be 8-15cm / min. Preferably, the pultrusion speed of the multiple sets of mandrels is 10-12cm / min, which helps the resin to penetrate evenly into the fibers and fabrics to form a uniform composite material structure.
[0040] The fibers and multi-axial fabrics are threaded and laid out as required to form a multi-layer fiber and fabric structure on each mandrel. Multiple mandrels are connected in series through stud bolts to ensure the stability of the mandrels, achieve mass production, and improve production efficiency.
[0041] Step 4: Dipping: Under the action of traction, the fibers and fabrics around the serially connected mandrels are dipped in resin to allow the resin to fully penetrate and evenly cover the multi-layer fiber and fabric structure to form a uniform composite material structure.
[0042] The core material of the root bolt sleeve assembly in the present invention has poor temperature resistance and is prone to heat charring or deformation. Therefore, the dipping resin uses a resin that starts the reaction at medium to low temperatures and has low curing heat release. In step four, the glass transition temperature Tg of the resin used for dipping is controlled between 95°C and 110°C. The core material part uses a relatively high temperature-resistant PET core material (temperature resistant 150-200°C) to replace the traditional non-heat-resistant PVC core material (temperature resistant 80°C). This temperature range is lower than the temperature resistance range of the PET core material, ensuring that the resin will not cause thermal damage to the PET core material during the curing process.
[0043] Step 5, preforming: according to the center line of the preforming mold, the center line of the mandrel is positioned by using the mandrel holding follower tooling, so that it can smoothly enter the preforming tooling and the mold, and complete the preforming process together with the fibers and fabrics soaked with resin around it, and obtain a semi-finished product of the bolt sleeve assembly;
[0044] In step five, when positioning the center line of one set of mandrels, the mandrel holding follower tooling moves to the release point at the entrance of the preforming mold, releases the clamping of the mandrel, and continues to support and position the center line of the next set of mandrels.
[0045] In the present invention, the position of the tooling 30 cm away from the preforming mold is set as the release point, and the mandrels are connected by studs. The tooling moves synchronously with the pultruded mandrel to locate the center line of the mandrel. When it moves to the release point close to the preforming mold, that is, when the tooling is 30 cm away from the preforming mold, the clamping of the mandrel is released. Since the mandrel and the tooling move at the same speed, when the mandrel is released, the mandrel continues to pultrude, and the tooling will not stop immediately, but will gradually slow down and continue to move forward to a distance within 30 cm, and move in the opposite direction to the next group of mandrels after stopping, locate their center lines, and repeat this step to locate the center line of the mandrel that is about to enter the preforming mold to ensure that the mandrel enters the mold at a suitable speed.
[0046] The fluctuation problem of the center line of the mandrel is solved or controlled by the mandrel holding follower tooling. Preferably, the mandrel holding follower tooling includes a guide rail bracket and at least two brackets arranged on the guide rail bracket; the guide rail bracket is arranged at the entrance of the preforming mold or the preforming bracket, and the lower ends of the two brackets are installed with sliders or pulleys, and the upper ends of the brackets clamp the mandrel and move synchronously with the mandrel on the slide rail, and by adjusting the height of the two brackets, the center line of the mandrel and the center line of the mold are always kept coincident.
[0047] Specifically, the tooling design allows the adjustment of at least two brackets, providing flexibility to accommodate mandrels of different lengths or diameters. A slider or pulley is installed at the lower end of the bracket, which helps to move smoothly on the guide rail and reduce vibration and friction. The upper end of the bracket clamps the mandrel and can move synchronously with the mandrel on the guide rail to ensure the stability of the mandrel during the pultrusion process; and by adjusting the height of the bracket, it can ensure that the center line of the mandrel is consistent with the center line of the mold, thereby achieving precise positioning.
[0048] In order to control the forming of fibers and fabrics during the pultrusion process, during the threading layout of fibers and multi-axial fabrics, the end faces formed by the fibers and multi-axial fabrics will reserve a distance from the end face of the mandrel. Therefore, before entering the preforming mold, two brackets are used to position the two metal bolt sleeves at both ends of the mandrel. The metal bolt sleeves may provide a larger contact area and a more stable support point, which is conducive to precise positioning.
[0049] Step 6: Heating and curing: The semi-finished product of the bolt sleeve assembly is heated and cured through a pultrusion curing die to obtain a finished product of the bolt sleeve assembly;
[0050] Combined with the material characteristics requirements (PET core material has a temperature resistance of 150-200°C, and the core material will soften and deform if it exceeds or is exposed to this temperature for a long time), in step six, the pultrusion curing mold is provided with a first heating area, a second heating area, and a third heating area along the pultrusion direction, and the corresponding heating temperatures of the first heating area, the second heating area, and the third heating area are 100-120°C, 125-155°C, and 125-145°C, respectively. The lower temperature of the first heating area helps the resin flow and impregnation in the fiber without curing immediately. The temperature of the highest heating area is controlled within the temperature resistance range of the PET core material to prevent the core material from softening or deforming due to overheating. The temperature settings of different heating areas can control the curing rate of the resin to ensure that the resin is fully cured without damaging the PET core material.
[0051] Step 7: Cutting: Cut the solidified multiple sets of bolt sleeve assemblies at the position of the stud bolts to obtain a single set of bolt sleeve assemblies; pay attention to avoid damaging the bolt sleeves; facilitate subsequent processing and packaging, while maintaining the integrity of the product.
[0052] Step 8. Bevel cutting: According to the requirements of the drawing, bevel the PET core area of the finished single bolt sleeve assembly to obtain two independent bolt sleeve assemblies with the same external dimensions; bevel cutting can provide a specific installation angle to meet specific application requirements.
[0053] Step 9: Milling of the bolt sleeve end: Milling of the solidified FRP composite at the bolt sleeve end in the bolt sleeve assembly; preferably, the distance between the FRP composite and the bolt sleeve end face is 5 mm ± 0.5 mm, so that a 5 mm length area at the bolt sleeve end is not covered by the FRP composite, which can provide a more accurate positioning point and facilitate positioning during application.
[0054] Step 10. Check and package: After milling, clean the dust from the bolt sleeve and remove the remaining bolts cut from the outer port. Use an endoscope or a go / no-go gauge to check whether there is resin glue on the inner thread of the bolt sleeve. If the inspection is qualified, it can be packaged.
[0055] The present invention prefabricates the root bolt assembly through the pultrusion process, thereby reducing the time for installing and laying the bolt sleeve components when manufacturing the root of the blade and improving work efficiency; the stress concentration and cavity defect problems caused by uneven distribution of fibers are solved through precise distribution and control of fibers and fabrics; and the use of pultruded wedges is eliminated through the integrated molding of the bolt sleeve, core material and yarn / fabric, thereby effectively improving the bonding of the components in the bolt sleeve assembly and the bearing capacity of the blade root bolt assembly.
[0056] Compared with the traditional preparation process, the finished product quality of the root bolt sleeve is greatly improved, the load strength of the root bolt is effectively improved, and at the same time, the cracking damage problem of the traditional root wedge caused by uneven force is effectively solved.
[0057] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for mass production of pultrusion root bolt sleeve components for wind turbine blades. It is characterized in that The following steps are involved: Step 1: Pretreatment of the metal bolt sleeve: First, sandblast the outer surface of the metal bolt sleeve, and then use a plug with a sealing ring to seal one end of the inner hole of the metal bolt sleeve; Step 2: Mandrel production: Select two pre-treated metal bolt sleeves, and connect the ends with plugs to the two ends of the PET core material to form a mandrel; Step 3: Start pultrusion: Fibers and multi-axial fabrics are used to thread yarns on the mandrel. During the threading process, a distance is reserved between the end face formed by the fiber and multi-axial fabric and the end face of the mandrel, and two metal bolt sleeves are connected between the mandrels through stud bolts to realize the series connection of multiple sets of mandrels. Step 4: Dipping: Under the action of traction, the fibers and fabrics around the serially connected mandrels are dipped in glue; the glass transition temperature Tg of the resin used for dipping is controlled between 95°C and 110°C; Step 5, preforming: according to the center line of the preforming mold, the center line of the mandrel is positioned by using the mandrel holding follower tooling, so that it can smoothly enter the preforming tooling and the mold, and complete the preforming process together with the fibers and fabrics soaked with resin around it, and obtain a semi-finished product of the bolt sleeve assembly; In step 5, when positioning the center line of a set of mandrels, the mandrel holding follower tooling moves to the release point at the entrance of the preforming mold, releases the clamping of the mandrel, and continues to support and position the center line of the next set of mandrels; The mandrel holding follower tooling includes a guide rail bracket and two brackets arranged on the guide rail bracket; the guide rail bracket is arranged at the entrance of the preforming mold, and the lower ends of the two brackets are equipped with sliders or pulleys, and the upper ends of the brackets clamp the mandrel, follow the mandrel to move synchronously on the slide rail, and by adjusting the heights of the two brackets, the center line of the mandrel and the center line of the mold are always kept coincident; before entering the preforming mold, the two metal bolt sleeves at both ends of the mandrel are positioned by using the two brackets; Step 6: Heating and curing: The semi-finished product of the bolt sleeve assembly is heated and cured through a pultrusion curing die to obtain a finished product of the bolt sleeve assembly; Step 7, cutting: cutting the multiple sets of bolt sleeve assembly finished products after curing at the position of the stud bolts to obtain a single set of bolt sleeve assembly finished products; Step 8: Bevel cutting: Bevel cutting the PET core material area of the finished single bolt sleeve assembly according to the drawing requirements to obtain two independent bolt sleeve assemblies with the same external dimensions; Step 9: Milling of the bolt sleeve end: Milling of the solidified FRP composite material at the bolt sleeve end in the bolt sleeve assembly; Step 10. Check and package: After milling, clean the dust from the bolt sleeve and remove the remaining bolts cut from the outer port. Use an endoscope or a go / no-go gauge to check whether there is resin glue on the inner thread of the bolt sleeve. If the inspection is qualified, it can be packaged.
2. The method for mass production of pultrusion of root bolt sleeve assembly for wind turbine blades according to claim 1, It is characterized in that In step 2, one end of the metal bolt sleeve with a plug is connected to the PET core material by a combination of mortise and tenon structure, latch structure, threaded structure or adhesive connection.
3. The method for mass production of pultrusion of root bolt sleeve assembly for wind turbine blades according to claim 1, It is characterized in that In step three, the pultrusion speed of the multiple sets of mandrels connected in series is 8-15 cm / min.
4. The method for mass production of pultrusion of root bolt sleeve components for wind turbine blades according to claim 3, It is characterized in that The pultrusion speed of multiple sets of mandrels is 10-12cm / min.
5. The method for mass production of pultrusion of root bolt sleeve assembly for wind turbine blades according to claim 1, It is characterized in that In step six, a first heating zone, a second heating zone and a third heating zone are provided in the pultrusion curing mold along the pultrusion direction, and the heating temperatures corresponding to the first heating zone, the second heating zone and the third heating zone are 100-120°C, 125-155°C and 125-145°C respectively.
6. The method for mass production of pultrusion of root bolt sleeve components for wind turbine blades according to claim 1, It is characterized in that The distance between the fiberglass composite material and the end face of the bolt sleeve is 5mm±0.5mm.
Citation Information
Patent Citations
Method for manufacturing embedded bolt sleeve at root of fan blade by pultrusion process
CN103909662A
Adjustable core rod connecting device
CN108085732A
Insert for a wind turbine blade root
CN111684155A
Embedded threaded sleeve assembly, forming method and blade root embedded connecting structure
CN118008678A
Glass fiber pultrusion grid continuous production line moving core mould circulation mechanism
CN205148950U