Double perovskite nano-phosphor for enhancing near-infrared emission, preparation method thereof and preparation method of LED device
By doping Yb and Sb in double perovskite, using quantum tailoring of Tb-Yb and modification of Sb, the problem of low near-infrared quantum yield of double perovskite is solved, and nano-fluorescence with high-efficiency near-infrared emission is achieved. The preparation of powder and the application of LED devices provide a non-toxic, highly stable and efficient solution.
Patent Information
- Application Number
- CN202410527831.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-29
AI Technical Summary
The existing double perovskites have low near-infrared quantum yield, which limits their further development in many fields.
Using Cs2NaTbCl6 as the matrix material, doped with Yb and Sb, using quantum tailoring of Tb-Yb and Sb modification of the material to enhance the near-infrared emission effect, nano-phosphors with high near-infrared quantum yield were prepared and applied in LED devices.
It significantly improves the near-infrared emission intensity and quantum yield, avoids the toxicity and self-absorption problems of lead-based perovskite, and provides non-toxic, highly stable nanophosphors suitable for the preparation of LED devices.
Smart Images

Figure CN118406495B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to near-infrared luminescent nano fluorescent powder, a preparation method thereof and application in the LED field, belonging to the technical field of luminescent materials. Background Art
[0002] Near-infrared light sources (NIR) have great development potential in many fields such as food, security, biology and medicine. Research on efficient near-infrared fluorescent materials has become a hot topic. In the past few decades, people have made extensive efforts to develop multifunctional near-infrared inorganic phosphors or luminescent materials based on transition metal ions or rare earth ions. However, most of these phosphors are micron-sized powders, and their low absorption coefficient, low photoluminescence quantum yield (PLQY) and toxicity have hindered their further application. For example, lead-based perovskites have the advantages of easy manufacture, high absorption coefficient and high PLQY, but the toxicity and instability of lead and the strong self-absorption of the material itself have greatly limited its further development in many fields.
[0003] The use of monovalent and trivalent cations instead of Pb 2+ The formed non-toxic nanoscale double perovskite has very weak self-absorption, good stability and is non-toxic, and is regarded as a light-emitting material with great potential. However, due to the nature of parity-forbidden transitions, the near-infrared emission of double perovskites is weak. Summary of the invention
[0004] The present invention aims to solve the technical problem of low near-infrared quantum yield of the existing double perovskite and provide a double perovskite nano-phosphor for enhancing near-infrared emission, a preparation method thereof and a preparation method of an LED device.
[0005] The chemical formula of the double perovskite nano-phosphor for enhancing near-infrared emission of the present invention is Cs2NaTbCl6:x%Yb,y%Sb, wherein 0<x≤15, 0<y≤15. The double perovskite nano-phosphor for enhancing near-infrared emission of the present invention uses Cs2NaTbCl6 as a matrix material, rare earth ion Tb as a lattice component element of the double perovskite, and provides an emission center and an intermediate state energy level for energy transfer at the same time, Yb and Sb are doped in the matrix, and the effect of enhancing near-infrared emission is achieved by utilizing quantum tailoring between Tb-Yb and effective modification of the material by Sb, and can emit near-infrared signals under ultraviolet excitation, and is a nano-phosphor with a high near-infrared quantum yield.
[0006] Furthermore, the chemical formula of the double perovskite nano-phosphor for enhancing near-infrared emission is Cs2NaTbCl6:x%Yb,y%Sb, where 0<x≤15, 1≤y≤5. The emission intensity of the phosphor in the near-infrared is relatively high.
[0007] The preparation method of the above-mentioned double perovskite nano-phosphor for enhancing near-infrared emission is carried out according to the following steps:
[0008] Step 1: weigh a cesium source, a sodium source, a terbium source, an antimony source, and a ytterbium source according to the chemical formula Cs2NaTbCl6:x%Yb,y%Sb, wherein 0<x≤15, 0<y≤15 in a stoichiometric ratio; then weigh a trimethylchlorosilane liquid, wherein the amount of trimethylchlorosilane is 2% to 5% higher than the stoichiometric ratio of the chlorine element in the chemical formula;
[0009] Step 2: adding a cesium source, a sodium source, a terbium source, an antimony source and an ytterbium source into a reaction vessel, and then adding oleic acid, oleylamine and octadecene, stirring and heating the reaction vessel under a vacuum state, raising the temperature to 100-130° C. and maintaining it for 50-70 minutes so that the added raw materials are dissolved in the organic solution, and then introducing argon gas and raising the temperature to 160-200° C. and maintaining it for 10-15 minutes;
[0010] Step 3: inject trimethylchlorosilane into the reaction vessel after the operation in step 2 is completed, and after the injection is completed, keep the temperature at 160-200° C. for 1-8 minutes, and cool the system to room temperature to obtain a crude product;
[0011] Step 4: Centrifuge the crude product to obtain double perovskite nano-phosphor with enhanced near-infrared emission.
[0012] Furthermore, in step 2, the amount of oleic acid added is 1 mmol: (7-10) mL in terms of the volume ratio of the amount of the cesium source to the volume of the oleic acid.
[0013] Furthermore, in step 2, the amount of oleylamine added is 1 mmol: (1.5-2.5) mL in terms of the ratio of the amount of the cesium source to the volume of oleylamine.
[0014] Furthermore, in step 2, the amount of octadecene added is 1 mmol: (25-35) mL in terms of the ratio of the amount of the cesium source to the volume of octadecene.
[0015] Furthermore, the centrifugal separation described in step 4 is specifically performed as follows: first, the crude product is centrifuged at 6000 rpm for 5 minutes, and the precipitate is retained; cyclohexane is added to the precipitate for dispersion, and the mixture is centrifuged at 7000 rpm for 5 minutes, and the supernatant is retained; ethyl acetate is added to the supernatant, and the mixture is centrifuged at 7000 rpm for 10 minutes, and the solid phase is retained; the solid phase is dispersed in cyclohexane and centrifuged at 7000 rpm for 5 minutes, and the precipitate is removed to obtain the final product.
[0016] Furthermore, the cesium source in step 1 is one or a combination of cesium acetate, cesium carbonate, cesium nitrate and cesium sulfate.
[0017] Furthermore, the sodium source in step 1 is one or a combination of sodium acetate, sodium carbonate, sodium nitrate and sodium sulfate.
[0018] Furthermore, the terbium source in step 1 is one or a combination of terbium acetate, terbium carbonate, terbium nitrate and terbium sulfate.
[0019] Furthermore, the antimony source in step 1 is one or a combination of antimony acetate, antimony carbonate, antimony nitrate and antimony sulfate.
[0020] Furthermore, the ytterbium source in step 1 is one or a combination of ytterbium acetate, ytterbium carbonate, ytterbium nitrate and ytterbium sulfate.
[0021] The method for preparing an LED device using the above-mentioned double perovskite nano-phosphor for enhancing near-infrared emission is carried out in the following steps:
[0022] Step 1: Adding double perovskite nano-phosphor with enhanced near-infrared emission and polystyrene into a container, and then adding toluene and ultrasonically mixing until completely dissolved to obtain a colloid;
[0023] Step 2: Load the colloid onto a commercial 340nm UV chip, let it stand and dry, and obtain an LED device.
[0024] Furthermore, the mass ratio of the double perovskite nano-phosphor for enhancing near-infrared emission, polystyrene, and toluene is 1:5:10.
[0025] The double perovskite nano-phosphor Cs2NaTbCl6: x% Sb, y% Yb with enhanced near-infrared emission of the present invention constructs a new energy transfer pathway, utilizes the quantum tailoring process of Tb-Yb to achieve a significant enhancement of the quantum yield, and produces characteristic emissions of Tb and Yb respectively under ultraviolet light excitation, with a total quantum yield of up to 155%, which can be excited by a commercial 340nm chip to produce efficient visible-near-infrared emission.
[0026] The double perovskite nano-phosphor with enhanced near-infrared emission Cs2NaTbCl6: x% Sb, y% Yb of the present invention uses Tb as the main lattice component element, effectively avoiding the lattice and energy level mismatch problem caused by rare earth ion doping, and uses Tb as the main component element of the matrix, which increases the sensitizer concentration in the quantum tailoring process and avoids the problem of weak emission caused by low sensitizer concentration. At the same time, the double perovskite nano-phosphor with enhanced near-infrared emission Cs2NaTbCl6: x% Sb, y% Yb of the present invention has an energy transfer process from the matrix to Tb, avoiding the problem of insufficient absorption caused by the narrow rare earth ion absorption cross section.
[0027] The near-infrared emission-enhanced double perovskite nano-phosphor Cs2NaTbCl6: x% Sb, y% Yb of the present invention has the advantages of small size, potential for preparing flexible films, and the advantages of non-toxicity and high stability compared to traditional lead-based perovskites. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the X-ray diffraction pattern of the Cs2NaTbCl6 double perovskite nano-phosphor obtained in Comparative Example 1.
[0029] Figure 2 This is a transmission electron microscope photograph of the Cs2NaTbCl6 double perovskite nanophosphor obtained in Comparative Example 1.
[0030] Figure 3 This is the emission spectrum of the Cs2NaTbCl6 double perovskite nano-phosphor obtained in Example 1 in the visible band under ultraviolet 280nm excitation at room temperature.
[0031] Figure 4 This is the UV-visible absorption spectrum of Cs2NaTbCl6:2%Sb prepared in Comparative Example 2.
[0032] Figure 5 This is the XRD spectrum of the Cs2NaTbCl6:2%Sb,2%Yb double perovskite nano-phosphor obtained in Example 1.
[0033] Figure 6 This is a transmission electron microscope image of the Cs2NaTbCl6:2%Sb,2%Yb double perovskite nano-phosphor obtained in Example 1.
[0034] Figure 7 This is the emission spectrum of the Cs2NaTbCl6:2%Sb,2%Yb double perovskite nano-phosphor obtained in Example 1 in the visible band under 280nm excitation.
[0035] Figure 8 This is the emission spectrum of the Cs2NaTbCl6:2%Sb,2%Yb double perovskite nano-phosphor obtained in Example 1 in the near-infrared band under 280nm excitation.
[0036] Fig. 9 It is an emission spectrum diagram of Cs2NaTbCl6:2% Sb, 2% Yb obtained in Example 1 and Cs2NaTbCl6:6% Sb, 2% Yb obtained in Example 2 in the visible band under 280nm excitation.
[0037] Fig.10Near-infrared emission spectra of Cs2NaTbCl6:2% Sb, 2% Yb obtained in Example 1 and Cs2NaTbCl6:6% Sb, 2% Yb obtained in Example 2 under 280nm excitation.
[0038] Fig.11 This is a photo of an LED device loaded with the Cs2NaTbCl6:2%Sb,2%Yb double perovskite nano-phosphor of Example 1 and a commercial 340nm LED chip.
[0039] Fig.12 This is a spectrum diagram of an LED device prepared using the Cs2NaTbCl6:2%Sb,2%Yb double perovskite nano-phosphor powder of Example 1 and a commercial 340nm LED chip.
[0040] Fig.13 This is a quantum yield diagram of the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 1: Cs2NaTbCl6: 2% Sb, 2% Yb. DETAILED DESCRIPTION
[0041] Example 1: The preparation method of the double perovskite nano-phosphor with enhanced near-infrared emission in this example is carried out according to the following steps:
[0042] Step 1: Weigh 0.1062 g of cesium acetate, 0.0263 g of sodium acetate, 0.1075 g of terbium acetate, 0.0018 g of antimony acetate, 0.0027 g of ytterbium acetate and 0.26 mL of trimethylsilyl chloride according to the chemical formula Cs2NaTbCl6:2%Sb,2%Yb;
[0043] Step 2: Add cesium acetate, sodium acetate, terbium acetate, antimony acetate, and ytterbium acetate into a three-necked flask, and then add 2.5 mL of oleic acid, 0.66 mL of oleylamine, and 10 mL of octadecene, and then evacuate the three-necked flask to a vacuum degree of 0.098 MPa, stir and heat, raise the temperature to 110° C. and maintain for 60 minutes, so that the added raw materials are dissolved in the organic solution, and then introduce argon gas and raise the temperature to 180° C. and maintain for 10 minutes;
[0044] Step 3: inject trimethylchlorosilane into the reaction vessel in which the operation in step 2 is completed, maintain the temperature at 180° C. for 3 minutes, and then cool the system to room temperature within one minute to obtain a crude product;
[0045] Step 4: First, centrifuge the crude product at 6000rpm for 5 minutes and retain the precipitate; add 8mL of cyclohexane to disperse it, and then centrifuge the mixture at 7000rpm for 5 minutes, and retain the supernatant; then add 12mL of ethyl acetate to the supernatant, and centrifuge it at 7000rpm for 10 minutes to retain the solid phase; then disperse the solid phase in 8mL of cyclohexane and centrifuge it at 7000rpm for 5 minutes to remove the precipitate to obtain the double perovskite nanophosphor Cs2NaTbCl6: 2% Sb, 2% Yb with enhanced near-infrared emission.
[0046] Example 2: The preparation method of the double perovskite nano-phosphor with enhanced near-infrared emission of this example is carried out according to the following steps:
[0047] Step 1: weigh 0.1062 g of cesium acetate, 0.0263 g of sodium acetate, 0.1075 g of terbium acetate, 0.0054 g of antimony acetate, 0.0027 g of ytterbium acetate and 0.26 mL of trimethylsilyl chloride according to the chemical formula Cs2NaTbCl6:6%Sb,2%Yb;
[0048] Step 2: Add cesium acetate, sodium acetate, terbium acetate, antimony acetate, and ytterbium acetate into a three-necked flask, and then add 2.5 mL of oleic acid, 0.66 mL of oleylamine, and 10 mL of octadecene, and then evacuate the three-necked flask to a vacuum degree of 0.098 MPa, stir and heat, raise the temperature to 110° C. and maintain for 60 minutes, so that the added raw materials are dissolved in the organic solution, and then introduce argon gas and raise the temperature to 180° C. and maintain for 10 minutes;
[0049] Step 3: inject trimethylchlorosilane into the reaction vessel in which the operation in step 2 is completed, maintain the temperature at 180° C. for 3 minutes, and then cool the system to room temperature within one minute to obtain a crude product;
[0050] Step 4: First, centrifuge the crude product at 6000rpm for 5 minutes and retain the precipitate; add 8mL of cyclohexane to disperse it, and then centrifuge the mixture at 7000rpm for 5 minutes, and retain the supernatant; then add 12mL of ethyl acetate to the supernatant, and centrifuge it at 7000rpm for 10 minutes to retain the solid phase; then disperse the solid phase in 8mL of cyclohexane and centrifuge it at 7000rpm for 5 minutes to remove the precipitate to obtain a double perovskite nanophosphor Cs2NaTbCl6: 6% Sb, 2% Yb with enhanced near-infrared emission.
[0051] Comparative Example 1: In this comparative example, double perovskite nano-phosphor Cs2NaTbCl6 is prepared, and the specific steps are as follows:
[0052] Step 1: Weigh 0.1062 g of cesium acetate, 0.0263 g of sodium acetate, 0.1075 g of terbium acetate and 0.26 mL of trimethylsilyl chloride according to the stoichiometric ratio of the chemical formula Cs2NaTbCl6;
[0053] Step 2: Add cesium acetate, sodium acetate and terbium acetate into a three-necked flask, then add 2.5 mL of oleic acid, 0.66 mL of oleylamine and 10 mL of octadecene, evacuate the three-necked flask to a vacuum degree of 0.098 MPa, stir and heat, raise the temperature to 110° C. and maintain for 60 minutes so that the added raw materials are dissolved in the organic solution, then introduce argon gas and raise the temperature to 180° C. and maintain for 10 minutes;
[0054] Step 3: inject trimethylchlorosilane into the reaction vessel in which the operation in step 2 is completed, maintain the temperature at 180° C. for 3 minutes, and then cool the system to room temperature within one minute to obtain a crude product;
[0055] Step 4: First, centrifuge the crude product at 6000rpm for 5 minutes and retain the precipitate; add 8mL of cyclohexane to disperse it, and then centrifuge the mixture at 7000rpm for 5 minutes, and retain the supernatant; then add 12mL of ethyl acetate to the supernatant, and centrifuge it at 7000rpm for 10 minutes to retain the solid phase; then disperse the solid phase in 8mL of cyclohexane and centrifuge it at 7000rpm for 5 minutes to remove the precipitate to obtain the double perovskite nanophosphor Cs2NaTbCl6.
[0056] Comparative Example 2: In this comparative example, double perovskite nano-phosphor Cs2NaTbCl6:2%Sb is prepared, and the specific steps are as follows:
[0057] Step 1: Weigh 0.1062 g of cesium acetate, 0.0263 g of sodium acetate, 0.1075 g of terbium acetate, 0.0018 g of antimony acetate and 0.26 mL of trimethylsilyl chloride according to the stoichiometric ratio of the chemical formula Cs2NaTbCl6;
[0058] Step 2: Add cesium acetate, sodium acetate and terbium acetate into a three-necked flask, then add 2.5 mL of oleic acid, 0.66 mL of oleylamine and 10 mL of octadecene, evacuate the three-necked flask to a vacuum degree of 0.098 MPa, stir and heat, raise the temperature to 110° C. and maintain for 60 minutes so that the added raw materials are dissolved in the organic solution, then introduce argon gas and raise the temperature to 180° C. and maintain for 10 minutes;
[0059] Step 3: inject trimethylchlorosilane into the reaction vessel in which the operation in step 2 is completed, keep it for 3 minutes after the injection is completed, and cool the system to room temperature within one minute to obtain a crude product;
[0060] Step 4: First, centrifuge the crude product at 6000rpm for 5 minutes and retain the precipitate; add 8mL of cyclohexane to disperse it, and then centrifuge the mixture at 7000rpm for 5 minutes, and retain the supernatant; then add 12mL of ethyl acetate to the supernatant, and centrifuge it at 7000rpm for 10 minutes to retain the solid phase; then disperse the solid phase in 8mL of cyclohexane and centrifuge it at 7000rpm for 5 minutes to remove the precipitate to obtain the double perovskite nanophosphor Cs2NaTbCl6:2%Sb.
[0061] Figure 1 This is the XRD spectrum of Cs2NaTbCl6 prepared by the improved hot injection method in Example 1. From this figure, it can be seen that the prepared Cs2NaTbCl6 corresponds to the standard diffraction peak and has a cubic phase structure.
[0062] Figure 2 This is a transmission electron microscope picture of Cs2NaTbCl6 prepared in Comparative Example 1. From this picture, it can be seen that the prepared Cs2NaTbCl6 has a cubic phase structure and a size of 20nm.
[0063] Figure 3 The emission spectrum of Cs2NaTbCl6 prepared in Comparative Example 1 shows that the prepared Cs2NaTbCl6 only contains Tb in the visible light band without any doped ions. 3+ Feature emission.
[0064] Figure 4 The absorption spectrum of Cs2NaTbCl6:2%Sb prepared in Comparative Example 2 shows that the prepared Cs2NaTbCl6 has a high absorption rate when doped with Sb. 3+ In the case of an additional absorption band, this means that Sb 3+ The introduction of adds an energy transfer process sensitized by Sb to the material, further increasing the material's absorption of ultraviolet light.
[0065] Figure 5 This is the XRD spectrum of the double perovskite nano-phosphor with enhanced near-infrared emission Cs2NaTbCl6: 2% Sb, 2% Yb prepared in Example 1. From the figure, it can be seen that the prepared Cs2NaTbCl6: 2% Sb, 2% Yb still has the same structure as Cs2NaTbCl6 after doping, proving that doping does not change the crystal structure of the material.
[0066] Figure 6 This is a transmission electron microscope image of the double perovskite nano-phosphor with enhanced near-infrared emission Cs2NaTbCl6:2% Sb, 2% Yb prepared in Example 1. From this figure, it can be seen that the prepared Cs2NaTbCl6:2% Sb, 2% Yb still has a size similar to that of Cs2NaTbCl6 after doping.
[0067] Figure 7 This is the visible band emission spectrum of the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 1: 2% Sb, 2% Yb. 3+ and Yb 3+ The material still has Tb 3+ characteristic emission.
[0068] Figure 8 This is the near-infrared emission spectrum of the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 1: 2% Sb, 2% Yb. 3+ The doping introduces near-infrared emission into the material.
[0069] Fig. 9 The visible band emission spectra of the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 1: 2% Sb, 2% Yb and the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 2: 6% Sb, 2% Yb. 3+ Tb does not change the material 3+ characteristic emission peak position, but the higher Sb 3+ The content will quench Tb 3+ characteristic emission.
[0070] Fig.10 The near-infrared emission spectra of the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 1: 2% Sb, 2% Yb and the double perovskite nano-phosphor with enhanced near-infrared emission prepared in Example 2: 6% Sb, 2% Yb. 3+ Will not change the material 3+ characteristic emission peak position, but the higher Sb 3+ The content will quench Yb 3+ characteristic emission.
[0071] The LED device is prepared using the double perovskite nano-phosphor powder Cs2NaTbCl6: 2% Sb, 2% Yb with enhanced near-infrared emission prepared in Example 1 as a light conversion material. The specific process is as follows:
[0072] Step 1: Weigh 0.01 g of the double perovskite nano-phosphor Cs2NaTbCl6: 2% Sb, 2% Yb prepared in Example 1 and 0.1 g of polystyrene and add them into a 20 ml sample bottle, then add 2 mL of toluene and sonicate for 1 h, at which time the solid matter is completely dissolved to obtain a colloid;
[0073] Step 2: Apply the colloid evenly on the surface of a commercial 340nm UV chip (6mm in diameter and 2mm in thickness), and after drying for 4 hours, obtain an LED device.
[0074] Fig.11 This is a photo of an LED device made of the double perovskite nano-phosphor Cs2NaTbCl6:2% Sb, 2% Yb with enhanced near-infrared emission prepared in Example 1 as a light conversion material. Fig.11 It can be seen that the prepared LED device emits bright green light.
[0075] Fig.12 The light spectrum of the LED device prepared by using the double perovskite nano-phosphor Cs2NaTbCl6:2% Sb, 2% Yb with enhanced near-infrared emission prepared in Example 1 as the light conversion material is shown in FIG. Fig. 9 It can be seen that under the excitation of the 340nm LED chip, the LED device emits Tb 3+ and Yb 3+ Corresponding characteristic emission peaks in the visible and near-infrared bands.
[0076] Fig.13 This is the quantum yield of the double perovskite nano-phosphor Cs2NaTbCl6: 2% Sb, 2% Yb with enhanced near-infrared emission prepared in Example 1. As can be seen from the figure, its quantum yield is significantly enhanced, and the total quantum yield can reach 155%.
[0077] In Example 1, luminescent centers are introduced by doping ions to achieve effective luminescence enhancement. Rare earth ions Tb and Yb have radiation energy levels with emission ranges covering deep ultraviolet to mid-infrared and unique luminescence characteristics. The quantum tailoring process that exists in them improves the quantum yield. At the same time, the high absorption coefficient of Sb-doped double perovskite materials can improve the problem of weak emission intensity caused by the narrow absorption cross section of rare earth ions. Through synergistic effects, the double perovskite nano-phosphor with enhanced near-infrared emission has efficient near-infrared emission.
Claims
1. A double perovskite nano-phosphor with enhanced near-infrared emission, characterized in that The chemical formula of the nano fluorescent powder is Cs2NaTbCl6:x%Yb,y%Sb, wherein 0<x≤2, 0<y≤6.
2. A method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission, characterized in that The method proceeds as follows: Step 1: weigh a cesium source, a sodium source, a terbium source, an antimony source, and a ytterbium source according to the chemical formula Cs2NaTbCl6:x%Yb,y%Sb, wherein 0<x≤2, 0<y≤6 in a stoichiometric ratio; then weigh a trimethylchlorosilane liquid, wherein the amount of trimethylchlorosilane is 2% to 5% higher than the stoichiometric ratio of the chlorine element in the chemical formula; Step 2: adding a cesium source, a sodium source, a terbium source, an antimony source and an ytterbium source into a reaction vessel, and then adding oleic acid, oleylamine and octadecene, stirring and heating the reaction vessel under a vacuum state, raising the temperature to 100-130° C. and maintaining it for 50-70 minutes so that the added raw materials are dissolved in the organic solution, and then introducing argon gas and raising the temperature to 160-200° C. and maintaining it for 10-15 minutes; Step 3: inject trimethylchlorosilane into the reaction vessel after the operation in step 2 is completed, and after the injection is completed, keep the temperature at 160-200° C. for 1-8 minutes, and cool the system to room temperature to obtain a crude product; Step 4: Centrifuge the crude product to obtain double perovskite nano-phosphor with enhanced near-infrared emission.
3. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2, characterized in that In step 2, the amount of oleic acid added is 1 mmol: (7-10) mL according to the ratio of the amount of the cesium source to the volume of oleic acid.
4. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2 or 3, characterized in that In step 2, the amount of oleylamine added is 1 mmol: (1.5-2.5) mL according to the ratio of the amount of the cesium source to the volume of oleylamine.
5. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2 or 3, characterized in that: In step 2, the amount of octadecene added is 1 mmol: (35-35) mL according to the ratio of the amount of the cesium source to the volume of octadecene.
6. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2 or 3, characterized in that: The specific operation of the centrifugal separation described in step 4 is: first, centrifuge the crude product at 6000 rpm for 5 minutes, and retain the precipitate; add cyclohexane to the precipitate for dispersion, and then centrifuge the mixture at 7000 rpm for 5 minutes, and retain the supernatant; then add ethyl acetate to the supernatant, and centrifuge at 7000 rpm for 10 minutes, and retain the solid phase; then disperse the solid phase in cyclohexane and centrifuge at 7000 rpm for 5 minutes, remove the precipitate, and obtain the final product.
7. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2 or 3, characterized in that: The cesium source described in step one is one or a combination of cesium acetate, cesium carbonate, cesium nitrate and cesium sulfate; the sodium source described in step one is one or a combination of sodium acetate, sodium carbonate, sodium nitrate and sodium sulfate; the terbium source described in step one is one or a combination of terbium acetate, terbium carbonate, terbium nitrate and terbium sulfate.
8. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2 or 3, characterized in that: The antimony source in step 1 is one or a combination of antimony acetate, antimony carbonate, antimony nitrate and antimony sulfate.
9. The method for preparing a double perovskite nano-phosphor with enhanced near-infrared emission according to claim 2 or 3, characterized in that: The ytterbium source described in step 1 is one or a combination of ytterbium acetate, ytterbium carbonate, ytterbium nitrate and ytterbium sulfate.
10. A method for preparing an LED device using the double perovskite nano-phosphor with enhanced near-infrared emission according to claim 1, characterized in that The method proceeds as follows: Step 1: Adding double perovskite nano-phosphor with enhanced near-infrared emission and polystyrene into a container, and then adding toluene and ultrasonically mixing until completely dissolved to obtain a colloid; Step 2: Load the colloid onto a commercial 340nm UV chip, let it stand and dry, and obtain an LED device.