A high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy and a preparation method thereof

By forming the second phase with microalloyed elements and controlling the thermal deformation structure, the 7XXX aluminum alloy has been solved to take into account both the strength, plastic toughness and corrosion resistance of 7XXX aluminum alloy, and its corrosion resistance and toughness properties have been significantly improved.

CN118406937BActive Publication Date: 2024-11-15SUZHOU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410497728.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-11-15
Estimated Expiration
2044-04-24

AI Technical Summary

Technical Problem

While improving strength, the plastic toughness and corrosion resistance of 7XXX series aluminum alloys are difficult to take into account. The existing technology mostly relies on nano-strengthening phase regulation, affecting the alloy strength.

Method used

The second phase is formed by microalloying elements, and the deformed structure is regulated during the thermal deformation process, forming layered heterogeneous structure, improving plastic toughness and reducing corrosion crack propagation capabilities, and improving the corrosion resistance of the alloy.

Benefits of technology

It achieves significant improvement of plastic toughness and corrosion resistance while ensuring the strength of the alloy, and coordinates the strength of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118406937B_ABST
    Figure CN118406937B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of aluminum alloy materials, and specifically relates to a high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy and a preparation method thereof. The high-strength, tough, and corrosion-resistant aluminum alloy material mainly comprises Zn, Mg, and Cu alloy elements, as well as one or more microalloying elements such as Zr, Mn, Cr, Sc, and V. The aluminum alloy comprises one or more second phases after homogenization heat treatment, and the second phase can regulate the alloy deformation structure; the aluminum alloy comprises a nano-strengthening phase after aging heat treatment, which can improve the alloy strength. The aluminum alloy preparation method is based on deformation treatment, and a layered heterogeneous deformation structure is obtained in the alloy, which improves the strength and toughness of the alloy while greatly reducing the corrosion crack propagation ability, thereby improving its corrosion resistance. The 7XXX series aluminum alloy product prepared by the present invention can optimize the contradictory relationship between the strength, toughness, and corrosion resistance of the aluminum alloy, and effectively improve its corrosion resistance while obtaining high strength and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aluminum alloy materials, and in particular relates to a high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy and a preparation method thereof. Background Art

[0002] Lightweight, high-strength 7XXX series aluminum alloys are widely used in aerospace, marine engineering, transportation and other fields. As a typical ultra-high-strength aluminum alloy, the material requirements for 7XXX series aluminum alloys in the past mainly focused on how to improve the strength of the alloy. Therefore, by increasing the content of Zn, Mg, and Cu alloy elements to improve the precipitation strengthening effect, the strength of the alloy can be significantly improved. At the same time, the improvement in strength will lead to a decrease in the plasticity, toughness and corrosion resistance of the alloy.

[0003] During the service process, material products will face complex and harsh external service environments, in which the materials may suffer varying degrees of damage. In this process, in addition to material strength, its plasticity, toughness and corrosion resistance also become extremely critical. Good plasticity, toughness and corrosion resistance can ensure that material products are not prone to sudden failure under service loads or corrosive media. Therefore, while ensuring the strength of the alloy, how to improve the plasticity, toughness and corrosion resistance of 7XXX series aluminum alloys has become a key issue that needs to be solved urgently.

[0004] Chinese invention patent CN116536552A provides an ultra-high strength and corrosion-resistant 7 series Al-Zn-Mg-Cu aluminum alloy and a preparation method thereof. The method reduces the corrosion potential of the alloy, slows down the corrosion rate, and improves its corrosion resistance through the synergistic effect between cold deformation treatment and heat treatment process.

[0005] Chinese invention patent CN116463532A provides a high-strength and corrosion-resistant 7XXX series aluminum alloy sheet for vehicles and a preparation method thereof. The method improves the corrosion resistance and fracture toughness of the alloy by adding rare earth elements to the alloy.

[0006] Similarly, Chinese invention patent CN115768682A also improves a corrosion-resistant, high-strength weldable aluminum alloy for structural applications by microalloying with rare earth elements. Chinese invention patent CN116875862A provides a large-size plate of high-strength, high-toughness, corrosion-resistant aluminum alloy and a manufacturing method thereof. It can be seen that the existing technology mostly regulates the alloy nano-strengthening phase to regulate the corrosion resistance of the alloy, but it usually has a certain degree of influence on the alloy strength. Summary of the invention

[0007] The purpose of the present invention is to overcome the problems of the prior art and provide a high-strength, tough and corrosion-resistant 7XXX series aluminum alloy and a preparation method thereof. The alloy forms a second phase by microalloying elements, and controls the deformation structure to obtain a layered heterogeneous structure during the hot deformation process, thereby improving the plastic toughness of the material while reducing the corrosion crack propagation ability and improving the corrosion resistance of the alloy.

[0008] In order to solve the above-mentioned technical problems, this application provides the following technical solutions:

[0009] The present invention provides a high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy, wherein the alloy components of the high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy include conventional alloying elements and microalloying elements; the conventional alloying elements are selected from Zn, Mg, and Cu, and the microalloying elements are selected from one or more of Zr, Mn, Cr, Sc, and V.

[0010] Preferably, in the high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy, the micro-alloying elements include, by mass percentage: Zr: 0.1-0.2%; Mn: 0.1-0.5%; Cr: 0.1-0.3%; Sc: 0.05-0.2%; V: 0.05-0.2%.

[0011] Preferably, the high-strength, toughness, and corrosion-resistant 7XXX series aluminum alloy is subjected to homogenization heat treatment, and the second phase precipitated from the high-strength, toughness, and corrosion-resistant 7XXX series aluminum alloy after homogenization heat treatment comprises Al3Zr, Al6Mn, Al7Cr, Al3Sc, Al3(Sc,Zr) and Al 21 One or more of V2.

[0012] Preferably, the alloy deformation structure of the high-strength, toughness, and corrosion-resistant 7XXX series aluminum alloy is a layered heterogeneous structure, which improves the strength and toughness of the alloy while reducing the corrosion crack propagation ability and improving the corrosion resistance of the alloy.

[0013] The present invention also provides a method for preparing the above-mentioned high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy, comprising the following steps: obtaining an alloy ingot by semi-continuous casting, and subjecting the alloy ingot to homogenization heat treatment, hot working deformation, solid solution and aging heat treatment to obtain the high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy.

[0014] Preferably, the homogenization heat treatment is carried out at a temperature of 450-475° C. and for a time of 16-30 hours.

[0015] Preferably, the hot working deformation is forging or rolling at a temperature of 350-450°C.

[0016] Preferably, the solution treatment temperature is 450-475°C and the time is 0.5-3h.

[0017] Preferably, the aging heat treatment is artificial aging heat treatment.

[0018] Furthermore, the aging heat treatment is performed at a temperature of 100-130° C. and for a time of 12-30 hours.

[0019] The technical solution of the present invention has the following advantages over the prior art:

[0020] Compared with the prior art, the high-strength, toughness, and corrosion-resistant 7XXX series aluminum alloy and its preparation method provided by the present invention regulate the thermal deformation structure through the second phase introduced by microalloying to obtain a layered heterogeneous structure, which can not only ensure the strength of the alloy, but also synergistically improve the plasticity, toughness and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The deformation structure and corrosion depth diagram of the alloy in Example 1;

[0022] Figure 2 The deformation structure and corrosion depth diagram of the alloy in Example 2;

[0023] Figure 3 The deformation structure and corrosion depth diagram of the alloy in Example 3;

[0024] Figure 4 This is the deformation structure and corrosion depth diagram of the comparative alloy;

[0025] Figure 5 The mechanical properties of the alloys of the comparative examples and embodiments are shown in FIG. DETAILED DESCRIPTION

[0026] In view of the aforementioned contradiction between the strength, plasticity and toughness and corrosion resistance of the existing aluminum alloy materials, the present invention proposes a high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy and a preparation method thereof. The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0027] Example 1

[0028] The alloy composition of this embodiment is Al-6.5Zn-1.8Mg-0.25Cu-0.5Mn-0.15Zr (mass percentage), and the embodiment alloy ingot is produced by semi-continuous casting.

[0029] The alloy ingot is subjected to homogenization heat treatment in a heat treatment furnace at a temperature of 470°C for 24 hours, and then taken out of the furnace and air-cooled.

[0030] The alloy samples after homogenization heat treatment were hot forged at a forging temperature of 420°C and a deformation amount of 70%.

[0031] The forged alloy samples were subjected to solution heat treatment at a temperature of 460°C and a heat treatment time of 1 h.

[0032] Then, the alloy samples after solid solution were subjected to artificial aging heat treatment at a temperature of 120°C and a heat treatment time of 24 h.

[0033] Example 2

[0034] The alloy composition of this embodiment is Al-6.5Zn-1.8Mg-0.25Cu-0.3Cr-0.15Zr (mass percentage), and the embodiment alloy ingot is produced by semi-continuous casting.

[0035] The alloy ingot is subjected to homogenization heat treatment in a heat treatment furnace at a temperature of 470°C for 24 hours, and then taken out of the furnace and air-cooled.

[0036] The alloy samples after homogenization heat treatment were hot forged at a forging temperature of 420°C and a deformation amount of 70%.

[0037] The forged alloy samples were subjected to solution heat treatment at a temperature of 460°C and a heat treatment time of 1 h.

[0038] Then, the alloy samples after solid solution were subjected to artificial aging heat treatment at a temperature of 120°C and a heat treatment time of 24 h.

[0039] Example 3

[0040] The alloy composition of this embodiment is Al-6.5Zn-1.8Mg-0.25Cu-0.5Mn-0.2Cr-0.15Zr (mass percentage), and the embodiment alloy ingot is produced by semi-continuous casting.

[0041] The alloy ingot is subjected to homogenization heat treatment in a heat treatment furnace at a temperature of 470°C for 24 hours, and then taken out of the furnace and air-cooled.

[0042] The alloy samples after homogenization heat treatment were hot forged at a forging temperature of 420°C and a deformation amount of 70%.

[0043] The forged alloy samples were subjected to solution heat treatment at a temperature of 460°C and a heat treatment time of 1 h.

[0044] Then, the alloy samples after solid solution were subjected to artificial aging heat treatment at a temperature of 120°C and a heat treatment time of 24 h.

[0045] Example 4

[0046] The alloy composition of this embodiment is Al-6.5Zn-1.8Mg-0.25Cu-0.5Mn-0.15Zr (mass percentage), which is the same as that of embodiment 1. The embodiment alloy ingot is prepared by semi-continuous casting.

[0047] The alloy ingot was subjected to homogenization heat treatment in a heat treatment furnace at a temperature of 450°C for 16 hours, and then taken out of the furnace and air-cooled.

[0048] The alloy samples after homogenization heat treatment were hot forged at a forging temperature of 350° C. and a deformation amount of 70%.

[0049] The forged alloy samples were subjected to solution heat treatment at a temperature of 450°C and a heat treatment time of 0.5 h.

[0050] Then, the alloy samples after solid solution were subjected to artificial aging heat treatment at a temperature of 100°C and a heat treatment time of 12 h.

[0051] Example 5

[0052] The alloy composition of this embodiment is Al-6.5Zn-1.8Mg-0.25Cu-0.5Mn-0.15Zr (mass percentage), which is the same as that of embodiment 1. The embodiment alloy ingot is prepared by semi-continuous casting.

[0053] The alloy ingot was subjected to homogenization heat treatment in a heat treatment furnace at a temperature of 475°C for 30 hours, and then taken out of the furnace and air-cooled.

[0054] The alloy samples after homogenization heat treatment were hot forged at a forging temperature of 450°C and a deformation amount of 70%.

[0055] The forged alloy samples were subjected to solution heat treatment at a temperature of 475°C and a heat treatment time of 3 h.

[0056] Then, the alloy sample after solid solution was subjected to artificial aging heat treatment at a temperature of 130°C for 30 hours.

[0057] The alloy composition of this embodiment is Al-6.5Zn-1.8Mg-0.25Cu (mass percentage), and the embodiment alloy ingot is produced by semi-continuous casting.

[0058] The alloy ingot is subjected to homogenization heat treatment in a heat treatment furnace at a temperature of 470°C for 24 hours, and then taken out of the furnace and air-cooled.

[0059] The alloy samples after homogenization heat treatment were hot forged at a forging temperature of 420°C and a deformation amount of 70%.

[0060] The forged alloy samples were subjected to solution heat treatment at a temperature of 460°C and a heat treatment time of 1 h.

[0061] Then, the alloy samples after solid solution were subjected to artificial aging heat treatment at a temperature of 120°C and a heat treatment time of 24 h.

[0062] Effect evaluation 1

[0063] The deformation microstructure of the prepared examples 1, 2, 3 and comparative alloy samples was analyzed by EBSD; the exfoliation corrosion test was analyzed according to GB / T22639-2008 standard; and the mechanical properties of the alloy were analyzed by tensile test according to GB / T16865-2013 standard.

[0064] Figure 1 , 2 , 3 are the deformation structures and corrosion depth results of the alloys of Examples 1, 2, and 3 respectively. Figure 4 For comparison of alloy deformation structure and corrosion depth results, Figure 5 The maximum corrosion depth of the alloy in Example 1 is 163.17 μm, the maximum corrosion depth of the alloy in Example 2 is 129.55 μm, the maximum corrosion depth of the alloy in Example 3 is 116.25 μm, and the maximum corrosion depth of the comparative alloy is 285.01 μm. By comparison, it can be found that the high-toughness and corrosion-resistant 7XXX series aluminum alloy and its preparation method proposed in the present invention can significantly improve the corrosion resistance of the alloy. In addition, by Figure 5 It can be seen from the mechanical property test results that the high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy and the preparation method thereof proposed in the present invention also significantly improve the strength and toughness of the alloy.

[0065] The technical contents and technical features of the present invention have been disclosed as above. However, those skilled in the art may still make various substitutions and modifications based on the teachings and disclosures of the present invention without departing from the spirit of the present invention. Therefore, the protection scope of the present invention should not be limited to the contents disclosed in the embodiments, but should include various substitutions and modifications that do not depart from the present invention and are covered by the claims of this patent application.

Claims

1. A high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy, It is characterized in that The alloy composition of the high-strength, tough and corrosion-resistant 7XXX series aluminum alloy comprises conventional alloying elements and micro-alloying elements; the conventional alloying elements are selected from Zn, Mg and Cu, and the micro-alloying elements are selected from Zr, Mn and Cr; The elements in the high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy, by mass percentage, include: Zn: 6.5%; Mg: 1.8%; Cu: 0.25%; Zr: 0.15%; Mn: 0.5%; Cr: 0.2%; the high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy is subjected to homogenization heat treatment, and the second phase precipitated from the high-strength, tough, and corrosion-resistant 7XXX series aluminum alloy after the homogenization heat treatment includes Al 6 Mn、Al 7 Cr and Al 3 Zr; the alloy deformation structure of the high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy is a layered heterogeneous structure; The method for preparing the high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy comprises the following steps: obtaining an alloy ingot by semi-continuous casting, and subjecting the alloy ingot to homogenization heat treatment, hot working deformation, solid solution and aging heat treatment to obtain the high-strength, toughness and corrosion-resistant 7XXX series aluminum alloy; The temperature of the homogenization heat treatment is 470°C and the time is 24 h; the hot working deformation is hot forging, the temperature is 420°C, and the deformation is 70%; the temperature of the solid solution is 460°C and the time is 1 h; the aging heat treatment is artificial aging heat treatment; the temperature of the aging heat treatment is 120°C and the time is 24 h.

Citation Information

Cited By

  • Processing method of wrought aluminum alloy

    CN120443075A

  • Corrosion-resistant 7-series aluminum alloy for 3C products and processing method of corrosion-resistant 7-series aluminum alloy

    CN122503709A