Graphene-reinforced nickel-based alloy materials and their preparation methods, and graphene-reinforced nickel-based alloy reinforcing layers.
By combining modified graphene with nickel-based alloy powder to form CO covalent bonds, the performance deficiencies of graphene-reinforced nickel-based alloy strengthening layers under high-temperature and heavy-load environments are solved, and the hardness and corrosion resistance are improved.
Patent Information
- Application Number
- CN202410502651.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-25
AI Technical Summary
Existing laser-formed graphene-reinforced nickel-based alloy reinforcing layers have poor performance, especially under high temperature, heavy load and corrosive environments. Poor graphene dispersion and poor wettability with the matrix metal result in insufficient hardness and corrosion resistance.
The graphene powder is mixed with modifiers and dispersants and then ultrasonically treated with nickel-based alloy powder, filtered and ground, followed by heat treatment at a set temperature to form CO covalent bonds to improve dispersibility and interfacial bonding. Finally, a graphene-reinforced nickel-based alloy strengthening layer is formed by laser forming.
It improves the interfacial bonding and dispersibility between graphene and nickel-based alloys, forming a dense and uniform reinforced layer with a surface hardness of 43-50 HRC and good corrosion resistance, thus solving the problem of insufficient performance in the existing technology.
Smart Images

Figure CN118417556B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of additive manufacturing technology, and in particular to a graphene-reinforced nickel-based alloy material and its preparation method, and a graphene-reinforced nickel-based alloy reinforcing layer. Background Technology
[0002] The service conditions of critical components in the metallurgical field are complex and demanding, mainly involving strong coupling damage from multiple thermo-mechanical-fluid fields under high temperature, heavy load, strong friction, and multi-cycle service conditions. Traditional single alloy reinforcement layers are gradually failing to meet the repair requirements of critical components, especially for laser-manufactured reinforcement layers in thermal alternating environments, where the requirements for strength and toughness are even more stringent. Laser coaxial powder feeding additive manufacturing utilizes a high-energy-density laser beam to clad a material with specific properties onto the surface of a substrate material, fusing them together to form an alloy cladding layer with completely different composition and properties from the substrate. Currently, this technology is widely used in the repair of metal structures and the improvement of surface properties.
[0003] Nickel-based alloys possess excellent fatigue resistance, high-temperature creep resistance, high-temperature strength, and oxidation corrosion resistance, making them widely used in the surface repair of equipment components. However, their performance, especially their corrosion resistance, is limited in harsher environments, necessitating composites with other materials for improvement. Graphene materials exhibit a variety of excellent physical properties. When combined with metals to form composites, they can effectively transfer loads, induce crack deflection, and enhance the mechanical properties of the material. They can also effectively facilitate carrier propagation and block ion implantation, strengthening the material's functional characteristics. However, current combinations still suffer from poor graphene dispersion and poor wettability with the matrix metal, which negatively impacts the hardness and corrosion resistance of the composite reinforcement layer. Summary of the Invention
[0004] This application provides a graphene-reinforced nickel-based alloy material and its preparation method, as well as a graphene-reinforced nickel-based alloy reinforcing layer, to solve the technical problem of poor performance of existing laser-formed graphene-reinforced nickel-based alloy reinforcing layers.
[0005] In a first aspect, this application provides a method for preparing a graphene-reinforced nickel-based alloy material, the method comprising:
[0006] Graphene powder, modifier, and dispersant are first mixed and first ultrasonically treated to obtain a graphene mixed solution;
[0007] The graphene mixed solution and nickel-based alloy powder are subjected to a second mixing and a second ultrasonic treatment, followed by filtration and grinding to obtain graphene-nickel-based alloy mixed powder.
[0008] The graphene-nickel-based alloy mixed powder is heat-treated to obtain a graphene-reinforced nickel-based alloy material; wherein the boiling point of the modifier has a set difference from the temperature of the heat treatment.
[0009] Optionally, the heat treatment temperature is 200℃~300℃, and the boiling point of the modifier and the heat treatment temperature satisfy the following relationship:
[0010] 50℃≤T2-T1≤150℃
[0011] In the formula, T2 represents the heat treatment temperature, and T1 represents the boiling point of the modifier.
[0012] The temperature of the heat treatment is determined based on the boiling point of the modifier.
[0013] Optionally, the modifier includes one of the following: peroxybenzoic acid, aminodiphenyl ether, or polystyrene sulfonic acid.
[0014] Optionally, if the modifier is peroxybenzoic acid, then the amount of peroxybenzoic acid is 0.1 to 1 g relative to 100 mL of the dispersant;
[0015] If the modifier is aminodiphenyl ether, then the amount of aminodiphenyl ether is 0.5 to 1 g relative to 100 mL of the dispersant;
[0016] If the modifier is polystyrene sulfonic acid, then the amount of polystyrene sulfonic acid is 0.5 to 1 g relative to 100 mL of the dispersant.
[0017] Optionally, the graphene powder has a sheet diameter ≤ 50 μm, and / or,
[0018] The particle size of the nickel-based alloy powder is 50–150 μm.
[0019] Optionally, the process parameters for the first and second ultrasonic treatments include: ultrasonic power of 100-300W and ultrasonic time of 2-3h.
[0020] Optionally, the grinding process parameters include: grinding speed of 200-400 r / min and grinding time of 2-4 h.
[0021] Optionally, the weight ratio of the graphene powder to the nickel-based alloy powder is (0.5-2):(98-99.5).
[0022] Secondly, this application provides a graphene-reinforced nickel-based alloy material, which is prepared by the method described in the first aspect.
[0023] Thirdly, this application provides a graphene-reinforced nickel-based alloy strengthening layer, which is obtained by laser forming of the graphene-reinforced nickel-based alloy material described in the second aspect on the surface of a substrate.
[0024] The technical solutions provided in this application have the following advantages compared with the prior art:
[0025] The method for preparing the graphene-reinforced nickel-based alloy material provided in this application involves modifying the graphene to form covalent bonds such as CO, resulting in better dispersibility in ethanol solution. Simultaneously, the chemical affinity and interfacial bonding with the nickel-based alloy are significantly improved, making it easier to form MOC covalent bonds (M representing the metal element in the nickel-based alloy). This allows for effective interfacial bonding between the graphene sheets and the nickel-based alloy. A predetermined difference between the boiling point of the modifier and the heat treatment temperature is used to remove excess dispersant and modifier, while preventing the oxidized portion of the graphene from being reduced at high temperatures and losing its modifying effect. This graphene-reinforced nickel-based alloy material can be used for laser forming to obtain a graphene-reinforced nickel-based alloy strengthening layer. This strengthening layer has a surface hardness of 43–50 HRC and good corrosion resistance, thus solving the technical problem of poor performance in existing laser-formed graphene-reinforced nickel-based alloy strengthening layers. Attached Figure Description
[0026] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0027] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 A schematic flowchart illustrating a method for preparing a graphene-reinforced nickel-based alloy material, provided in an embodiment of this application;
[0029] Figure 2 This is a SEM image of a graphene-reinforced nickel-based alloy material provided in Embodiment 1 of this application;
[0030] Figure 3 Metallographic diagram of a graphene-reinforced nickel-based alloy strengthening layer provided in Embodiment 1 of this application;
[0031] Figure 4 XRD characterization results of a graphene-reinforced nickel-based alloy strengthening layer provided in Example 2 of this application;
[0032] Figure 5 Tafel curves for a graphene-reinforced nickel-based alloy strengthening layer and a graphene-free nickel-based alloy strengthening layer provided in Embodiment 2 of this application.
[0033] Figure 6 SEM image of a graphene-reinforced nickel-based alloy material provided for Comparative Example 1 of this application. Detailed Implementation
[0034] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0035] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.
[0036] In this application, the terms "comprising," "including," etc., mean "including but not limited to." Relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.
[0037] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0038] Figure 1 A schematic flowchart illustrating a method for preparing a graphene-reinforced nickel-based alloy material, provided in an embodiment of this application;
[0039] Please see Figure 1 This application provides a method for preparing graphene-reinforced nickel-based alloy materials, the method comprising:
[0040] S1. Graphene powder, modifier and dispersant are first mixed and first ultrasonically treated to obtain graphene mixed solution;
[0041] In the embodiments of this application, after modification, graphene forms covalent bonds such as CO. The dispersant can be water, ethanol, etc., with better dispersibility in ethanol solution. Ethanol is non-toxic and volatile, and it easily disperses graphene and the modifier, and can also serve as a subsequent grinding medium.
[0042] In some embodiments, the modifier includes one of the following: peroxybenzoic acid, aminodiphenyl ether, or polystyrene sulfonic acid.
[0043] In some embodiments, if the modifier is peroxybenzoic acid, then the amount of peroxybenzoic acid is 0.1 to 1 g relative to 100 mL of the dispersant;
[0044] If the modifier is aminodiphenyl ether, then the amount of aminodiphenyl ether is 0.5 to 1 g relative to 100 mL of the dispersant;
[0045] If the modifier is polystyrene sulfonic acid, then the amount of polystyrene sulfonic acid is 0.5 to 1 g relative to 100 mL of the dispersant.
[0046] In this embodiment, the aforementioned modifier is selected to facilitate its removal through heat treatment in subsequent processes. The modifier can be selected from one of peroxybenzoic acid, aminodiphenyl ether, or polystyrene sulfonic acid. The dosage of the modifier is determined based on the selected modifier. Different modifiers have different modifying abilities and dispersion effects. The dosage of the modifier directly affects the modification and dispersion effect of the graphene material. If the dosage of the modifier is too low, the amount of CO in the modified graphene will be relatively small, making it prone to agglomeration during powder preparation. If the dosage of the modifier is too high, the removal of the modifier in subsequent heat treatment steps will be incomplete, affecting the performance of the final graphene-reinforced nickel-based alloy material. For example, relative to 100 mL of the above-mentioned dispersant, the peroxybenzoic acid may be 0.1 g, 0.2 g, 0.4 g, 0.6 g, 0.8 g, 1 g, etc.; relative to 100 mL of the above-mentioned dispersant, the aminodiphenyl ether may be 0.5 g, 0.6 g, 0.7 g, 0.8 g, 0.9 g, 1 g, etc.; relative to 100 mL of the above-mentioned dispersant, the polystyrene sulfonic acid may be 0.5 g, 0.6 g, 0.7 g, 0.8 g, 0.9 g, 1 g, etc.
[0047] S2. The graphene mixed solution and nickel-based alloy powder are subjected to a second mixing and a second ultrasonic treatment, followed by filtration and grinding to obtain graphene-nickel-based alloy mixed powder.
[0048] In some embodiments, the graphene powder has a sheet diameter ≤ 50 μm, and / or,
[0049] The particle size of the nickel-based alloy powder is 50–150 μm.
[0050] In this embodiment, the sheet size of the graphene powder is limited. The graphene modification process mainly acts on the C atoms at the edges or defective parts of the sheets. If the sheet size of the graphene powder is too large, the modification effect will inevitably be poor, and the material will be more prone to agglomeration during ball milling. The particle size of the nickel-based alloy is related to the performance of the final reinforced layer. If the particle size is too large, it may lead to uneven melting of particles in the graphene-reinforced nickel-based alloy material, with unmelted particles present; however, if the particle size is too small, the cost will increase. For example, the sheet size of the graphene powder can be 50μm, 48μm, 46μm, 44μm, 42μm, 35μm, 30μm, etc.; the particle size of the nickel-based alloy powder can be 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, etc.
[0051] Furthermore, in the embodiments of this application, the sphericity of the nickel-based alloy is ≥95%, and its main components are as follows (by mass fraction): Cr: 15%–25%, Mo: 10%–20%, W: 0–5%, Fe: 0–1%, Mn: 0–1%, with the remainder being Ni. The selection of this nickel-based alloy composition aims to achieve "good toughness, suitable for repairing large-area wear-resistant and high-temperature-resistant metallurgical components."
[0052] In some embodiments, the process parameters for the first and second ultrasonic treatments include: ultrasonic power of 100-300W and ultrasonic time of 2-3h.
[0053] In this embodiment, the first ultrasonic treatment affects the dispersion of graphene in the ethanol solution, and the second ultrasonic treatment, as a continuation of the first ultrasonic treatment, ensures uniform mixing of the materials. For example, the power of both the first and second ultrasonic treatments can be 200W, 250W, 300W, 350W, 400W, etc.; and the duration of both the first and second ultrasonic treatments can be 2h, 3h, 4h, etc.
[0054] In some embodiments, the grinding process parameters include: a grinding speed of 200-400 r / min and a grinding time of 2-4 h.
[0055] In this embodiment, the grinding process is ball milling. This ball milling process affects the bonding effect between graphene and metal powder. If the milling time is too short or the rotation speed is too slow, the bonding will be insufficient; if the time is too long or the rotation speed is too fast, it may affect the morphology of the graphene and the sphericity of the powder, thus affecting the cladding effect. For example, the milling speed can be 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, etc.; the milling time can be 2 r / min, 3 r / min, 4 r / min, etc. After the ball milling, the diameter of the alloy powder is 50-150 μm, the graphene sheet diameter is 10-20 μm, and the graphene is distributed on the surface of the nickel-based alloy powder without agglomerating.
[0056] S3. The graphene-nickel-based alloy mixed powder is subjected to heat treatment to obtain a graphene-reinforced nickel-based alloy material; wherein the boiling point of the modifier has a set difference from the temperature of the heat treatment.
[0057] In some embodiments, the heat treatment temperature is 200°C to 300°C, and the boiling point of the modifier satisfies the following relationship with the heat treatment temperature:
[0058] 50℃≤T2-T1≤150℃
[0059] In the formula, T2 represents the heat treatment temperature, and T1 represents the boiling point of the modifier.
[0060] In this embodiment, the difference between the boiling point of the modifier and the heat treatment temperature is limited, ensuring that the heat-treated graphene-reinforced nickel-based alloy powder does not contain modifiers or dispersants. The graphene-nickel-based alloy powder is heat-treated under an inert gas atmosphere. A suitable heat treatment temperature effectively removes excess modifiers and dispersants from the powder while maintaining the modified structure. This appropriate temperature ensures the complete removal of modifiers and ethanol, guaranteeing the cladding effect. Simultaneously, excessively high heat treatment temperatures are avoided, as the covalent bonds of CO in the graphene-modified powder may be reduced, leading to agglomeration and affecting coating performance. For example, the difference between T2 and T1 can be 50℃, 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃, 140℃, 150℃, etc.; the temperature of the heat treatment can be 200℃, 210℃, 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, 290℃, 300℃, etc.
[0061] In some embodiments, the weight ratio of the graphene powder to the nickel-based alloy powder is (0.5-2):(98-99.5).
[0062] In this embodiment, the weight ratio of graphene powder to nickel-based alloy powder ensures a balanced performance of the graphene-reinforced nickel-based alloy material, allowing both powders to maximize their respective benefits. An appropriate amount of graphene powder prevents agglomeration; insufficient graphene may lead to a decrease in the performance of the graphene-reinforced nickel-based alloy material. For example, the weight ratio of graphene powder to nickel-based alloy powder is 0.5:99.5, 1:99, 2:98, etc.
[0063] Based on a general inventive concept, this application provides a graphene-reinforced nickel-based alloy material, which is prepared by the method described in the first aspect.
[0064] The graphene-reinforced nickel-based alloy material is realized based on the above-described preparation method of graphene-reinforced nickel-based alloy material. The specific steps of the preparation method of graphene-reinforced nickel-based alloy material can be referred to the above embodiments. Since the graphene-reinforced nickel-based alloy material adopts some or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be elaborated here.
[0065] Based on a general inventive concept, this application provides a graphene-reinforced nickel-based alloy reinforcing layer, which is obtained by laser forming of the graphene-reinforced nickel-based alloy material described in the second aspect on the surface of a substrate.
[0066] In this embodiment, the laser forming process includes: using a laser coaxial powder feeding process to perform laser additive manufacturing on the surface of a metal part, ultimately obtaining a graphene-reinforced nickel-based alloy strengthening layer. The laser forming must be performed under inert gas protection, with an argon protective gas flow rate of 5.1-5.5 m³ / h. 3 The laser forming process parameters are as follows: laser power 2000-3000W, spot diameter Φ4-5mm, scanning speed 10-20mm / s, powder feeding speed 20-25g / min, and overlap rate 50%. These parameters result in excellent cladding effects for the graphene-reinforced nickel-based alloy material, producing a dense and uniform reinforced layer with good adhesion to the substrate. Defects such as "unmelted, pores, and cracks" were not observed. The reinforced layer, with a thickness of 1.0-1.4mm, exhibits an epitaxial columnar crystal microstructure, a surface hardness of 43-50HRC, and good corrosion resistance. This graphene-reinforced nickel-based alloy reinforced layer can be applied to the repair of metallurgical components.
[0067] The graphene-reinforced nickel-based alloy strengthening layer is based on the above-mentioned graphene-reinforced nickel-based alloy material. The specific preparation method of the graphene-reinforced nickel-based alloy material can be referred to the above embodiments. Since the graphene-reinforced nickel-based alloy strengthening layer adopts some or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be elaborated here.
[0068] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to national standards. If there is no corresponding national standard, then general international standards, conventional conditions, or conditions recommended by the manufacturer are followed.
[0069] Example 1
[0070] 200 mL of ethanol was placed in a beaker, along with 2 g of graphene powder and 0.2 g of peroxybenzoic acid. The mixture was ultrasonically treated using an ultrasonic disperser at 300 W for 2 hours. Then, 98 g of nickel-based alloy powder (with a particle size of 50-150 μm, sphericity of 98%, and main components: Cr: 20%, Mo: 16%, W: 2%, Fe: 1%, Mn: 0.5%, and the remainder Ni) was added to the mixture while stirring at a rate of 300 r / min and maintaining the ultrasonic power at 300 W for 2 hours. After ultrasonic treatment, the mixture was filtered through slow-speed filter paper with a pore size <20 μm. The filtered powder was then placed in a heat treatment furnace and heated to 230 °C under argon protection for 2 hours, followed by cooling to room temperature to obtain a graphene-reinforced nickel-based alloy material.
[0071] The graphene-reinforced nickel-based alloy material from Example 1 was added to a laser forming device. Nitrogen gas was used as the protective gas, and the following parameters were adjusted: laser power 2300W, spot diameter 5mm, scanning rate 15mm / s, powder feeding speed 22g / min, and overlap rate 50%. Printing was then performed to obtain a graphene-reinforced nickel-based alloy strengthening layer.
[0072] Example 2
[0073] 200 mL of ethanol was placed in a beaker, along with 1 g of graphene powder and 1.2 g of aminodiphenyl ether. The mixture was ultrasonically treated using an ultrasonic disperser at 250 W for 2 hours. Then, 99 g of nickel-based alloy powder (with a particle size of 50-150 μm, sphericity of 98%, and main components: Cr: 18%, Mo: 16%, W: 4%, Fe: 1%, Mn: 1%, and the remainder Ni) was added to the mixture while stirring at a stirring rate of 300 r / min and an ultrasonic power of 250 W for 2 hours. After ultrasonic treatment, the mixture was filtered using slow-speed filter paper with a pore size <20 μm. The filtered powder was then placed in a heat treatment furnace and heated to 300 °C under argon protection for 2 hours, followed by cooling to room temperature to obtain a graphene-reinforced nickel-based alloy material.
[0074] The graphene-reinforced nickel-based alloy material from Example 2 was added to a laser forming device. Argon gas was used as the protective gas, and the following parameters were adjusted: laser power 2700w, spot diameter 4mm, scanning rate 20mm / s, powder feeding speed 24g / min, and overlap rate 50%. Printing was then performed to obtain a graphene-reinforced nickel-based alloy strengthening layer.
[0075] Example 3
[0076] 200 mL of ethanol was placed in a beaker, along with 0.5 g of graphene powder and 1 g of polystyrene sulfonic acid. The mixture was ultrasonically treated using an ultrasonic disperser at 200 W for 3 hours. Then, 99.5 g of nickel-based alloy powder (with a particle size of 50-150 μm, sphericity of 98%, and main components: Cr: 20%, Mo: 16%, W: 2%, Fe: 1%, Mn: 0.5%, and the remainder Ni) was added to the mixture while stirring at a rate of 300 r / min and maintaining the ultrasonic power at 200 W for 2 hours. After ultrasonic treatment, the mixture was filtered using slow-speed filter paper with a pore size <20 μm. The filtered powder was then placed in a heat treatment furnace and heated to 200 °C under argon protection for 2 hours, followed by cooling to room temperature to obtain a graphene-reinforced nickel-based alloy material.
[0077] The graphene-reinforced nickel-based alloy material from Example 3 was added to a laser forming device. Nitrogen gas was used as the protective gas, and the following parameters were adjusted: laser power 2500W, spot diameter 5mm, scanning rate 15mm / s, powder feeding speed 22g / min, and overlap rate 50%. Printing was then performed to obtain a graphene-reinforced nickel-based alloy strengthening layer.
[0078] Comparative Example 1
[0079] 200 mL of ethanol was placed in a beaker, and 1 g of graphene powder was added. The mixture was ultrasonically treated using an ultrasonic disperser at 200 W for 3 hours. Then, 99 g of nickel-based alloy powder (with a particle size of 50-150 μm, sphericity of 98%, and main components as follows: Cr: 20%, Mo: 16%, W: 2%, Fe: 1%, Mn: 0.5%, and the remainder Ni) was added to the mixture while stirring at a stirring rate of 300 r / min and an ultrasonic power of 200 W for 2 hours. After the treatment, the mixture was filtered using slow-speed filter paper with a pore size <20 μm. The filtered powder was then placed in a heat treatment furnace and heated to 300 °C under argon protection for 2 hours, after which it was cooled to room temperature to obtain a graphene-reinforced nickel-based alloy material.
[0080] The graphene-reinforced nickel-based alloy material from Comparative Example 1 was added to a laser forming device. Nitrogen gas was used as the protective gas, and the following parameters were adjusted: laser power 2500W, spot diameter 5mm, scanning rate 15mm / s, powder feeding speed 22g / min, and overlap rate 50%. Printing was then performed, and a graphene-reinforced nickel-based alloy strengthening layer was finally obtained.
[0081] The hardness of the reinforced layer obtained in Example 1 is 44 HRC, and the self-corrosion potential is -0.11 V, while the hardness of the same nickel-based alloy without graphene coating is 41 HRC, and the self-corrosion potential is -0.32 V, thus improving corrosion resistance. For example, Figure 2 This is a SEM image of a graphene-reinforced nickel-based alloy material provided in Embodiment 1 of this application; please refer to [link / reference]. Figure 2 This indicates that graphene and nickel-based alloys have been successfully combined, with graphene distributed on the surface of the nickel-based alloy powder. The area within the box in the figure represents graphene. Figure 3 A metallographic diagram of a graphene-reinforced nickel-based alloy strengthening layer provided in Embodiment 1 of this application; please refer to... Figure 3 This indicates that the graphene-reinforced nickel-based alloy strengthening layer has a dense and uniform structure and is well bonded to the matrix. A small amount of the heat-treated powder was attempted to be ignited; no flame was produced, indicating that the modifier and dispersant had been completely removed.
[0082] The reinforced layer obtained in Example 2 has a hardness of 47 HRC and a self-corrosion potential of -0.06 V, while the same nickel-based alloy without a graphene coating has a hardness of 41 HRC and a self-corrosion potential of -0.33 V, thus improving corrosion resistance. For example, Figure 4 The XRD characterization results of a graphene-reinforced nickel-based alloy strengthening layer provided in Example 2 of this application show that the main constituent phases of the strengthening layer are γ-Ni, M6C, and M... 23 C6, with few impurity peaks, and high purity of the graphene-reinforced nickel-based alloy strengthening layer.
[0083] Figure 5 Tafel curves for a graphene-reinforced nickel-based alloy strengthening layer and a graphene-free nickel-based alloy strengthening layer provided in Embodiment 2 of this application; please refer to... Figure 5 This indicates that graphene and nickel-based alloys form an effective bond, and the performance of the reinforced layer after laser coaxial powder feeding printing is superior to that of the alloy reinforced layer without graphene. A small amount of heat-treated powder was attempted to be ignited; no flame was produced, indicating that the modifier and dispersant have been completely removed.
[0084] The hardness of the reinforced layer obtained in Example 3 is 44 HRC, and the self-corrosion potential is -0.16 V, while the hardness of the nickel-based alloy without graphene coating is 41 HRC, and the self-corrosion potential is -0.32 V, indicating improved corrosion resistance. A small amount of the heat-treated powder was attempted to be ignited; no flame was produced, indicating that the modifier and dispersant had been completely removed.
[0085] The hardness of the reinforced layer obtained in Comparative Example 1 was 40 HRC, and the self-corrosion potential was -0.33 V. In contrast, the hardness of the nickel-based alloy without the graphene coating was 41 HRC, and the self-corrosion potential was -0.32 V. The slight decrease in hardness is due to the lack of graphene modification, resulting in graphene agglomeration and a less dense coating. For example, Figure 6 SEM image of a graphene-reinforced nickel-based alloy material provided in Comparative Example 1 of this application; please refer to [link / reference]. Figure 6 This indicates that the graphene powder and the nickel-based alloy did not form an effective bond, and the surface of the nickel-based alloy was relatively smooth.
[0086] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing graphene reinforced nickel-based alloy material suitable for laser coaxial powder forming, characterized in that, The method includes: Graphene powder, modifier, and dispersant are first mixed and first ultrasonically treated to obtain a graphene mixed solution. The modifier includes one of the following: peroxybenzoic acid, aminodiphenyl ether, and polystyrene sulfonic acid. The graphene mixed solution and nickel-based alloy powder with sphericity ≥95% are subjected to a second mixing and a second ultrasonic treatment, followed by filtration and ball milling to obtain graphene-nickel-based alloy mixed powder. After ball milling, the diameter of the nickel-based alloy powder is 50-150μm, the sheet size of graphene is 10-20μm, and the graphene is distributed on the surface of the nickel-based alloy powder. The graphene-nickel-based alloy mixed powder is heat-treated at 200℃~300℃ to obtain a graphene-reinforced nickel-based alloy material; wherein, the boiling point of the modifier and the heat treatment temperature satisfy the following relationship: 50℃≤T2-T1≤150℃ In the formula, T2 represents the heat treatment temperature, and T1 represents the boiling point of the modifier; The weight ratio of the graphene powder to the nickel-based alloy powder is (1~2):(98~99); The ball milling process parameters include: a ball milling speed of 200~400 r / min and a ball milling time of 2~4 h.
2. The method according to claim 1, characterized in that, If the modifier is peroxybenzoic acid, then the amount of peroxybenzoic acid is 0.1~1g relative to 100mL of the dispersant; If the modifier is an aminodiphenyl ether, then relative to 100 mL of the dispersant, the aminodiphenyl ether is 0.5~1g; If the modifier is polystyrene sulfonic acid, then relative to 100 mL of the dispersant, the polystyrene sulfonic acid... The amount is 0.5~1g.
3. The method according to claim 1, characterized in that, The process parameters for the first and second ultrasonic treatments include: ultrasonic power of 100~300w and ultrasonic time of 2~3h.
4. A graphene-reinforced nickel-based alloy material, characterized in that, The graphene-reinforced nickel-based alloy material is made of The method described in any one of claims 1 to 3 is used to prepare the product.
5. A graphene-reinforced nickel-based alloy strengthening layer, characterized in that, The graphene-reinforced nickel-based alloy reinforcing layer is obtained by laser coaxial powder feeding molding of the graphene-reinforced nickel-based alloy material as described in claim 4 on the substrate surface.
Citation Information
Patent Citations
Preparation method of graphene reinforced powder metallurgy nickel-based superalloy composite powder