A chemical mechanical polishing liquid and its preparation method and application

By using a two-stage filtration process to prepare a chemical-mechanical fine polishing liquid during the silicon wafer polishing process, the problem of metal impurities and particle residues on the surface of the silicon wafer is solved, the number of large particles and surface defects are reduced, and the polishing efficiency is improved. Effect.

CN118421208BActive Publication Date: 2024-10-18WANHUA CHEM GRP ELECTRONIC MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410894207.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-18
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively reduce metal impurities and particle residues on the silicon wafer surface during the chemical mechanical polishing process of silicon wafers, and fails to improve the application performance of the fine polishing liquid through improvements in the filtration process.

Method used

A two-stage filtration process is used to prepare the chemical mechanical fine polishing liquid. First, the intermediate mixture is filtered at two stages of intermediate product, then silica sol is added and the fine polishing liquid is filtered again at two stages. A filter element with a specific pore size and material is used to ensure the filtration pressure difference. and speed within the appropriate range to reduce the number of large particles.

Benefits of technology

It significantly reduces the number of large particles in the polishing liquid, improves the surface flatness of the silicon wafer, reduces the number of defects on the wafer surface, and improves the polishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118421208B_ABST
    Figure CN118421208B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of chemical mechanical polishing, and provides a chemical mechanical fine polishing liquid and a preparation method and application thereof; the preparation method of the present invention is used to prepare the fine polishing liquid, and a fine polishing liquid with a small number of large particles can be obtained, and the fine polishing liquid is applied to the chemical mechanical polishing of silicon wafers, which can reduce the number of surface defects of the wafers. The preparation method comprises the following steps: 1) the intermediate mixed liquid is sequentially subjected to the first stage filtration of the intermediate product and the second stage filtration of the intermediate product to obtain the intermediate product; the intermediate mixed liquid is a mixed material including water, a viscosity regulator and a pH regulator, and no silica sol is added to the intermediate mixed liquid; 2) the silica sol and the intermediate product are mixed, and the fine polishing liquid is sequentially subjected to the first stage filtration and the second stage filtration of the fine polishing liquid to obtain the fine polishing liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical mechanical polishing (CMP), and in particular to a chemical mechanical polishing liquid and a preparation method and application thereof. Background Art

[0002] Silicon is the first generation of semiconductor materials. It is abundant in reserves and low in cost, and is widely used in the integrated circuit and photovoltaic industries. In integrated circuit manufacturing, chemical mechanical polishing (CMP) is used to process the surface of silicon wafers to make them globally flat. With the reduction of integrated circuit feature size and the increase of silicon wafer size, higher requirements are placed on the metal impurities and particle residues on the surface of silicon wafers after CMP.

[0003] Fine polishing is the final process for preparing silicon wafers with complete crystal lattices and no surface damage. It has become a crucial step in semiconductor device manufacturing technology. To obtain silicon wafers with low surface metal impurities and residual particles, the most important thing is to control the number of metal ions and large particles in the fine polishing solution.

[0004] Chinese patent application CN115851138A discloses a silicon wafer polishing liquid, which uses a unit or multi-unit organic acid to adjust the final pH value in the presence of a specific content of high-purity ammonia water, and can inhibit the agglomeration of abrasive particles to a certain extent and reduce the contamination of particles on the surface of silicon wafers. Chinese patent application CN116554788A discloses a silicon wafer polishing liquid, which changes the surface properties of silicon wafers by adding macromolecular polymers, improves the hydrophilicity of the silicon wafer surface, prevents the adhesion of abrasive particles to the surface of silicon wafers after chemical mechanical polishing, reduces the contamination of particles on the surface of silicon wafers, and reduces the particle defects on the surface of silicon wafers. Chinese patent application CN116948532A discloses a silicon wafer polishing liquid, which improves the dispersibility of silica sol by imidazole-modified high-purity silica sol, weakens the electrostatic repulsion between silica sol and silicon wafers, and significantly improves the polishing rate of silicon wafers. At the same time, after polishing, there are very few contaminating particles on the surface of silicon wafers, no scratches or depressions on the surface, and the surface state is good. None of the above patent applications involve solutions to improve the application performance of polishing liquids by improving the filtration process. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a chemical mechanical polishing liquid and a preparation method and application thereof. By adopting the preparation method of the present invention to prepare the polishing liquid, a polishing liquid with a small number of large particles can be obtained, and the polishing liquid is applied to the chemical mechanical polishing of silicon wafers, which can reduce the number of surface defects of the wafers.

[0006] To achieve the purpose, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a chemical mechanical polishing liquid, comprising the following steps:

[0008] 1) subjecting the intermediate mixed liquid to first-stage filtration of the intermediate product and second-stage filtration of the intermediate product in sequence to obtain an intermediate product; the intermediate mixed liquid is a mixture comprising water, a viscosity regulator and a pH regulator, and no silica sol is added to the intermediate mixed liquid;

[0009] The first-stage filtration of the intermediate product adopts a filter element I with a pore size of 1 μm to 10 μm, and the second-stage filtration of the intermediate product adopts a filter element II with a pore size of 0.053 μm to 1.7 μm, and the pore size ratio of the filter element I to the filter element II is 6 to 19:1; the material of the filter element I is polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF), and the material of the filter element II is polysulfone (PSF), polyethersulfone (PES), sulfonated polyethersulfone (SPES) or nylon;

[0010] 2) mixing the silica sol and the intermediate product, and sequentially performing first-stage filtration of the fine polishing liquid and second-stage filtration of the fine polishing liquid to obtain the fine polishing liquid;

[0011] The first-stage filtration of the fine polishing liquid adopts a filter element III with a pore size of 1μm~10μm, and the second-stage filtration of the fine polishing liquid adopts a filter element IV with a pore size of 0.11μm~3.3μm, and the pore size ratio of the filter element III and the filter element IV is 3~9:1; the material of the filter element III is polyethylene (PE) or polypropylene (PP), and the material of the filter element IV is polyethylene (PE) or polypropylene (PP).

[0012] Preferably, the pore size of the filter element I is 1 μm to 5 μm, and the material is polyvinylidene fluoride (PVDF);

[0013] And / or, the pore size of the filter element II is 0.067 μm to 0.5 μm, the material is sulfonated polyethersulfone or nylon, and the pore size ratio of the filter element I to the filter element II is 10 to 15:1;

[0014] And / or, the pore size of the filter element III is 1 μm to 5 μm, and the material is polypropylene (PP);

[0015] And / or, the pore size of the filter element IV is 0.14 μm~1 μm, the material is polypropylene, and the pore size ratio of the filter element III and the filter element IV is 5~7:1.

[0016] Preferably, the filtration pressure difference of the first stage filtration of the intermediate product and the second stage filtration of the intermediate product are ≤0.5MPa, and the filtration speed is <10 L / min;

[0017] And / or, the filtration pressure difference of the first stage filtration of the fine polishing liquid and the second stage filtration of the fine polishing liquid are respectively ≤0.5MPa, and the filtration speeds are respectively <6 L / min.

[0018] Further preferably, the filtration pressure difference of the first stage filtration of the intermediate product and the second stage filtration of the intermediate product are ≤0.3MPa, and the filtration speed is <5 L / min;

[0019] And / or, the filtration pressure difference between the first stage filtration of the fine polishing liquid and the second stage filtration of the fine polishing liquid is ≤0.3MPa; and the filtration speed is <3 L / min.

[0020] In some implementations, based on the total mass of the polishing liquid, the content of the viscosity regulator is 0.08% to 1.5%, the content of the pH regulator is 0.1% to 1%, and the content of the silica sol is 3% to 13%.

[0021] And / or, the metal ion content in the silica sol is less than 0.1 ppm, and the primary particle size is 10-50 nm.

[0022] Furthermore, in step 1), the first stage filtration of the intermediate product and the second stage filtration of the intermediate product are performed only once;

[0023] In step 2), the first stage filtration of the polishing liquid and the second stage filtration of the polishing liquid are both performed only once.

[0024] Specifically, the pH adjuster is selected from one or more of organic bases and inorganic bases.

[0025] In some embodiments, the pH regulator is selected from one or more of ammonia water, KOH, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), and piperazine; the viscosity regulator is selected from one or more of hydroxypropyl starch, carboxymethyl starch, carboxyethyl starch, hydroxyethyl starch, hydroxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.

[0026] The present invention also provides a chemical mechanical polishing liquid, which is prepared by the preparation method described above.

[0027] The present invention also provides the use of the chemical mechanical polishing liquid described above in chemical mechanical polishing of a wafer, wherein the wafer is a silicon wafer or a wafer with silicon as a substrate.

[0028] The technical solution provided by the present invention has the following beneficial effects:

[0029] For a fine polishing liquid prepared based on materials such as silica sol, a viscosity regulator (such as hydroxypropyl starch), a pH regulator, etc., the method of the present invention is used to prepare the fine polishing liquid, so that a fine polishing liquid with a small number of large particles can be obtained, and the fine polishing liquid is applied to chemical mechanical polishing of silicon wafers, which can reduce the number of surface defects of the wafers. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the particle size distribution image of the intermediate product in Comparative Example 1.

[0031] Figure 2 This is the particle size distribution image of the intermediate product in Example 4. DETAILED DESCRIPTION

[0032] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the invention belongs. The term "and / or" as may be used herein includes any and all combinations of one or more of the associated listed items.

[0034] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0035] In this specification, the terms “first”, “second”, etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance.

[0036] One aspect of the present invention provides a method for preparing a chemical mechanical polishing liquid, comprising the following steps:

[0037] 1) subjecting the intermediate mixed liquid to first-stage filtration of the intermediate product and second-stage filtration of the intermediate product in sequence to obtain an intermediate product; the intermediate mixed liquid is a mixture comprising water, a viscosity regulator and a pH regulator, and no silica sol is added to the intermediate mixed liquid;

[0038] The first-stage filtration of the intermediate product adopts a filter element I with a pore size of 1μm~10μm, and the second-stage filtration of the intermediate product adopts a filter element II with a pore size of 0.053μm~1.7μm, and the pore size ratio of the filter element I and the filter element II is 6~19:1 (for example, 6:1, 8:1, 10:1, 12:1, 14:1, 16:1, 19:1, etc.); the material of the filter element I is polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF), and the material of the filter element II is polysulfone (PSF), polyethersulfone (PES), sulfonated polyethersulfone (SPES) or nylon;

[0039] 2) mixing the silica sol and the intermediate product, and sequentially performing first-stage filtration of the fine polishing liquid and second-stage filtration of the fine polishing liquid to obtain the fine polishing liquid;

[0040] The first-stage filtration of the fine polishing liquid adopts a filter element III with a pore size of 1μm~10μm, and the second-stage filtration of the fine polishing liquid adopts a filter element IV with a pore size of 0.11μm~3.3μm, and the pore size ratio of the filter element III and the filter element IV is 3~9:1 (for example, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, etc.); the material of the filter element III is polyethylene (PE) or polypropylene (PP), and the material of the filter element IV is polyethylene (PE) or polypropylene (PP).

[0041] The preparation method of the present invention is directed to a fine polishing liquid prepared based on materials such as silica sol and a viscosity modifier (such as hydroxypropyl starch). In the process of preparing the fine polishing liquid, before adding the silica sol, the mixed material of other components is first subjected to two-stage filtration, and then subjected to two-stage filtration again after adding the silica sol, and the two-stage filtrations before and after use a filter element with a specific aperture and aperture ratio, and a specific filter element material is used in combination; the fine polishing liquid prepared by the method can significantly reduce the particle size of the intermediate product, and finally obtain a fine polishing liquid with a small number of large particles, which is used in the chemical mechanical polishing of silicon wafers to reduce the number of surface defects of the wafers. When the preparation method of the present invention is used to prepare the fine polishing liquid, the two-stage filtration of step 1) and the two-stage filtration of step 2) only need to be performed once, without repeating multiple times, and the process is simple.

[0042] In the process of preparing the fine polishing liquid of the present invention, the intermediate mixed liquid is first subjected to a two-stage filtration, and a specific two-stage filter element material and aperture ratio are used; through the first two-stage filtration, large-size particles can be effectively intercepted to prevent the large-size particles from adhering to the silica sol during the preparation of the fine polishing liquid, thereby causing an adverse effect on the fine polishing liquid. After that, a second two-stage filtration is performed after adding the silica sol, and a specific aperture ratio is used, which can effectively reduce the number of large particles in the fine polishing liquid (for example, the number of large particles >0.56μm in the fine polishing liquid can be reduced), achieving the effect of reducing the number of surface defects of the wafer.

[0043] In the present invention, the material of the filter element I is polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF); the material of the filter element II is polysulfone (PSF), polyethersulfone (PES), sulfonated polyethersulfone (SPES) or nylon (Nylon); the material of the filter element III is polyethylene (PE) or polypropylene (PP); the material of the filter element IV is polyethylene (PE) or polypropylene (PP). The inventors found that in the preparation method of the fine polishing liquid of the present invention, at different filtration stages, a specific combination of filter element materials is used for filter elements I-IV, and the specific pore size and pore size ratio selection of the first two-stage filtration and the second two-stage filtration can significantly improve the quality of the obtained fine polishing liquid, which is beneficial to reduce the number of large particles in the fine polishing liquid and improve the application performance of the fine polishing liquid.

[0044] In a preferred embodiment, the pore size of the filter element I is 1 μm to 5 μm, and the material is polyvinylidene fluoride (PVDF).

[0045] In a preferred embodiment, the pore size of the filter element II is 0.067 μm to 0.5 μm, the material is sulfonated polyethersulfone (SPES) or nylon, and the pore size ratio of the filter element I to the filter element II is 10 to 15:1.

[0046] In a preferred embodiment, the pore size of the filter element III is 1 μm to 5 μm, and the material is polypropylene (PP).

[0047] In a preferred embodiment, the pore size of the filter element IV is 0.14 μm to 1 μm, the material is polypropylene (PP), and the pore size ratio of the filter element III to the filter element IV is 5 to 7:1.

[0048] In some better embodiments, the pore size of the filter element I is 1 μm to 5 μm, and the material is polyvinylidene fluoride (PVDF); the pore size of the filter element II is 0.067 μm to 0.5 μm, and the material is sulfonated polyethersulfone (SPES) or nylon, and the pore size ratio of the filter element I to the filter element II is 10 to 15:1; the pore size of the filter element III is 1 μm to 5 μm, and the material is polypropylene (PP); the pore size of the filter element IV is 0.14 μm to 1 μm, and the material is polypropylene (PP), and the pore size ratio of the filter element III to the filter element IV is 5 to 7:1. The use of the preferred material combination and pore size for the filter elements I-IV is conducive to taking into account the relatively small number of large particles in the fine polishing liquid, and can further improve the application performance of the fine polishing liquid.

[0049] In some embodiments, the filtration pressure difference of the first stage filtration of the intermediate product and the second stage filtration of the intermediate product is ≤0.5MPa, and the filtration speed is <10 L / min. Preferably, the filtration pressure difference of the first stage filtration of the intermediate product and the second stage filtration of the intermediate product is ≤0.3MPa, and the filtration speed is <5 L / min. The use of the preferred filtration conditions is conducive to further reducing the number of large particles in the fine polishing liquid and further improving the application performance of the fine polishing liquid.

[0050] In some embodiments, the filtration pressure difference of the first stage filtration of the polishing liquid and the second stage filtration of the polishing liquid is ≤0.5MPa, and the filtration speed is <6 L / min. Preferably, the filtration pressure difference of the first stage filtration of the polishing liquid and the second stage filtration of the polishing liquid is ≤0.3MPa; the filtration speed is <3 L / min. The use of the preferred filtration conditions is conducive to taking into account the relatively small number of large particles in the polishing liquid and can further improve the application performance of the polishing liquid.

[0051] Preferably, based on the total mass of the polishing liquid, the content of the viscosity regulator is 0.08%~1.5% (for example, 0.08%, 0.1%, 0.5%, 1%, 1.5%, etc.), the content of the pH regulator is 0.1%~1% (for example, 0.1%, 0.5%, 1%); the content of the silica sol is 3%~13%, for example (3%, 5%, 10%, 13%), and water is the balance.

[0052] Preferably, the silica sol is ultra-high purity silica sol, wherein the metal ion content is less than 0.1 ppm and the primary particle size is 10-50 nm. The "primary particle size" refers to the size of the silica sol under a scanning electron microscope image.

[0053] Furthermore, the first-stage filtration of the intermediate product and the second-stage filtration of the intermediate product in step 1) are both performed only once; the first-stage filtration of the fine polishing liquid and the second-stage filtration of the fine polishing liquid in step 2) are both performed only once; that is, in the preparation method of the present invention, filtration at each stage does not need to be repeated or cyclically performed, and a fine polishing liquid with good quality can be obtained by performing only a single filtration.

[0054] Specifically, the pH regulator is selected from one or more organic bases and inorganic bases, such as piperazine, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), etc., and inorganic bases such as ammonia water, KOH, etc. A second aspect of the present invention provides a chemical mechanical polishing liquid, which is prepared by the preparation method described above.

[0055] Specifically, the viscosity modifier can be selected from one or more of hydroxypropyl starch, carboxymethyl starch, carboxyethyl starch, hydroxyethyl starch, hydroxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.

[0056] A third aspect of the present invention provides use of the chemical mechanical polishing liquid described above in chemical mechanical polishing of a wafer, wherein the wafer is a silicon wafer or a wafer with silicon as a substrate.

[0057] In some embodiments, the polishing is performed after the polishing liquid is diluted 10-80 times (by mass) with water (preferably ultrapure water). In some embodiments, when the polishing liquid is used for polishing a silicon wafer, the polishing conditions are, for example: a silicon wafer diameter of 200 or 300 mm, a polishing pressure of 100-200 g / cm 2, polishing temperature is 25~30℃, polishing head and polishing disc speed is 80~100 rpm, polishing time is 1~10 min, polishing liquid flow rate is 0.1~1 L / min; polishing pad is POLYPAS 27NX series. In one example, the polishing conditions are: using polishing machine EBARA, silicon wafer diameter is 300 mm, polishing pad is POLYPAS 275NX, polishing pressure is 150 g / cm 2 , the polishing temperature was 25°C, the rotation speeds of the polishing disc and polishing head were 95 rpm and 86 rpm respectively, the polishing time was 2 min, and the polishing liquid flow rate was 0.3 L / min.

[0058] The main raw materials used in the examples and comparative examples of the present invention are described as follows:

[0059] Ultra-high purity silica sol: purchased from FUSO Company of Japan, with a metal ion content of 50 ppb and a primary particle size of 10-50 nm;

[0060] Other reagents are common raw materials purchased from the market unless otherwise specified;

[0061] Unless otherwise specified, the filter elements are ordinary filter elements purchased on the market.

[0062] Embodiments 1 to 9

[0063] A chemical mechanical polishing liquid for silicon wafers is prepared, wherein the polishing liquid includes, by mass percentage, 3%-13% ultra-high purity silica sol, 0.08%-1.5% viscosity modifier, 0.1%-1% pH modifier, and the remainder is ultrapure water, and the sum of the mass percentages of each component is 100%. In the polishing liquid of each embodiment, the components and the mass content of each component are shown in Table 1. The preparation process of the polishing liquid comprises the following steps:

[0064] 1) Mixing a viscosity regulator, a pH regulator and water uniformly to obtain an intermediate mixed liquid, and subjecting the intermediate mixed liquid to intermediate product first-stage filtration and intermediate product second-stage filtration in sequence to obtain an intermediate product; wherein the intermediate product first-stage filtration is performed by filter element I, and the intermediate product second-stage filtration is performed by filter element II. The materials and pore sizes of the filter element I and filter element II used in each embodiment are shown in Table 2; the filtering conditions for the intermediate product first-stage filtration and the intermediate product second-stage filtration in step 1) of each embodiment are all referred to the "intermediate product filtration conditions" in Table 2;

[0065] 2) Add the ultra-high purity silica sol to the intermediate product of step 1), mix well, and then sequentially perform first-stage filtration and second-stage filtration of the polishing liquid on the obtained mixed material to obtain the chemical mechanical polishing liquid for silicon wafers. The first-stage filtration of the polishing liquid is performed by filter element III, and the second-stage filtration of the polishing liquid is performed by filter element IV. The materials and pore sizes of the filter elements III and IV used in each embodiment are shown in Table 2. The filtering conditions for the first-stage filtration and the second-stage filtration of the polishing liquid in step 2) of each embodiment are all referred to the "Finishing Liquid Filtration Conditions" in Table 2.

[0066] Table 1 Composition of chemical mechanical polishing liquid for silicon wafers in Examples 1 to 9

[0067]

[0068] Table 2 Silicon wafer chemical mechanical polishing liquid filtration process of Examples 1 to 9

[0069]

[0070] Example 10

[0071] The method is carried out in accordance with Example 4, except that: in step 1), the filtering conditions for the intermediate product are a filtering pressure difference of 0.5 MPa and a filtering speed of 6.0 L / min; and the filtering conditions for the fine polishing liquid in step 2) are a filtering pressure difference of 0.5 MPa and a filtering speed of 4.0 L / min.

[0072] Embodiment 11

[0073] The method is carried out with reference to Example 4, except that: the pore size of filter element I is 10 μm, the pore size of filter element II is 1 μm, and the pore size ratio of the two is 10:1; the pore size of filter element III is 10 μm, the pore size of filter element IV is 2 μm, and the pore size ratio of the two is 5:1.

[0074] Comparative Example 1

[0075] The same method is carried out as in Example 4, except that no filtering is performed in step 1) and step 2).

[0076] Comparative Example 2

[0077] The method is carried out in accordance with Example 4, except that: in step 2), the first stage filtration of the polishing liquid and the second stage filtration of the polishing liquid are not performed.

[0078] Comparative Example 3

[0079] The method is carried out in accordance with Example 4, except that in step 1), the first stage filtration and the second stage filtration of the intermediate product are not performed.

[0080] Comparative Example 4 (pore size ratio of filter element I and filter element II is 5)

[0081] The method is carried out with reference to Example 4, except that the pore size of filter element I is 1 μm, and the pore size of filter element II is 0.2 μm.

[0082] Comparative Example 5 (pore size ratio of filter element I and filter element II is 20)

[0083] The method is carried out with reference to Example 4, except that the pore size of filter element I is 1 μm, and the pore size of filter element II is 0.05 μm.

[0084] Comparative Example 6 (pore size ratio of filter element III and filter element IV is 2)

[0085] The method is carried out with reference to Example 4, except that the pore size of filter element III is 1 μm, and the pore size of filter element IV is 0.5 μm.

[0086] Comparative Example 7 (pore size ratio of filter element III and filter element IV is 10)

[0087] The method is carried out with reference to Example 4, except that the pore size of filter element III is 1 μm, and the pore size of filter element IV is 0.1 μm.

[0088] Comparative Example 8

[0089] Refer to Example 4, the only difference is that the material of filter element I is polypropylene (PP) and the material of filter element II is polypropylene (PP).

[0090] Comparative Example 9

[0091] The method is carried out with reference to Example 4, except that the material of the filter element III is polyvinylidene fluoride (PVDF), and the material of the filter element IV is nylon.

[0092] The particle size of the intermediate product obtained in step 1) and the number of large particles with a particle size > 0.56 μm in the polishing liquid obtained in step 2) in the above embodiments and comparative examples were statistically analyzed, as shown in Table 3. The detection method is as follows:

[0093] Particle size of intermediate product: tested with Zetasizer Nano ZS90, Malvern, UK. The intermediate product was placed in a DTS0012 particle size tube and tested three times to obtain the average value.

[0094] Number of large particles in fine polishing liquid: Use American PSS AccuSize A9000 FX Nano for detection. The system pre-dilutes the fine polishing liquid 13 times, and then automatically injects and dilutes it. The test is performed three times and the average value is taken to record the number of large particles >0.56μm.

[0095] The chemical mechanical polishing liquid for silicon wafer prepared in the above-mentioned embodiment and comparative example was used to polish silicon wafers, and the application performance was examined:

[0096] The diameter of the silicon wafer used is 300 mm and is provided by Huahai Qingke Co., Ltd.

[0097] The fine polishing liquid should be diluted 30 times (by mass) with ultrapure water before use.

[0098] Polishing conditions are as follows: polishing machine is Japanese EBARA. Polishing pad is Japanese FUJIBO POLYPAS 275NX. Polishing pressure is 150 g / cm 2 , the polishing pad temperature was 27 °C, the polishing disc and polishing head speeds were 95 rpm and 86 rpm respectively, the polishing time was 2 min, and the polishing liquid flow rate was 0.3 L / min.

[0099] The number of surface defects of the polished silicon wafer is counted, as shown in Table 3. The method for detecting the number of surface defects of the silicon wafer is as follows:

[0100] Use China Science and Technology Feice Spruce-800 to detect and record the number of defects on the wafer surface with a defect size of more than 40 nm. Test 25 pieces and take the average value.

[0101] Table 3 Particle size of intermediate products in various embodiments and comparative examples, number of large particles in fine polishing liquid > 0.56 μm

[0102] and number of defects on silicon wafer surface

[0103]

[0104] Compared with Example 4, the intermediate product and the polishing liquid in Comparative Example 1 were not filtered, resulting in a significant increase in the particle size of the intermediate product and the number of large particles in the polishing liquid, and a high number of surface defects on the silicon wafer after polishing. Figure 1 and Figure 2 As shown, after adding the filtration of the intermediate product, large-size particles can be effectively intercepted and the average particle size value can be reduced. In Comparative Example 2, the intermediate product was filtered, but the fine polishing liquid was not filtered; the intermediate product of Comparative Example 3 was not filtered, but the fine polishing liquid was filtered; compared with Comparative Example 1, the number of surface defects of silicon wafers can be reduced to a certain extent, but it still cannot meet the requirements of the application that the number of defects above 40 nm is less than 100. Comparative Examples 4 and 5 adjust the filtration aperture ratio of the intermediate product. If the filtration aperture ratio is enlarged, the intermediate product cannot be effectively filtered. If the filtration aperture ratio is narrowed, the effective components in the intermediate product are lost, which will increase the number of defects on the wafer surface. Similarly, Comparative Examples 6 and 7 adjust the filtration aperture ratio of the fine polishing liquid, which will increase the number of defects on the wafer surface.

[0105] Examples 1 to 9 simultaneously perform two-stage filtration on the intermediate product and the fine polishing liquid, respectively. The particle size of the intermediate product and the number of large particles in the fine polishing liquid are significantly reduced compared with Comparative Examples 1-3, and the number of surface defects of the silicon wafer is further reduced. Comparative Example 8 replaces the material of the intermediate product filter element. The filter element has no interception effect on the intermediate product, and its effect on the wafer surface is equivalent to that of Comparative Example 3. Comparative Example 9 replaces the material of the fine polishing liquid filter element. The filter element blocks all the effective ingredients of the fine polishing liquid, has no protective effect on the wafer surface, and the number of surface defects increases significantly. Example 10 does not adopt the preferred filtering conditions, and the filtration pressure difference increases, resulting in an increase in the filtration flow rate and a decrease in the filtration fineness; Example 11 does not adopt the preferred filter element pore size, and the filter element pore size increases, which reduces the filtration effect on the intermediate product and the fine polishing liquid, both of which cause an increase in the number of wafer surface defects.

[0106] In summary, the present invention can achieve the effect of reducing the particle size of the intermediate product and the number of large particles in the fine polishing liquid by filtering the intermediate product and the fine polishing liquid in two stages respectively, and the fine polishing liquid obtained can significantly reduce the number of defects on the wafer surface in application. Using the fine polishing liquid of the present invention, the number of defects larger than 40 nm on the surface of the silicon wafer is less than 100.

[0107] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.

Claims

1. A method for preparing a chemical mechanical polishing liquid, characterized in that: The steps include: 1) subjecting the intermediate mixed liquid to first-stage filtration of the intermediate product and second-stage filtration of the intermediate product in sequence to obtain an intermediate product; the intermediate mixed liquid is a mixture comprising water, a viscosity regulator and a pH regulator, and no silica sol is added to the intermediate mixed liquid; The first-stage filtration of the intermediate product adopts a filter element I with a pore size of 1μm~10μm, and the second-stage filtration of the intermediate product adopts a filter element II with a pore size of 0.053μm~1.7μm, and the pore size ratio of the filter element I and the filter element II is 6~19:1; the material of the filter element I is polytetrafluoroethylene or polyvinylidene fluoride, and the material of the filter element II is polysulfone, polyethersulfone, sulfonated polyethersulfone or nylon; the filtration pressure difference of the first-stage filtration of the intermediate product and the second-stage filtration of the intermediate product is ≤0.5MPa, and the filtration speed is <10 L / min respectively; 2) mixing the silica sol and the intermediate product, and sequentially performing first-stage filtration of the fine polishing liquid and second-stage filtration of the fine polishing liquid to obtain the fine polishing liquid; The first-stage filtration of the fine polishing liquid adopts a filter element III with a pore size of 1μm~10μm, and the second-stage filtration of the fine polishing liquid adopts a filter element IV with a pore size of 0.11μm~3.3μm, and the pore size ratio of the filter element III and the filter element IV is 3~9:1; the material of the filter element III is polyethylene or polypropylene, and the material of the filter element IV is polyethylene or polypropylene; the filtration pressure difference of the first-stage filtration of the fine polishing liquid and the second-stage filtration of the fine polishing liquid are ≤0.5MPa, respectively, and the filtration speed is <6 L / min, respectively.

2. The preparation method according to claim 1, characterized in that: The pore size of the filter element I is 1 μm to 5 μm, and the material is polyvinylidene fluoride; And / or, the pore size of the filter element II is 0.067 μm to 0.5 μm, the material is sulfonated polyethersulfone or nylon, and the pore size ratio of the filter element I to the filter element II is 10 to 15:1; And / or, the pore size of the filter element III is 1 μm to 5 μm, and the material is polypropylene; And / or, the pore size of the filter element IV is 0.14 μm~1 μm, the material is polypropylene, and the pore size ratio of the filter element III and the filter element IV is 5~7:

1.

3. The preparation method according to claim 1 or 2, characterized in that The filtration pressure difference of the first stage filtration of the intermediate product and the second stage filtration of the intermediate product are ≤0.3MPa, and the filtration speed is <5 L / min; And / or, the filtration pressure difference between the first stage filtration of the fine polishing liquid and the second stage filtration of the fine polishing liquid is ≤0.3MPa; Filtration rate <3 L / min.

4. The preparation method according to claim 1 or 2, characterized in that: Based on the total mass of the polishing liquid, the content of the viscosity regulator is 0.08% to 1.5%, the content of the pH regulator is 0.1% to 1%, and the content of the silica sol is 3% to 13%; And / or, the metal ion content in the silica sol is less than 0.1 ppm, and the primary particle size is 10-50 nm.

5. The preparation method according to claim 1 or 2, characterized in that: In step 1), the first stage filtration of the intermediate product and the second stage filtration of the intermediate product are both performed only once; In step 2), the first stage filtration of the polishing liquid and the second stage filtration of the polishing liquid are both performed only once.

6. The preparation method according to claim 1 or 2, characterized in that: The pH adjuster is selected from one or more of organic bases and inorganic bases.

7. The preparation method according to claim 6, characterized in that: The pH regulator is selected from one or more of ammonia water, KOH, tetramethylammonium hydroxide, tetraethylammonium hydroxide, and piperazine; And / or, the viscosity modifier is selected from one or more of hydroxypropyl starch, carboxymethyl starch, carboxyethyl starch, hydroxyethyl starch, hydroxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl cellulose.

8. A chemical mechanical polishing liquid, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the chemical mechanical polishing liquid according to claim 8 in chemical mechanical polishing of a wafer, wherein the wafer is a silicon wafer or a wafer with silicon as a substrate.

Citation Information

Patent Citations

  • Silicon fine polishing liquid capable of reducing particle contamination on surface of silicon wafer

    CN115851138A

  • Fine polishing liquid for reducing particle defects on surface of silicon wafer as well as preparation method and use method of fine polishing liquid

    CN116554788A

  • Monocrystalline silicon fine polishing liquid and preparation method thereof

    CN116948532A

  • Polishing liquid for reducing microscratch of surfaces of silicon wafers and preparation and use method thereof