A method for preparing a double-layer Cr coating with ultrafine needle-shaped crystals / nearly equiaxed crystals on the surface of a zirconium alloy cladding
The Cr coating with ultra-fine needle crystal/near equiaxed crystal double-layer structure is prepared by high-power pulse magnetron sputtering technology, which solves the problem of oxidation erosion of zirconium alloy cladding in high temperature environment and achieves the rapid formation of dense oxide film. And the effect of improving high temperature oxidation resistance.
Patent Information
- Application Number
- CN202410723535.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-05
AI Technical Summary
Zirconium alloy cladding is easily corroded by oxygen and water vapor in high temperature environments. The columnar crystal structure of traditional Cr coatings has a slow oxidation process, making it difficult to effectively protect the zirconium alloy matrix, resulting in the risk of serious accidents in nuclear reactors.
High-power pulse magnetron sputtering technology is used to prepare a Cr coating with an ultra-fine needle crystal/near equiaxed crystal double-layer structure. The crystal grains are formed by controlling parameters such as bias voltage, target distance, sputtering power, and argon gas flow rate. Nearly equiaxed crystals with a size of 0.1-0.5μm and ultra-fine needle-shaped crystals with an aspect ratio of 4-10μm ≥ 12 can quickly generate a dense Cr2O3 protective film.
Significantly shortens the formation time of the oxide film, improves the high-temperature oxidation resistance of the zirconium alloy cladding, can maintain the integrity of the oxide film after high-temperature oxidation in water vapor at 1300°C for 3000 seconds, and enhances the mechanical properties and wear resistance of the coating. Significantly improves the durability of the material.
Smart Images

Figure CN118422127B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nuclear fuel cladding surface coatings, and in particular relates to a method for preparing a Cr coating with an ultrafine needle-shaped crystal / nearly equiaxed crystal double-layer structure on the surface of a zirconium alloy cladding. Background Art
[0002] Zirconium alloys have been used stably in the field of water-cooled reactor nuclear fuel cladding materials and the nuclear industry for a long time due to their excellent corrosion resistance, low neutron absorption cross section, excellent mechanical properties and thermal conductivity. However, if the cooling system is damaged, the nuclear reactor loses its cooling capacity, causing the temperature to rise, triggering the melting of nuclear fuel and the generation of hydrogen, which can easily cause hydrogen explosion. Therefore, it is urgent to design a solution to improve the high-temperature oxidation resistance of zirconium alloys.
[0003] The preparation of anti-oxidation coating on the surface of zirconium alloy cladding has the advantages of short R&D cycle and low cost, showing great potential for engineering application. Metal Cr can generate denser and more protective Cr in oxidizing medium. 2 O 3 The Cr coating is a kind of coating with high compatibility with zirconium alloy matrix, so it has become one of the preferred materials for cladding surface coating. However, the grain size and morphology of Cr coating are difficult to control, and different grain structures lead to great differences in the formation speed of protective oxide film of Cr coating. Cr coating prepared by traditional physical vapor deposition technology usually has a columnar crystal structure, which is oxidized to form Cr in high temperature steam environment. 2 O 3 The process of oxidation is relatively slow, and the zirconium alloy matrix is easily corroded by oxygen and water vapor during this period. Therefore, it is urgent to provide a preparation method of Cr coating suitable for zirconium alloy, and to adjust the structure of Cr coating so that it forms Cr during high temperature oxidation. 2 O 3 The rate is accelerated, thereby effectively protecting the zirconium alloy fuel cladding and improving the cladding's ability to withstand severe accidents. Summary of the invention
[0004] In view of the problems existing in the above-mentioned prior art, the present invention proposes a method for preparing a Cr coating with an ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure on the surface of a zirconium alloy cladding.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A double-layer Cr coating with ultrafine needle-shaped crystals / near-equiaxed crystals on the surface of a zirconium alloy cladding, wherein the coating is formed by closely arranging an ultrafine needle-shaped crystal coating perpendicular to a zirconium alloy substrate, and the surface of the ultrafine needle-shaped crystal coating is a near-equiaxed crystal coating with a grain size of 0.1-0.5 μm; the grain length of the ultrafine needle-shaped crystal coating is 4-10 μm, the width is 0.1-0.5 μm, and the aspect ratio is ≥12:1; the overall thickness of the coating is 6.3-13 μm, of which the thickness of the ultrafine needle-shaped crystal coating is 6-11 μm, and the thickness of the near-equiaxed crystal coating is 0.3-2 μm.
[0007] The present invention also provides a method for preparing the ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure Cr coating on the surface of the zirconium alloy cladding, comprising the following steps:
[0008] The pretreated zirconium alloy substrate is subjected to target pre-sputtering treatment and argon plasma etching treatment, and then a Cr coating is sputtered to obtain the Cr coating with an ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure on the surface of the zirconium alloy cladding;
[0009] Among them, in the process of sputtering Cr coating, the ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure coating is obtained through the following strategy. In practical applications, the adjustment of one parameter will affect the change of all parameters. Therefore, it is not possible to obtain the target product by changing a single variable, but the overall coordination is required:
[0010] A. Adjust the bias voltage: When preparing ultrafine needle-shaped crystal coatings, adjust the bias voltage to -60 to -120V; when preparing surface near-equiaxed crystal coatings, adjust the bias voltage to -140V to -200V;
[0011] B. Adjust the target-substrate distance: when preparing ultrafine needle-shaped crystal coatings, the target-substrate distance is 10-18 cm; when preparing surface near-equiaxed crystal coatings, the target-substrate distance is 18-30 cm.
[0012] C. Regulate the sputtering power: when preparing ultrafine needle-shaped crystal coating, the sputtering power is 2500-3500W; when preparing surface near-equiaxed crystal coating, the sputtering power is 1500-2500W;
[0013] D. Regulating the argon flow rate and tube wall temperature in the tube: Control the argon flow rate into the tube to 5-50 sccm. Specifically, when preparing ultrafine needle-shaped crystal coatings, control the argon flow rate in the tube to 5-30 sccm to adjust the tube wall temperature to 280-400°C; when preparing surface near-equiaxed crystal coatings, control the argon flow rate to 30-50 sccm to adjust the tube wall temperature to 120-240°C.
[0014] Furthermore, the total deposition time of the coating is 6-18 hours. When sputtering the ultrafine needle-shaped crystal coating, the deposition time is 5.5-15 hours; when sputtering the near-equiaxed crystal coating, the deposition time is 0.5-3 hours.
[0015] Furthermore, the pretreatment method is: using 400#, 800#, 1200#, 2000#, 3000# and 4000# sandpaper to grind the surface of the zirconium alloy substrate in sequence, and then polishing it with 3μm, 1μm and 0.3μm diamond suspension in sequence; finally, immersing the sample in acetone solution for ultrasonic cleaning for 10-20 minutes, taking it out, drying it, and putting it in a vacuum box for standby use.
[0016] Furthermore, the parameters of the target pre-sputtering treatment are: the temperature of the magnetron sputtering chamber is 180-300°C, the chamber vacuum is 3-5×10 -4 Pa, high-purity argon gas is introduced to make the chamber pressure 0.6-1.2Pa, the power is 200-500W, and the sputtering time is 15-35min.
[0017] Furthermore, during the argon plasma etching process: temperature 200-350° C., argon gas flow rate 20-50 sccm, ion source current 0.5-2A, bias voltage -50 to -170V, etching time 15-30min.
[0018] Furthermore, in the process of sputtering the Cr coating: the sputtering gas pressure is 0.1-1.0 Pa, the pulse frequency is 200-500 Hz, the pulse width is 30-90 μs, the duty cycle is 2-5%, the deposition temperature is 120-400° C., and the deposition time is 6-18 h.
[0019] In the coating preparation process of the present invention, a high-power pulsed magnetron sputtering self-modification device (such as Figure 1 ), the device precisely controls the grain morphology and size of the plated pure Cr coating by adding an Ar flow rate control system in the zirconium alloy tube and a target-substrate distance dynamic adjustment system.
[0020] Compared with the prior art, the present invention has the following advantages and technical effects:
[0021] The present invention relates to a novel accident-resistant zirconium alloy cladding surface coating, the main component of which is pure chromium, and presents a double-layer structure of ultrafine needle-shaped crystals near the matrix and near-equiaxed crystals on the surface. The unique structure of the ultrafine needle-shaped crystals has the characteristics of high grain boundary density, and the grain boundaries are closely arranged perpendicular to the matrix, which accelerates the atomic diffusion rate and greatly shortens the time for the surface oxide film to form. The near-equiaxed crystal structure on the coating surface has the characteristics of uniform grain boundary distribution and extremely high grain boundary density. It is attached to the ultrafine needle-shaped crystal structure, which helps the sample surface to quickly form a uniform and dense Cr in the early stage of oxidation. 2 O 3Protective film. Based on this, this ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure coating can form a dense oxide film within 2-5 minutes, while the common columnar crystal structure Cr coating generally requires more than 10 minutes to form a dense oxide film, which can significantly delay the direct corrosion of oxygen and water vapor on the substrate at high temperature. After testing, the pure Cr ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure coating has excellent resistance to high-temperature oxidation. After high-temperature oxidation at 1300℃ water vapor for 3000s, the oxide film and residual Cr coating did not peel off after oxidation, the zirconium alloy matrix was not oxidized, and the Cr coating had good protection for the zirconium alloy matrix. At the same time, the ultrafine needle-shaped crystal structure near the matrix has superior mechanical properties, with high hardness and strength, which can improve the wear resistance of the coating and improve the durability of the material. The micromechanical properties of the sample were tested using a nanoindenter. After high-temperature oxidation at 1200℃ water vapor for 3600s, the surface Cr 2 O 3 The nano-hardness of the protective film can reach 5047MPa, and the nano-hardness of the residual Cr coating can reach 10056MPa, showing good hardness. The present invention also adjusts the bias voltage, target-substrate distance, sputtering power, Ar flow rate in the tube (tube wall temperature) and other parameters, and deposits different times to obtain ultrafine needle-shaped crystal coatings and near-equiaxed crystal coatings of different thicknesses. Considering the influence of the Cr coating on the circumferential and axial thermal expansion properties of the zirconium alloy tube, a too thick coating will increase the interface stress and cause cracking and other problems, while a too thin coating will not provide sufficient protection for the substrate. Therefore, the thickness of the ultrafine needle-shaped crystal coating and the near-equiaxed crystal coating is also limited in the present invention.
[0022] The present invention uses high-power pulsed magnetron sputtering technology to deposit a chromium coating with a thickness of 6.3-13μm on the surface of the Zr-4 alloy. By independently modifying the HiPIMS equipment, argon gas is introduced into the zirconium alloy cladding tube and the flow rate of argon gas in the tube is controlled (to control the tube wall temperature), and the bias voltage, target substrate distance, sputtering power and other parameters are comprehensively adjusted to obtain a pure Cr ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure coating. The ultrafine needle-shaped crystal coating has a grain length of 4-10μm, a width of 0.1-0.5μm, and an aspect ratio of ≥12:1. It is closely arranged vertically on the zirconium alloy substrate, has a large aspect ratio, and has a high grain boundary density; the surface near-equiaxed crystal grain size is 0.1-0.5μm, attached to the ultrafine needle-shaped crystal structure, with uniform grain boundary distribution and extremely high grain boundary density. The present invention dynamically controls the argon gas flow rate (controls the tube wall temperature), bias voltage, target-substrate distance and sputtering power in the sample tube during the sputtering process to control a certain Cr atom nucleation rate, coating deposition rate and cooling rate, so that the grains grow vertically to the substrate to obtain ultrafine needle-shaped crystals; by controlling the relevant parameters to obtain a sufficient temperature gradient to provide sufficient thermal supercooling, increase the Cr atom nucleation rate and promote atomic diffusion, and control the coating deposition rate and cooling rate at the same time, thereby inducing the formation of fine and dense near-equiaxed crystals on the surface of ultrafine needle-shaped crystals. When zirconium alloy is oxidized in a high temperature environment, Cr atoms will diffuse outward rapidly along the dense needle-shaped crystal boundaries and react with oxygen and water vapor in the environment. The reaction product Cr 2 O 3 It is quickly formed on the surface of fine and dense near-equiaxed crystals, generating a dense layer of Cr in a very short time. 2 O 3 The double-layer coating also exhibits excellent high-temperature oxidation resistance during service after the oxide film is formed.
[0023] The ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure Cr coating improves the high-temperature oxidation resistance of the zirconium alloy cladding and can significantly enhance the ability of the fuel cladding to resist severe reactor accidents. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0025] Figure 1 This is a schematic diagram of the self-modified equipment for high-power pulsed magnetron sputtering;
[0026] Figure 2 BC+IPF diagram of the zirconium alloy sample deposited with Cr coating prepared in Example 1;
[0027] Figure 3BC+IPF diagram of the zirconium alloy sample deposited with Cr coating prepared in Comparative Example 2;
[0028] Figure 4 This is a SEM image of the sample prepared in Example 4 after being oxidized under high-temperature steam conditions at 1200°C for 3600s;
[0029] Figure 5 This is a SEM image of the sample prepared in Comparative Example 4 after being oxidized under high-temperature steam conditions at 1200°C for 3600s. DETAILED DESCRIPTION
[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0031] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0032] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0033] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0035] The "room temperature" mentioned in the present invention is 20-30°C unless otherwise specified.
[0036] The present invention adopts high-power pulsed magnetron sputtering technology to deposit a chromium coating with a thickness of 6.3-13μm on the surface of Zr-4 alloy. By independently modifying the HiPIMS equipment, argon gas is introduced into the zirconium alloy cladding tube and the flow rate of argon gas in the tube is controlled, and the bias voltage, target substrate distance, sputtering power and other parameters are comprehensively adjusted to obtain a pure Cr ultrafine needle crystal / near equiaxed crystal double-layer structure coating. The ultrafine needle crystal coating has a grain length of 4-10μm, a width of 0.1-0.5μm, and an aspect ratio of ≥12:1. It is closely arranged vertically on the zirconium alloy substrate, and the surface is composed of a layer of fine and dense near equiaxed crystals with a grain size of 0.1-0.5μm. The overall thickness of the coating is 6.3-13μm, of which the thickness of the pure Cr ultrafine needle crystal coating is 6-11μm, and the thickness of the surface near equiaxed crystal is 0.3-2μm. When the pure Cr coating with ultrafine needle-shaped crystals / nearly equiaxed crystals double-layer structure designed by the present invention is oxidized in a high temperature environment, Cr atoms will diffuse outward rapidly along the dense needle-shaped crystal boundaries and react with oxygen and water vapor in the environment. The reaction product Cr 2 O 3 It is quickly formed on the surface of fine and dense near-equiaxed crystals, generating a dense layer of Cr in a very short time. 2 O 3 The double-layer coating also exhibits excellent high-temperature oxidation resistance during service after the oxide film is formed.
[0037] The specific technical solution is: a double-layer Cr coating with ultrafine needle-shaped crystals / near equiaxed crystals on the surface of a zirconium alloy cladding, wherein the ultrafine needle-shaped crystals of the coating have a grain length of 4-10 μm, a width of 0.1-0.5 μm, and an aspect ratio of ≥12:1, and are closely arranged vertically on the zirconium alloy matrix; the surface is a layer of fine and dense near equiaxed crystals with a grain size of 0.1-0.5 μm. The overall thickness of the coating is 6.3-13 μm, of which the thickness of the pure Cr ultrafine needle-shaped crystal coating is 6-11 μm, and the thickness of the surface near equiaxed crystals is 0.3-2 μm.
[0038] The pure Cr ultrafine needle-shaped crystal / near equiaxed crystal double-layer structure coating can quickly form a dense Cr layer on the surface when oxidized in a high temperature environment. 2 O 3 , which greatly shortens the time for oxide film formation and prevents the zirconium alloy from being oxidized and corroded during the process. At the same time, the ultrafine needle-shaped crystal structure has superior mechanical properties, high hardness and strength, which can improve the wear resistance of the coating and the durability of the material. In addition, considering the influence of the Cr coating thickness on the circumferential and axial thermal expansion properties of the zirconium alloy pipe, and the influence of the Cr coating thickness on the protective ability of the substrate, the present invention limits the thickness of the ultrafine needle-shaped crystal coating and the near-equiaxed crystal coating respectively.
[0039] The present invention also provides a method for preparing the ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure Cr coating on the surface of the zirconium alloy cladding, which is plated on the base material by a high-power pulsed magnetron sputtering process, comprising the following steps:
[0040] 1) Matrix pretreatment: prepare a Zr-4 alloy tube with the following dimensions: outer diameter 8.5-10.5 mm, thickness 0.45-0.65 mm, length 10-25 cm, composition of Zr 98.0-98.5%, Sn 1.0-2.0%, Fe 0.2-0.3%, Cr 0.1-0.2%; polish the sample surface with 400#, 800#, 1200#, 2000#, 3000# and 4000# sandpaper in turn; then polish with 3μm, 1μm and 0.3μm diamond suspension; finally, soak the sample in acetone solution and ultrasonically clean it for 10-20 min, take it out, dry it and put it in a vacuum box for standby use;
[0041] 2) Substrate installation and target pre-sputtering treatment: Fix the pre-treated sample on the sample stage of the magnetron sputtering chamber, heat the magnetron sputtering chamber to 180-300°C, and evacuate the chamber to 3-5×10 -4 P a, high-purity argon gas is introduced into the chamber of the magnetron sputtering instrument until the chamber pressure is 0.6-1.2 Pa, and the Cr target is pre-sputtered for 15-35 minutes at a power of 200-500 W;
[0042] 3) Argon plasma etching: etching for 15-30 minutes at a temperature of 200-350°C, an argon gas flow rate of 20-50 sccm, an ion source current of 0.5-2A, and a bias voltage of -50 to -170V;
[0043] 4) Sputtering Cr coating: Turn on the high-power pulse sputtering power supply, control the sputtering gas pressure to 0.1-1.0Pa, the pulse frequency to 200-500Hz, the pulse width to 30-90μs, and the duty cycle to 2-5%. Dynamically control the following parameters: bias voltage -60~-200V, target-substrate distance to 10-30cm, sputtering power to 1500-3500W, control the Ar gas flow rate in the tube to 5-50sccm, deposition temperature to 120-400℃, deposition time for each layer of coating to 0.5-15h, total deposition time to 6-18h, thickness of each layer of coating to 0.3-11μm, and total coating thickness to 6.3-13μm. In order to control the grain size and thickness of the ultrafine needle-shaped crystal layer and the nearly equiaxed crystal layer coating, specifically:
[0044] a. Sputtering ultrafine needle-shaped crystal coating: control bias voltage -60~-120V, target-substrate distance 10-18cm, sputtering power 2500-3500W, through infrared temperature meter-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 5-30sccm, so that the outer wall temperature of the tube (ie, deposition temperature) is maintained at 280-400℃, and the deposition time is 5.5-15h to obtain ultrafine needle-shaped crystal coating;
[0045] b. Sputtering near-equiaxed crystal coating: control the bias voltage at -140 to -200 V, the target-substrate distance at 18 to 30 cm, the sputtering power at 1500 to 2500 W, and through the infrared temperature sensor-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of the Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 30 to 50 sccm, so that the temperature of the outer wall of the tube (i.e., the deposition temperature) is maintained at 120 to 240 ° C, and the deposition time is 0.5 to 3 hours to obtain a near-equiaxed crystal coating.
[0046] In order to obtain a coating with specified grain morphology, grain size and thickness, the present invention strictly controls the range of parameter values such as bias voltage, target substrate distance, sputtering power and Ar gas flow rate in the tube (deposition temperature), so as to obtain the required ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure characteristic organization of a certain thickness.
[0047] The raw materials used in the following examples of the present invention are all commercially available.
[0048] The following examples serve as further illustrations of the technical solutions of the present invention.
[0049] Example 1
[0050] A method for preparing a double-layer Cr coating with ultrafine needle-shaped crystals / near-equiaxed crystals on the surface of a zirconium alloy cladding comprises the following steps:
[0051] 1) Matrix pretreatment: Prepare a Zr-4 alloy tube with the following dimensions: outer diameter 9.5 mm, thickness 0.57 mm, length 20 cm, composition of Zr 98.5%, Sn 1.15%, Fe 0.23%, Cr 0.12%; polish the sample surface with 400#, 800#, 1200#, 2000#, 3000# and 4000# sandpaper in turn; then polish with 3μm, 1μm and 0.3μm diamond suspension; finally, soak the sample in acetone solution and ultrasonically clean it for 15 min, take it out, dry it, and put it in a vacuum box for standby use;
[0052] 2) Substrate installation and target pre-sputtering treatment: The pre-treated sample is fixed on the sample stage of the magnetron sputtering chamber, the magnetron sputtering chamber is heated to 280°C, and the chamber is vacuumed to 4×10 -4Pa, high-purity argon gas was introduced into the chamber of the magnetron sputtering instrument until the chamber pressure was 1.0 Pa, and the Cr target was pre-sputtered for 20 min at a power of 350 W;
[0053] 3) Argon plasma etching treatment: etching for 20 min at a temperature of 300°C, an argon gas flow rate of 40 sccm, an ion source current of 1.2 A, and a bias voltage of -110 V;
[0054] 4) Sputtering Cr coating: Turn on the high-power pulse sputtering power supply, control the sputtering gas pressure to 0.6Pa, the pulse frequency to 350Hz, the pulse width to 60μs, and the duty cycle to 3%. Dynamically control the following parameters: bias voltage -60~-200V, target substrate distance 10-30cm, sputtering power 1500-3500W, control the Ar gas flow rate in the tube to 5-50sccm, deposition temperature 120-400℃, deposition time for each layer of coating 0.5-15h, total deposition time 6-18h, thickness of each layer of coating 0.3-11μm, total coating thickness 6.3-13μm. The specific steps are as follows:
[0055] a. Sputtering ultrafine needle-shaped crystal coating: control bias voltage -90V, target-substrate distance 15cm, sputtering power 3000W, through infrared temperature meter-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 5-30sccm, so that the outer wall temperature of the tube (i.e., deposition temperature) is maintained at 320-330℃, and the deposition is carried out for 10h to obtain ultrafine needle-shaped crystal structure;
[0056] b. Sputtering near-equiaxed crystal coating: control the bias voltage to -150V, control the connecting rod through the servo motor, slowly move the Cr target within 3 minutes so that the target-substrate distance becomes 22cm, and control the sputtering power to 2000W. Through the infrared temperature sensor-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of the Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 30-50sccm, so that the temperature of the outer wall of the tube (i.e., the deposition temperature) is maintained at 180-190℃, and the deposition is carried out for 1h to obtain a near-equiaxed crystal structure.
[0057] The total deposition time of this embodiment is 11 hours, and a zirconium alloy sample with a Cr coating is obtained. After testing, the total thickness of the coating is 9.8μm, of which the thickness of the ultrafine needle-shaped crystal coating is 8.7μm and the thickness of the near-equiaxed crystal coating is 1.1μm. The average grain length of the ultrafine needle-shaped crystal coating is 7.2μm, the width is 0.26μm, and the aspect ratio is 27.7; the average grain size of the near-equiaxed crystal coating is 0.38μm.
[0058] Figure 2This is the BC+IPF diagram of the zirconium alloy sample deposited with Cr coating prepared in Example 1. It can be seen from the figure that the coating grains are ultrafine needle-shaped and nearly equiaxed, respectively, and are divided into two layers. The overall thickness of the coating is uniform and the surface is flat; the film-base bonding force is strong, and the coating is not easy to peel off.
[0059] Example 2
[0060] A method for preparing a double-layer Cr coating with ultrafine needle-shaped crystals / near-equiaxed crystals on the surface of a zirconium alloy cladding comprises the following steps:
[0061] 1) Matrix pretreatment: Prepare a Zr-4 alloy tube with the following dimensions: outer diameter 9.5 mm, thickness 0.57 mm, length 20 cm, composition of Zr 98.5%, Sn 1.15%, Fe 0.23%, Cr 0.12%; polish the sample surface with 400#, 800#, 1200#, 2000#, 3000# and 4000# sandpaper in turn; then polish with 3μm, 1μm and 0.3μm diamond suspension; finally, soak the sample in acetone solution and ultrasonically clean it for 20 min, take it out, dry it, and put it in a vacuum box for standby use;
[0062] 2) Substrate installation and target pre-sputtering treatment: The pre-treated sample is fixed on the sample stage of the magnetron sputtering chamber, the magnetron sputtering chamber is heated to 250°C, and the chamber is vacuumed to 4×10 -4 Pa, high-purity argon gas was introduced into the chamber of the magnetron sputtering instrument until the chamber pressure was 0.9 Pa, and the Cr target was pre-sputtered for 25 min at a power of 400 W;
[0063] 3) Argon plasma etching treatment: etching for 15 min at a temperature of 280°C, an argon gas flow rate of 30 sccm, an ion source current of 1.4 A, and a bias voltage of -120 V;
[0064] 4) Sputtering Cr coating: Turn on the high-power pulse sputtering power supply, control the sputtering gas pressure to 0.8Pa, the pulse frequency to 380Hz, the pulse width to 50μs, and the duty cycle to 2%. Dynamically control the following parameters: bias voltage -60~-200V, target substrate distance 10-30cm, sputtering power 1500-3500W, control the Ar gas flow rate in the tube to 5-50sccm, deposition temperature 120-400℃, deposition time for each layer of coating 0.5-15h, total deposition time 6-18h, thickness of each layer of coating 0.3-11μm, total coating thickness 6.3-13μm. The specific steps are as follows:
[0065] a. Sputtering ultrafine needle-shaped crystal coating: control bias voltage -110V, target-substrate distance 14cm, sputtering power 2800W, through infrared temperature meter-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 5-30sccm, so that the outer wall temperature of the tube (i.e., deposition temperature) is maintained at 305-315℃, and the deposition is carried out for 12h to obtain ultrafine needle-shaped crystal structure;
[0066] b. Sputtering of near-equiaxed crystal coating: control the bias voltage to -170V, control the connecting rod through the servo motor, slowly move the Cr target within 3 minutes so that the target-substrate distance becomes 24cm, and control the sputtering power to 1800W. Through the infrared temperature sensor-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of the Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 30-50sccm, so that the temperature of the outer wall of the tube (i.e., the deposition temperature) is maintained at 170-180℃, and the deposition is 1.5h to obtain a near-equiaxed crystal structure.
[0067] The total deposition time of this embodiment is 13.5h, and a zirconium alloy sample with a Cr coating is obtained. After testing, the total thickness of the coating is 10.8μm, of which the thickness of the ultrafine needle-shaped crystal coating is 9.5μm and the thickness of the near-equiaxed crystal coating is 1.3μm. The average grain length of the ultrafine needle-shaped crystal coating is 5.7μm, the width is 0.18μm, the aspect ratio is 31.7, and the average grain size of the near-equiaxed crystal coating is 0.29μm.
[0068] Example 3
[0069] A method for preparing a double-layer Cr coating with ultrafine needle-shaped crystals / near-equiaxed crystals on the surface of a zirconium alloy cladding comprises the following steps:
[0070] 1) Matrix pretreatment: prepare a Zr-4 alloy tube with the following dimensions: outer diameter 9.5 mm, thickness 0.57 mm, length 20 cm, composition of Zr98.5%, Sn1.15%, Fe0.23%, Cr0.12%; polish the sample surface with 400#, 800#, 1200#, 2000#, 3000# and 4000# sandpaper in turn; then polish with 3μm, 1μm and 0.3μm diamond suspension; finally, soak the sample in acetone solution and ultrasonically clean it for 20 min, take it out, dry it and put it in a vacuum box for standby use;
[0071] 2) Substrate installation and target pre-sputtering treatment: The pre-treated sample is fixed on the sample stage of the magnetron sputtering chamber, the magnetron sputtering chamber is heated to 300°C, and the chamber is vacuumed to 4×10 -4 Pa, high-purity argon gas was introduced into the chamber of the magnetron sputtering instrument until the chamber pressure was 0.8 Pa, and the Cr target was pre-sputtered for 30 min at a power of 280 W;
[0072] 3) Argon plasma etching treatment: etching for 25 min at a temperature of 250° C., an argon gas flow rate of 35 sccm, an ion source current of 1.0 A, and a bias voltage of -90 V;
[0073] 4) Sputtering Cr coating: Turn on the high-power pulse sputtering power supply, control the sputtering gas pressure to 0.5Pa, the pulse frequency to 300Hz, the pulse width to 40μs, and the duty cycle to 2%. Dynamically control the following parameters: bias voltage -60~-200V, target substrate distance 10-30cm, sputtering power 1500-3500W, control the Ar gas flow rate in the tube to 5-50sccm, deposition temperature 120-400℃, deposition time for each layer of coating 0.5-15h, total deposition time 6-18h, thickness of each layer of coating 0.3-11μm, total coating thickness 6.3-13μm. The specific steps are as follows:
[0074] a. Sputtering ultrafine needle-shaped crystal coating: control bias voltage -60V, target substrate distance 13cm, sputtering power 3200W, through infrared temperature meter-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 5-30sccm, so that the outer wall temperature of the tube (i.e., deposition temperature) is maintained at 355-365℃, and the deposition is 8h to obtain ultrafine needle-shaped crystal structure;
[0075] b. Sputtering of near-equiaxed crystal coating: control the bias voltage to -190V, control the connecting rod through the servo motor, slowly move the Cr target within 3 minutes so that the target-substrate distance becomes 23cm, and control the sputtering power to 2200W. Through the infrared temperature sensor-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of the Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 30-50sccm, so that the temperature of the outer wall of the tube (i.e., the deposition temperature) is maintained at 150-160℃, and the deposition is carried out for 0.5h to obtain a near-equiaxed crystal structure.
[0076] The total deposition time of this embodiment is 8.5h, and a zirconium alloy sample with a Cr coating is obtained. After testing, the total thickness of the coating is 8.6μm, of which the thickness of the ultrafine needle-shaped crystal coating is 8.2μm and the thickness of the nearly equiaxed crystal coating is 0.4μm. The average grain length of the ultrafine needle-shaped crystal coating is 7.7μm, the width is 0.32μm, the aspect ratio is 24.1, and the average grain size of the nearly equiaxed crystal coating is 0.32μm.
[0077] Example 4
[0078] A method for preparing a double-layer Cr coating with ultrafine needle-shaped crystals / near-equiaxed crystals on the surface of a zirconium alloy cladding comprises the following steps:
[0079] 1) Matrix pretreatment: Prepare a Zr-4 alloy tube with the following dimensions: outer diameter 9.5 mm, thickness 0.57 mm, length 20 cm, composition of Zr 98.5%, Sn 1.15%, Fe 0.23%, Cr 0.12%; polish the sample surface with 400#, 800#, 1200#, 2000#, 3000# and 4000# sandpaper in turn; then polish with 3μm, 1μm and 0.3μm diamond suspension; finally, soak the sample in acetone solution and ultrasonically clean it for 20 min, take it out, dry it, and put it in a vacuum box for standby use;
[0080] 2) Substrate installation and target pre-sputtering treatment: The pre-treated sample is fixed on the sample stage of the magnetron sputtering chamber, the magnetron sputtering chamber is heated to 220°C, and the chamber is vacuumed to 4×10 -4 Pa, high-purity argon gas was introduced into the chamber of the magnetron sputtering instrument until the chamber pressure was 1.1 Pa, and the Cr target was pre-sputtered for 20 min at a power of 250 W;
[0081] 3) Argon plasma etching treatment: etching for 15 min at a temperature of 320°C, an argon gas flow rate of 45 sccm, an ion source current of 1.2 A, and a bias voltage of -120 V;
[0082] 4) Sputtering Cr coating: Turn on the high-power pulse sputtering power supply, control the sputtering gas pressure to 0.5Pa, the pulse frequency to 300Hz, the pulse width to 80μs, and the duty cycle to 2%. Dynamically control the following parameters: bias voltage -60~-200V, target substrate distance 10-30cm, sputtering power 1500-3500W, control the Ar gas flow rate in the tube to 5-50sccm, deposition temperature 120-400℃, deposition time for each layer of coating 0.5-15h, total deposition time 6-18h, thickness of each layer of coating 0.3-11μm, total coating thickness 6.3-13μm. The specific steps are as follows:
[0083] a. Sputtering ultrafine needle-shaped crystal coating: control bias voltage -80V, target substrate distance 12cm, sputtering power 3300W, through infrared temperature detector-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 5-30sccm, so that the outer wall temperature of the tube (i.e., deposition temperature) is maintained at 325-335℃, and the deposition is carried out for 13h to obtain ultrafine needle-shaped crystal structure;
[0084] b. Sputtering of near-equiaxed crystal coating: control the bias voltage to -140V, control the connecting rod through the servo motor, slowly move the Cr target within 3 minutes so that the target-substrate distance becomes 20cm, and control the sputtering power to 2300W. Through the infrared temperature sensor-Ar gas flow rate controller system, according to the real-time temperature monitoring data of the outer wall of the Zr-4 alloy tube, actively and dynamically adjust the Ar flow rate in the tube at 30-50sccm, so that the temperature of the outer wall of the tube (i.e., the deposition temperature) is maintained at 200-210℃, and the deposition is carried out for 2.5 hours to obtain a near-equiaxed crystal structure.
[0085] The total deposition time of this embodiment is 15.5h, and a zirconium alloy sample with a Cr coating is obtained. After testing, the total thickness of the coating is 12.2μm, of which the thickness of the ultrafine needle-shaped crystal coating is 10.5μm and the thickness of the near-equiaxed crystal coating is 1.7μm. The average grain length of the ultrafine needle-shaped crystal coating is 9.2μm, the width is 0.15μm, the aspect ratio is 61.3, and the average grain size of the near-equiaxed crystal coating is 0.46μm.
[0086] Comparative Example 1
[0087] Same as Example 1, except that the bias voltages of the sputtered ultrafine needle-shaped crystal coating and the near-equiaxed crystal coating in step 4) are -50V and -100V respectively, and the other parameters are consistent with Example 1. The grain morphology of the obtained coating tends to be a coarse columnar crystal structure, and the coating cracks, which does not meet the requirements. The coarse columnar crystal structure of the coating reduces the grain boundary density, which is not conducive to the rapid formation of a protective oxide layer in an oxidizing environment or a corrosive environment, and easily causes material failure. In addition, the coating sample has lost the characteristics of ultrafine needle-shaped crystals and near-equiaxed crystals, which does not meet the requirements.
[0088] Comparative Example 2
[0089] Same as Example 2, except that the target-substrate distances of the sputtering ultrafine needle-shaped crystal coating and the near-equiaxed crystal coating in step 4) are 9 cm and 23 cm respectively, and the other parameters are the same as those in Example 2. Figure 3 As shown in the figure, the average grain length of the coating on the side of the zirconium alloy substrate is 5.6μm, the width is 0.7μm, the aspect ratio is 8, and the ultrafine needle-shaped crystal structure characteristics are lost; the average grain size of the near-equiaxed crystal coating is 0.33μm, but the surface near-equiaxed crystal coating is discontinuous, and it is difficult to quickly form a continuous protective Cr in an oxidizing environment or a corrosive environment. 2 O 3 Oxide film reduces the protection of the sample.
[0090] Comparative Example 3
[0091] The same as Example 3, except that in step 4), the sputtering powers of the ultrafine needle-shaped crystal coating and the near-equiaxed crystal coating are 2000 W and 1300 W respectively, and the other parameters are consistent with Example 3. The obtained near-zirconium alloy substrate side coating has an average grain length of 6.7 μm, a width of 2.5 μm, an aspect ratio of 2.7, and an average grain size of the near-equiaxed crystal coating is 0.78 μm, which does not meet the requirements.
[0092] Comparative Example 4
[0093] The same as Example 4, except that in step 4), the Ar gas flow rates in the tube for sputtering the ultrafine needle-shaped crystal coating and the near-equiaxed crystal coating are 40-60 sccm and 15-35 sccm respectively, and the deposition temperatures are controlled to be 255-265°C and 240-250°C respectively. The other parameters are consistent with Example 4. The obtained coating on the side of the zirconium alloy substrate has an average grain length of 3.7 μm, a width of 1.8 μm, an aspect ratio of 2.1, and an average grain size of the near-equiaxed crystal coating is 1.93 μm, which does not meet the requirements.
[0094] Performance Testing:
[0095] The zirconium alloy samples deposited with Cr coatings prepared in Example 4 and Comparative Example 4 were subjected to high temperature steam oxidation tests, the method being:
[0096] The high-temperature steam oxidation test was carried out in a horizontal tube furnace equipped with a steam generator. The temperature was raised from room temperature to the specified temperature of 1200°C at a heating rate of 10°C / min, and flowing Ar gas (purity of 99.999%) was introduced during the heating process to protect the sample from initial oxidation. When the expected temperature was reached, flowing steam was introduced into the tube at a rate of 2g / min, and once the steam flow was stable, the sample was placed in the center of the furnace. All samples were kept at 1200°C for 3600s and then air-cooled to room temperature.
[0097] The results show that the zirconium alloy sample with Cr coating in Example 4 has excellent resistance to high temperature steam oxidation. 2 O 3 The thickness is thinner and more uniform, and there is no peeling of oxide film and residual Cr coating after oxidation, and there is no debonding at the coating-substrate interface.
[0098] Figure 4 This is a SEM image of the sample prepared in Example 4 after being oxidized under high-temperature steam at 1200°C for 3600s. 2 O 3 Thickness 3.91μm, residual Cr thickness 9.54μm, Cr 2 O 3The protective layer is formed quickly, and the residual Cr coating is thick. The coating thickness is dense and uniform, without cracks, holes, or peeling, and the coating has good protection for the zirconium alloy substrate.
[0099] Figure 5 This is the SEM picture of the sample prepared in Comparative Example 4 after being oxidized for 3600s under high temperature steam conditions at 1200℃. As can be seen from the figure, due to the loss of ultrafine needle-shaped crystals and fine and dense near-equiaxed crystal characteristics, the grains are coarse and the grain boundary density is reduced, resulting in Cr 2 O 3 The formation speed is slow, and the coating is loose and porous after oxidation. Microcracks appear in the coating and the substrate, and "bulging" occurs inside the substrate. The substrate is oxidized in some areas, and some coatings are debonded from the substrate, and the coating loses its protective properties for the zirconium alloy substrate.
[0100] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A zirconium alloy cladding surface ultrafine needle crystal / near equiaxed crystal double-layer structure Cr coating, characterized in that: The coating is formed by closely arranging an ultrafine needle-shaped crystal coating vertically on a zirconium alloy substrate, and the surface of the ultrafine needle-shaped crystal coating is a nearly equiaxed crystal coating with a grain size of 0.1-0.5 μm; The ultrafine needle-shaped crystal coating has a grain length of 4-10 μm, a width of 0.1-0.5 μm, and an aspect ratio of ≥12:1; the overall coating thickness is 6.3-13 μm, of which the ultrafine needle-shaped crystal coating thickness is 6-11 μm and the nearly equiaxed crystal coating thickness is 0.3-2 μm.
2. A method for preparing the ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure Cr coating on the surface of the zirconium alloy cladding as claimed in claim 1, characterized in that: The following steps are involved: The pretreated zirconium alloy substrate is subjected to target pre-sputtering treatment and argon plasma etching treatment, and then a Cr coating is sputtered to obtain the Cr coating with an ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure on the surface of the zirconium alloy cladding; Among them, in the process of sputtering Cr coating, the ultrafine needle-shaped crystal / near equiaxed crystal double-layer structure Cr coating is obtained by the following strategy: A. Regulate the bias voltage: when preparing ultrafine needle-shaped crystal coatings, control the bias voltage to -60 to -120 V; when preparing surface near-equiaxed crystal coatings, control the bias voltage to -140 to -200 V; B. Regulating the target-substrate distance: When preparing ultrafine needle-shaped crystal coatings, the target-substrate distance is controlled to be 10-18 cm, and when preparing surface near-equiaxed crystal coatings, the target-substrate distance is controlled to be 18-30 cm; C. Regulate the sputtering power: when preparing ultrafine needle-shaped crystal coating, control the sputtering power to 2500-3500W; when preparing surface near-equiaxed crystal coating, control the sputtering power to 1500-2500W; D. Regulate the argon flow rate and wall temperature in the tube: When preparing ultrafine needle-shaped crystal coatings, the argon flow rate in the tube is controlled to 5-30 sccm to adjust the wall temperature to 280-400°C; when preparing surface near-equiaxed crystal coatings, the argon flow rate is controlled to 30-50 sccm to adjust the wall temperature to 120-240°C.
3. The preparation method according to claim 2, characterized in that: When sputtering ultrafine needle-shaped crystal coatings, the deposition time is 5.5-15 hours; when sputtering near-equiaxed crystal coatings, the deposition time is 0.5-3 hours.
4. The preparation method according to claim 2, characterized in that: The pretreatment method is: using 400#, 800#, 1200#, 2000#, 3000#, and 4000# sandpaper to grind the sample surface in sequence; then polishing with 3μm, 1μm, and 0.3μm diamond suspension; then, immersing the sample in acetone for ultrasonic cleaning for 10-20 minutes, taking it out, drying it, and putting it in a vacuum box for standby use.
5. The preparation method according to claim 2, characterized in that: During the target pre-sputtering process, the temperature of the magnetron sputtering chamber is 180-300°C, and the vacuum of the chamber is 3-5×10 -4 Pa, high-purity argon gas is introduced to make the chamber pressure 0.6-1.2Pa, the power is 200-500W, and the sputtering time is 15-35min.
6. The preparation method according to claim 2, characterized in that: During the argon plasma etching process: temperature 200-350° C., argon gas flow rate 20-50 sccm, ion source current 0.5-2A, bias voltage -50 to -170V, etching time 15-30min.
7. The preparation method according to claim 2, characterized in that: In the sputtering Cr coating process: the sputtering gas pressure is 0.1-1.0 Pa, the pulse frequency is 200-500 Hz, the pulse width is 30-90 μs, the duty cycle is 2-5%, the deposition temperature is 120-400° C., and the deposition time is 6-18 hours.
8. Use of the ultrafine needle-shaped crystal / near-equiaxed crystal double-layer structure Cr coating on the surface of the zirconium alloy cladding as claimed in claim 1 in improving the high-temperature service performance of the zirconium alloy cladding tube.