Negative electrode materials, preparation methods and applications

By adsorbing and decomposing silicon source gas on the porous substrate and forming a carbon cladding layer, the problem of volume expansion of silicon negative electrode material during lithium-embedded deliquency is solved, and the circulation performance and electrochemical stability of the negative electrode material are improved, so as to achieve Excellent cycle stability and high capacity of lithium-ion batteries.

CN118431452BActive Publication Date: 2024-11-05CARBON ONE NEW ENERGY GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410889616.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-05
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

As the negative electrode material, the volume expansion and contraction of silicon during the lithium-embedded deliquification process, resulting in the material powdering and falling off, affecting the electrochemical performance. The current silicon-carbon composite method has poor circulation performance.

Method used

Using a porous substrate as a carrier, the silicon source gas is adsorbed and decomposed through low-temperature adsorption and high-temperature pyrolysis steps to form nanosilicon particles, and a carbon cladding layer is formed in the pore structure, and the silicon element is distributed in the pores of the porous substrate to reduce floating silicon Content, volume expansion is suppressed by the porous structure of the porous substrate.

Benefits of technology

The cycling performance of the negative electrode material is improved, the electrochemical stability and conductivity are enhanced, and the cycling stability of lithium-ion batteries and the first-time Coulomb efficiency are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118431452B_ABST
    Figure CN118431452B_ABST
Patent Text Reader

Abstract

The present invention discloses anode materials, preparation methods and applications, and relates to the technical field of secondary battery anode materials. The anode materials include a porous substrate, silicon elements distributed in the pores of the porous substrate, and carbon coated on the surface of the porous substrate. The silicon content in the anode material is 30wt%-80wt%, the resistivity is less than 5Ω·cm, and the value of W is greater than 8, wherein W=silicon content / resistivity, the unit of silicon content is wt%, and the unit of resistivity is Ω·cm. The anode material in the present invention distributes silicon in the pores of the porous substrate, and utilizes the pore structure of the porous substrate to suppress the volume expansion of silicon during lithium insertion and extraction, thereby improving the cycle performance of the anode material. In the preparation method of the anode material in the present invention, a silicon source is first adsorbed in the cavities of the porous substrate; then the temperature in the furnace is increased to decompose silane in the cavities, and nano-silicon particles are deposited in the cavities, thereby reducing the content of floating silicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary battery negative electrode materials, and in particular to negative electrode materials, preparation methods and applications. Background Art

[0002] Silicon is currently the negative electrode material with the largest theoretical capacity, with a specific capacity of up to 4200mAh / g, which is much higher than the theoretical capacity of graphite (the theoretical capacity of graphite-based negative electrode materials is only 372mAh / g). Silicon has the advantages of low lithium insertion potential and low cost, and is expected to replace graphite as the next generation of lithium-ion battery negative electrode material. However, as a negative electrode material, silicon is accompanied by severe volume expansion and contraction during the lithium insertion and de-lithiation process, which makes the material easy to pulverize, fall off the current collector and lose its electrochemical performance.

[0003] Due to the structural stability of carbon materials, the volume change during charging and discharging is relatively small, and it has good cycle stability. In addition, due to the similar chemical properties to silicon, silicon and carbon are often compounded to achieve the purpose of improving the volume expansion effect of silicon and improving its electrochemical stability. However, the negative electrode materials obtained by the existing silicon-carbon composite method have poor cycle performance.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a negative electrode material, a preparation method and an application thereof, so as to improve the cycle performance of the negative electrode material.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a negative electrode material, comprising a porous substrate, silicon elements distributed in the pores of the porous substrate, and carbon coated on the surface of the porous substrate, wherein the silicon content in the negative electrode material is 30wt%-80wt%, the resistivity is less than 5Ω·cm, and the value of W is greater than 8, wherein W=silicon content / resistivity, the unit of silicon content is wt%, and the unit of resistivity is Ω·cm.

[0008] In an optional embodiment, the specific surface area of ​​the negative electrode material is 4m 2 / g-9m 2 / g;

[0009] And / or, the D50 of the negative electrode material is 1 μm-15 μm;

[0010] And / or, the tap density of the negative electrode material is 0.7 g / cm 3 -1.5g / cm 3 .

[0011] In a second aspect, the present invention further provides a method for preparing the negative electrode material according to any one of the aforementioned embodiments, comprising:

[0012] Low temperature adsorption, placing the porous substrate in an environment containing a silicon source gas and adsorbing the silicon source gas;

[0013] High-temperature pyrolysis, heating the porous substrate adsorbing the silicon source gas to decompose the silicon source gas, thereby obtaining a porous substrate with nano-silicon loaded in the pore structure;

[0014] The coating treatment forms a carbon coating layer on the porous substrate loaded with nano-silicon in the pore structure to obtain the negative electrode material.

[0015] In an optional embodiment, the low-temperature adsorption step is performed in a low-temperature adsorption device, and during the low-temperature adsorption, when the silicon source gas is discharged from the tail gas outlet of the low-temperature adsorption device, the low-temperature adsorption step ends;

[0016] Optionally, the low temperature adsorption temperature is 25°C-200°C, the pressure is 0.0001KPa-0.3KPa, and the time is 1h-30h; more preferably, the low temperature adsorption temperature is 30°C-150°C, the pressure is 0.001KPa-0.1KPa, and the time is 2h-25h;

[0017] Optionally, the silicon source is selected from at least one of monosilane, disilane, dichlorosilane and trichlorosilane;

[0018] Optionally, the silicon source-containing gas further comprises an inert gas, wherein the volume fraction of the silicon source is 50 vol%-99 vol%.

[0019] In an optional embodiment, the high-temperature pyrolysis step is performed in a high-temperature pyrolysis device. During the high-temperature pyrolysis, when the exhaust gas from the tail gas outlet of the high-temperature pyrolysis device does not contain hydrogen, the high-temperature pyrolysis step ends;

[0020] Optionally, the high temperature pyrolysis temperature is 300°C-800°C, the pressure is 0.01Kpa-5Kpa, and the time is 1h-50h; more preferably, the high temperature pyrolysis temperature is 400°C-700°C, the pressure is 0.01Kpa-3KPa, and the time is 1h-40h;

[0021] In an optional embodiment, the porous substrate satisfies at least one of the following AG:

[0022] A. SPAN value <1.5;

[0023] B. Dv50 is 2μm-20μm

[0024] C. The specific surface area of ​​the porous substrate is 400 m 2 / g-2000m 2 / g, optionally 900m 2 / g-2000m2 / g;

[0025] D. Average pore size is 1.2nm-7.0nm, optionally 1.5nm-5.0nm;

[0026] E. Pore volume is 0.3 cm 3 / g-2.0cm 3 / g, optionally 0.5cm 3 / g-1.8cm 3 / g;

[0027] F, pore size concentration is 0.3-6.0, calculated as (P V 90-P V 10) / P V 50, optionally 0.3-8:

[0028] G. The porous substrate is selected from at least one of porous carbon, porous metal oxide, coordination polymer, porous metal and porous ceramic, and is optionally porous carbon.

[0029] In an optional embodiment, the coating treatment includes passing a carbon-containing gas source into a reactor in which the porous substrate loaded with nano-silicon is placed in the pore structure to perform carbon deposition to form a carbon coating layer;

[0030] Optionally, the temperature of carbon deposition is 300°C-1300°C, and the carbon deposition time is 1h-10h; Optionally, the temperature of carbon deposition is 400°C-1000°C, more preferably 400°C-600°C;

[0031] Optionally, the carbon-containing gas source includes a carbon source gas, and the carbon source gas is selected from an alkane gas having a cracking temperature within the carbon deposition temperature range;

[0032] Optionally, the carbon-containing gas source further comprises an inert gas;

[0033] Optionally, the carbon source gas volume fraction in the carbon-containing source gas is 50 vol%-99 vol%;

[0034] In a third aspect, the present invention further provides a negative electrode plate, comprising the negative electrode material described in any one of the aforementioned embodiments or the negative electrode material prepared by the method of any one of the aforementioned embodiments.

[0035] In a fourth aspect, the present invention further provides a secondary battery, comprising the negative electrode sheet described in the aforementioned embodiment.

[0036] In a fifth aspect, the present invention further provides an electrical device, comprising the secondary battery described in the aforementioned embodiment.

[0037] The present invention has the following beneficial effects:

[0038] The negative electrode material of the present invention distributes silicon in the pores of a porous substrate, and utilizes the pore structure of the porous substrate to inhibit the volume expansion of silicon during lithium insertion and extraction, thereby improving the cycle performance of the negative electrode material.

[0039] In the preparation method of the negative electrode material of the present invention, the silicon source is first adsorbed in the cavities of the porous substrate; then the temperature in the furnace is increased to decompose the silane in the cavities, and nano-silicon particles are deposited in the cavities, thereby reducing the content of floating silicon. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0041] Figure 1 A technical roadmap for preparing negative electrode materials according to Example 1 of the present invention;

[0042] Figure 2 This is a SEM image of the negative electrode material prepared in Example 1 of the present invention;

[0043] Figure 3 This is a SEM image of the negative electrode material prepared in Comparative Example 6 of the present invention. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0045] An embodiment of the present invention provides a negative electrode material, including a porous substrate, silicon elements distributed in the pores of the porous substrate, and carbon coated on the surface of the porous substrate. The silicon content in the negative electrode material is 30wt%-80wt%, the resistivity is less than 5Ω·cm, and the value of W is greater than 8, wherein W=silicon content / resistivity, the unit of silicon content is wt%, and the unit of resistivity is Ω·cm.

[0046] Specifically, the silicon content in the negative electrode material can be 30wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt% or any value between 30wt% and 80wt%. Increasing the silicon content in the negative electrode material is beneficial to improving the capacity of the negative electrode material. However, since silicon as a negative electrode material is accompanied by severe volume expansion and contraction during the lithium insertion and delithiation process, it will affect the cycle performance of the negative electrode material. Therefore, the silicon content should not be too much.

[0047] When preparing negative electrode materials with existing technology, a large amount of silicon will exist on the surface of the negative electrode material, forming floating silicon. Since the porous substrate cannot buffer the volume expansion of floating silicon during silicon lithium storage, the presence of floating silicon will also affect the uniformity of carbon coating, which is not conducive to the cycle performance of the negative electrode material.

[0048] In order to ensure the cycle performance of the negative electrode material while increasing the capacity of the negative electrode material as much as possible, the negative electrode material in the present invention minimizes the presence of floating silicon, distributes silicon in the pores of the porous substrate, and utilizes the pore structure of the porous substrate to inhibit the volume expansion of silicon during lithium insertion and extraction, thereby improving the cycle performance of the negative electrode material.

[0049] In the embodiment of the present invention, as the floating silicon content increases, the resistivity of the material increases. The resistivity of the negative electrode material in the embodiment can be less than 1Ω·cm, 1Ω·cm, 2Ω·cm, 3Ω·cm, 4Ω·cm, 5Ω·cm or any value less than 5Ω·cm. The larger W is, the lower the floating silicon content is. The value of W of the negative electrode material in the embodiment can be 8, 9, 10, 20, greater than 20 or greater than 8.

[0050] In the present invention, carbon is coated on the porous substrate, which is beneficial to further alleviate the volume expansion of the negative electrode material during the lithium insertion process and improve the conductivity. In some embodiments, the carbon coating layer content in the silicon-carbon composite negative electrode material is 0.5wt%-10wt%.

[0051] In an optional embodiment, the specific surface area of ​​the negative electrode material is 4m 2 / g-9m 2 / g, specifically 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g or 4m 2 / g-9m 2 / g, the increase of specific surface area can increase the number of active sites for lithium insertion and extraction, which is beneficial to the extraction and extraction of lithium, but too large specific surface area is not conducive to the improvement of the cycle performance of the negative electrode material.

[0052] In an optional embodiment, the D50 of the negative electrode material is 1 μm-15 μm, specifically 1 μm, 3 μm, 5 μm, 7 μm, 9 μm, 11 μm, 13 μm, 15 μm or any value between 1 μm and 15 μm. If the particle size of the negative electrode material is too large, the path for lithium deintercalation at the center will increase, and the difficulty of lithium deintercalation will increase.

[0053] In an optional embodiment, the tap density of the negative electrode material is 0.7 g / cm 3 -1.5g / cm 3 , specifically 0.7 g / cm 3 , 0.8g / cm 3 , 0.9g / cm 3 , 1.0g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 or 0.7g / cm 3 -1.5g / cm 3 Increasing the tap density is beneficial to improving the energy density of the material, but too high a tap density will reduce the pore structure and increase the difficulty of lithium insertion and extraction.

[0054] An embodiment of the present invention provides a method for preparing the negative electrode material according to any one of the aforementioned embodiments, comprising:

[0055] Low temperature adsorption, placing the porous substrate in an environment containing a silicon source gas and adsorbing the silicon source gas;

[0056] High-temperature pyrolysis, heating the porous substrate adsorbing the silicon source gas to decompose the silicon source gas, thereby obtaining a porous substrate with nano-silicon loaded in the pore structure;

[0057] The coating treatment forms a carbon coating layer on the porous substrate loaded with nano-silicon in the pore structure to obtain the negative electrode material.

[0058] In the preparation method of the negative electrode material disclosed in the present invention, the porous substrate firstly exerts its adsorption effect on the silicon source, and adsorbs the silicon source into the cavities of the porous substrate; then the temperature in the furnace is increased to decompose the silane in the cavities, and nano-silicon particles are deposited in the cavities, so as to reduce the influence of the volume expansion caused by silicon lithium storage on the cycle performance of the negative electrode material.

[0059] As the silicon source decomposes inside the pores, it releases gas. As the gas escapes, a void structure is formed inside the deposited silicon, providing sufficient buffer space for the volume expansion of the subsequent nano-silicon particles during lithium extraction and insertion, thereby improving the stability of the negative electrode material.

[0060] The "adsorption first, decomposition later" silicon deposition mode disclosed in the present invention significantly improves the deposition efficiency and the utilization rate of the silicon source when the silicon deposition amount or the deposition time is the same; the lithium-ion battery assembled with the silicon-carbon negative electrode material prepared by the preparation method disclosed in the present invention has more excellent cycle stability and first coulombic efficiency.

[0061] In an optional embodiment, the low-temperature adsorption step is carried out in a low-temperature adsorption device. During the low-temperature adsorption, the low-temperature adsorption step ends when the silicon source gas is discharged from the exhaust gas outlet of the low-temperature adsorption device. The low-temperature adsorption device can be a deposition furnace or other device that can achieve low-temperature adsorption. When the gas leaving the exhaust gas outlet contains silicon source gas, it means that the porous substrate has been saturated with the adsorption of silicon source gas. At this time, if the silicon source gas continues to be introduced, part of the silicon source gas will be adsorbed on the surface of the porous substrate. In the subsequent high-temperature pyrolysis step, the decomposed silicon will be deposited on the surface of the porous substrate to form floating silicon, resulting in an increase in the floating silicon content.

[0062] In an optional embodiment, the low-temperature adsorption temperature is 25°C-200°C, specifically 25°C, 50°C, 75°C, 100°C, 125°C, 150°C, 175°C, 200°C or any value between 25°C and 200°C; the low-temperature adsorption pressure is 0.0001KPa-0.3Kpa, specifically 0.0001KPa-0.3Kpa or any value between 0.0001Kpa, 0.001Kpa, 0.01Kpa, 0.1Kpa, 0.2Kpa, and 0.3Kpa; the low-temperature adsorption time is 1h-30h, specifically 1h, 3h, 5h, 10h, 15h, 20h, 30h or any value between 1h-30h; more optionally, the low-temperature adsorption temperature is 30°C-150°C, the pressure is 0.001KPa-0.1KPa, and the time is 2h-25h.

[0063] Maintaining a low pressure during low-temperature adsorption is beneficial to promoting the adsorption of silicon source gas by the porous substrate and improving the adsorption efficiency; as the pressure increases, the gas molecules gather on the surface of the porous material and cannot effectively diffuse into the holes of the porous substrate, forming surface floating silicon on the surface of the substrate, affecting the cycle stability of the silicon-carbon negative electrode material.

[0064] The low-temperature adsorption step uses a relatively low temperature, which can effectively reduce the movement and diffusion of silicon source gas molecules and improve the adsorption effect of the porous substrate on the silicon source gas; but if the temperature is too low, the gas molecules move too slowly and are unevenly dispersed after entering the porous substrate, resulting in agglomeration of the nano-silicon particles obtained by subsequent pyrolysis, affecting the stability of the negative electrode material.

[0065] In an optional embodiment, the silicon source is selected from at least one of monosilane, disilane, dichlorosilane and trichlorosilane;

[0066] In an optional embodiment, the silicon source-containing gas further comprises an inert gas, wherein the volume fraction of the silicon source is 50 vol%-99 vol%. The presence of the inert gas is beneficial to improving safety.

[0067] In an optional embodiment, the high-temperature pyrolysis step is carried out in a high-temperature pyrolysis device. During the high-temperature pyrolysis, when the exhaust gas from the tail gas outlet of the high-temperature pyrolysis device does not contain hydrogen, the high-temperature pyrolysis step ends. The decomposition of the silicon source gas will release hydrogen. If no hydrogen is discharged from the tail gas outlet, the high-temperature pyrolysis step can be regarded as ending.

[0068] In an optional embodiment, the high-temperature pyrolysis temperature is 300°C-800°C, specifically 300°C, 300°C, 300°C, 300°C, 300°C, 800°C or any value between 300°C-800°C; the high-temperature pyrolysis pressure is 0.01Kpa-5Kpa, specifically 0.01Kpa, 0.1Kpa, 1Kpa, 2Kpa, 3Kpa, 4Kpa, 5Kpa or any value between 0.01Kpa-5Kpa; the high-temperature pyrolysis time is 1 h-50h; specifically, it can be 1h, 3h, 5h, 10h, 20h, 30h, 40h, 50h or any value between 1h-50h; more optionally, the high-temperature pyrolysis temperature is 400℃-700℃, the pressure is 0.01Kpa-3KPa, and the time is 1h-40h; the high-temperature pyrolysis step should provide a relatively high temperature on the one hand to ensure sufficient pyrolysis of the silicon source gas, and on the other hand, it should still be maintained at a relatively low pressure to ensure that the adsorbed silicon source gas continues to stay in the cavities of the porous substrate.

[0069] In an optional embodiment, the porous substrate satisfies at least one of the following AG:

[0070] A. SPAN value <1.5, specifically, it can be 1.5, 1.2, 0.9, 0.6, 0.3, or any value <1.5; the particle size distribution of the porous substrate is relatively uniform, which is conducive to obtaining a negative electrode material with uniform particle size distribution.

[0071] B. Dv50 is 2μm-20μm, specifically 2μm, 5μm, 10μm, 15μm, 20μm or any value between 2μm and 20μm; the particle size of the porous substrate will affect the particle size of the negative electrode material, so the particle size of the porous substrate also needs to be reasonably selected.

[0072] C. The specific surface area of ​​the porous substrate is 400 m 2 / g-2000m 2 / g, specifically 400m 2 / g、800m 2 / g、1200m 2 / g、1600m 2 / g, 2000m 2 / g or any value between 2μm-20μm; optionally 900m 2 / g-2000m 2 / g; the increase in the specific surface area of ​​the porous substrate is beneficial to increasing the amount of adsorbed silicon source gas, but a too large specific surface area will lead to an excessively high silicon content in the negative electrode material, which is not conducive to the improvement of the cycle performance; in addition, the specific surface area of ​​the porous substrate will be partially inherited by the negative electrode material, thereby affecting the specific surface area of ​​the negative electrode material.

[0073] D. The average pore size is 1.2nm-7.0nm, specifically 1.2nm, 3nm, 5nm, 7.0nm or any value between 1.2nm-7.0nm, optionally 1.5nm-5.0nm; if the pore size is too large, it is not conducive to the uniform dispersion of deposited silicon, and if the pore size is too small, it cannot accommodate the volume expansion of silicon after lithium insertion, which is not conducive to improving the cycle performance of the negative electrode material.

[0074] E. Pore volume is 0.3 cm 3 / g-2.0cm 3 / g, specifically 0.3cm 3 / g, 0.6cm 3 / g, 0.9cm 3 / g, 1.2cm 3 / g, 1.5cm 3 / g, 2.0cm 3 / g or 0.3cm 3 / g-2.0cm 3 Any value between / g, optionally 0.5cm 3 / g-1.8cm 3 / g; if the pore volume is too large, the strength of the porous substrate will be relatively low; if the pore volume is too small, it will not be able to accommodate enough silicon source gas, resulting in a decrease in the silicon content in the negative electrode material.

[0075] F, pore concentration is 0.3-6.0, specifically, it can be 0.3, 1, 2, 4, 6.0 or any value between 0.3-6.0, calculated as (P V 90-P V 10) / P V 50, optionally 0.3-8: wherein PV refers to pore volume. A relatively uniform pore volume is conducive to relatively uniform adsorption of silicon in the cavities of the porous substrate, and further conducive to uniform distribution of deposited silicon in the porous substrate.

[0076] G. The porous substrate is selected from at least one of porous carbon, porous metal oxides, coordination polymers, porous metals and porous ceramics, and can be porous carbon. The porous carbon substrate can provide a certain capacity while adsorbing silicon source gas and has good stability.

[0077] In an optional embodiment, the coating treatment includes passing a carbon-containing gas source into a reactor in which the porous substrate loaded with nano-silicon is placed in the pore structure to perform carbon deposition to form a carbon coating layer;

[0078] Optionally, the temperature of carbon deposition is 300°C-1300°C, specifically 300°C, 600°C, 900°C, 1100°C, 1300°C or any value between 300°C-1300°C, and the carbon deposition time is 1h-10h, specifically 1h, 3h, 5h, 7h, 10h or any value between 1h-10h; Optionally, the temperature of carbon deposition is 400°C-1000°C, more preferably 400°C-600°C;

[0079] Optionally, the carbon-containing gas source includes a carbon source gas, and the carbon source gas is selected from an alkane gas having a cracking temperature within the carbon deposition temperature range;

[0080] Optionally, the carbon-containing gas source further comprises an inert gas;

[0081] Optionally, the carbon source gas volume fraction in the carbon-containing source gas is 50 vol%-99 vol%;

[0082] In a third aspect, the present invention further provides a negative electrode plate, comprising the negative electrode material described in any one of the aforementioned embodiments or the negative electrode material prepared by the method of any one of the aforementioned embodiments.

[0083] In a fourth aspect, the present invention further provides a secondary battery, comprising the negative electrode plate described in the aforementioned embodiment, wherein the secondary battery has excellent cycle stability, and has both high reversible specific capacity and first coulombic efficiency.

[0084] In a fifth aspect, the present invention further provides an electrical device, comprising the secondary battery described in the aforementioned embodiment.

[0085] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0086] Example 1

[0087] This embodiment provides a method for preparing a negative electrode material. The technical roadmap is as follows: Figure 1 As shown, the following steps are included:

[0088] (1) Low temperature adsorption, the porous carbon substrate (average pore size 4.5nm, pore volume 1.0cm 3 / g, Dv50 is 7.8μm, and the specific surface area is 1873m 2 / g, SPAN value is 1.2, pore concentration is 2.4) is placed in a vapor deposition furnace, the temperature of the deposition furnace is adjusted to 100°C, the pressure in the furnace is adjusted to 0.05KPa, a mixed gas consisting of 70vol% monosilane and 30vol% nitrogen is introduced at a flow rate of 10L / min, and the exhaust gas from the tail pipe is observed by a mass spectrometer. When the insulation treatment time is 12h, silane gas appears in the exhaust gas, and the low-temperature adsorption step is completed. At this time, the introduction of silane gas is stopped and nitrogen is continued.

[0089] (2) After high-temperature pyrolysis and low-temperature adsorption, adjust the temperature of the deposition furnace to 550°C, adjust the pressure in the furnace to 1.5 KPa, keep nitrogen flowing continuously, and observe the exhaust gas from the tail pipe through a mass spectrometer. When the insulation treatment time is 15 hours, the hydrogen content in the exhaust gas drops to 0, and the high-temperature pyrolysis step is completed.

[0090] (3) Coating treatment: After the high-temperature pyrolysis step, the furnace temperature was adjusted to 800°C, and a mixed gas consisting of 60 vol% acetylene and 40 vol% nitrogen was introduced at a flow rate of 10 L / min. The deposition time was 2 h. After the carbon coating was completed, the temperature was cooled to room temperature. The material was dispersed, screened, demagnetized, and other means to obtain a silicon-carbon negative electrode material. SEM showed that Figure 2 shown.

[0091] Example 2: Low temperature adsorption pressure improvement

[0092] This embodiment provides a method for preparing a negative electrode material, which is basically the same as that of Embodiment 1, except that the pressure in the furnace in step (1) is adjusted to 0.15 KPa.

[0093] Example 3: Low temperature adsorption pressure reduction

[0094] This embodiment provides a method for preparing a negative electrode material, which is basically the same as that of Embodiment 1, except that the pressure in the furnace in step (1) is adjusted to 0.0008 KPa.

[0095] Example 4: Low temperature adsorption temperature rise

[0096] This embodiment provides a method for preparing a negative electrode material, which is basically the same as that of Embodiment 1, except that the temperature in the furnace in step (1) is adjusted to 180°C.

[0097] Example 5: Low temperature adsorption temperature reduction

[0098] This embodiment provides a method for preparing a negative electrode material, which is basically the same as that of Embodiment 1, except that the pressure in the furnace in step (1) is adjusted to 30° C.

[0099] Comparative Example 1: Low temperature adsorption pressure is too high

[0100] This comparative example provides a method for preparing a negative electrode material, which is basically the same as that of Example 1, except that the pressure in the furnace in step (1) is adjusted to 1 KPa.

[0101] Comparative Example 2: Low temperature adsorption temperature is too low

[0102] This comparative example provides a method for preparing a negative electrode material, which is basically the same as that of Example 1, except that the temperature in the furnace in step (1) is adjusted to 10°C.

[0103] Comparative Example 3: Low temperature adsorption temperature is too high

[0104] This comparative example provides a method for preparing a negative electrode material, which is basically the same as that of Example 1, except that the pressure in the furnace in step (1) is adjusted to 250°C.

[0105] Comparative Example 4: The low-temperature adsorption step was terminated before silane appeared in the low-temperature adsorption tail gas.

[0106] This comparative example provides a method for preparing a negative electrode material, which is basically the same as that of Example 1, except that the heat preservation treatment time in step (1) is adjusted to 10 h.

[0107] Comparative Example 5: After silane appears in the low-temperature adsorption tail gas, the low-temperature adsorption step is continued.

[0108] This embodiment provides a method for preparing a negative electrode material, which is basically the same as that of Embodiment 1, except that the heat preservation treatment time in step (1) is adjusted to 15 hours.

[0109] Comparative Example 6

[0110] This embodiment provides a method for preparing a negative electrode material, comprising the following steps:

[0111] (1) In an argon atmosphere, a porous carbon material (average pore size of 4.5 nm and pore volume of 0.98 cm) was used as a substrate. 3 / g, Dv50 is 7.5μm, and the specific surface area is 1847m 2 / g, SPAN value is 1.2, pore size concentration is 2.8) is placed in a deposition furnace at a temperature of 550°C; a mixed gas consisting of 70 vol% monosilane and 30 vol% acetylene is introduced into the deposition furnace at a flow rate of 10 L / min, and the tail pipe air pressure valve is adjusted to keep the pressure in the furnace at 1.5 KPa. The gas is continuously ventilated for 12 hours, and silicon particles and carbon particles are continuously nucleated and deposited inside the pores of the porous carbon material;

[0112] (2) After the silicon-carbon deposition is completed, the deposition furnace is heated to 800°C, and a mixed gas consisting of 60 vol% acetylene and 40 vol% nitrogen is introduced at a flow rate of 10 L / min. The deposition time is 2 h. After the carbon coating is completed, the temperature is lowered to room temperature. The material is dispersed, screened, demagnetized, and other means to obtain a silicon-carbon negative electrode material. SEM is shown as follows: Figure 3 shown.

[0113] Comparative Example 7

[0114] This embodiment provides a method for preparing a negative electrode material, comprising the following steps:

[0115] The method is basically the same as Comparative Example 6, except that the ventilation time in step (1) is adjusted to 15 h.

[0116] The composition and structure of the negative electrode materials obtained in the above examples and comparative examples were characterized, wherein the specific surface area was measured using a US Micromeritics TriStar 3020 specific surface area and pore size analyzer, the D50 was tested using a Mastersizer 3000 laser diffraction technique, and the tap density was tested using a tap density meter. The specific test results are shown in Table 1:

[0117] Table 1

[0118]

[0119] Application Examples

[0120] The negative electrode materials prepared in each embodiment are respectively assembled into batteries, which specifically includes the following steps.

[0121] (1) Preparation of positive electrode sheets: The positive electrode active material lithium nickel cobalt manganese oxide (NCM811), conductive agent SuperP, carbon nanotubes, binder polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) are mixed in a mass ratio of 97:1:0.5:1.5 to form a positive electrode slurry (solid content of 70%), which is then coated on both sides of the current collector aluminum foil, dried at 100°C, and cold pressed at 4MPa at room temperature. The positive electrode sheets are then trimmed, cut, and slit, and the tabs are welded to form positive electrode sheets.

[0122] (2) Preparation of negative electrode sheets: Under a nitrogen protective atmosphere, the solvent N-methylpyrrolidone (NMP) and the binder PVDF are stirred and mixed, and then the conductive agent SuperP is added and stirred and mixed. Then, the negative electrode active material is added and stirred and mixed thoroughly to make a negative electrode slurry (solid content is 50%).

[0123] The negative electrode slurry is coated on both sides of the current collector copper foil, dried at 100°C, cold pressed at 4MPa at room temperature, and then trimmed, cut, stripped, and the tabs are welded to make negative electrode sheets.

[0124] (3) Assembly of lithium-ion batteries

[0125] Using PE porous polymer film as a separator, the prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrode sheets, and the bare battery cell is wound; the bare battery cell is placed in an aluminum plastic shell package, and dried at 100°C to a moisture content of less than 100ppm under a relative vacuum pressure of -0.95×105Pa. The electrolyte is injected into the dried bare battery cell, wherein the electrolyte consists of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) (EC:EMC:DEC volume ratio = 1:1:1) and LiPF6 (1.0M), and the package, static, formation (0.02C constant current charging for 2h, 0.1C constant current charging for 2h), shaping, and capacity testing (capacity separation) are performed to make a soft-pack liquid lithium-ion battery.

[0126] When assembling the battery, five batteries are prepared for each test, and a total of five sets of data are tested. The final performance is the average value of the five sets of data.

[0127] The battery cycle performance is tested on the Xinwei equipment, specifically:

[0128] At 25°C, first discharge at 0.1C to 0.005V, then discharge at 0.08C to 0.001V, discharge at 0.05C to 0.001V, discharge at 0.02C to 0.001V, and let stand for 10 minutes; then charge to 1.5V at 0.1C, let stand for 10 minutes, record the charge and discharge capacity after the first cycle, and calculate the first coulomb efficiency; cycle 100 times in the above manner, record the charge and discharge capacity after 100 times, calculate the capacity retention rate after 100 cycles, and the test and calculation process of the capacity retention rate after 500 cycles adopt the same method; the resistivity is tested by a semiconductor powder resistivity tester (30MPa four-probe V1.4) at 25°C, and the specific test results are shown in Table 2 below.

[0129] Table 2

[0130] Serial number Silicon content (%) Reversible specific capacity (mAh / g) First coulombic efficiency (%) Capacity retention after 100 cycles (%) Capacity retention after 500 cycles (%) Resistivity (Ω·cm) Example 1 52.29 1857 92 96 89 4.51 Example 2 52.11 1849 90 94 87 3.67 Example 3 52.65 1870 92 95 86 4.14 Example 4 52.62 1869 91 93 88 3.75 Example 5 52.10 1850 91 90 82 4.91 Comparative Example 1 53.18 1889 93 84 70 47.63 Comparative Example 2 52.79 1875 92 80 63 14.33 Comparative Example 3 52.49 1864 92 89 76 35.75 Comparative Example 4 42.73 1547 85 96 88 5.48 Comparative Example 5 59.05 1993 93 76 / 105.37 Comparative Example 6 47.20 1709 87 90 79 39.85 Comparative Example 7 52.17 1849 91 84 69 74.97

[0131] It can be seen from the data of Examples 1-3 and Comparative Example 1 that in the low-temperature adsorption step, maintaining a relatively low pressure in the deposition furnace can effectively promote the adsorption of the porous substrate. The increase in the negative pressure can promote the improvement of the adsorption efficiency of the substrate; the decrease in the negative pressure causes the gas molecules to gather on the surface of the porous material and cannot effectively diffuse into it, forming surface floating silicon on the surface of the substrate, affecting the cycle stability of the silicon-carbon negative electrode material.

[0132] It can be seen from the data of Examples 1, 4-5 and Comparative Examples 2-3 that the relatively low temperature in the low-temperature adsorption step can effectively reduce the movement and diffusion of silane gas molecules and improve the adsorption effect of the substrate on silane gas; however, if the adsorption temperature is too low, the gas molecules move too slowly and are unevenly dispersed after entering the porous substrate, resulting in agglomeration after subsequent pyrolysis, affecting the stability of the negative electrode material.

[0133] It can be seen from Example 1 and Comparative Examples 4-5 that by determining the end time of the low-temperature adsorption step by the time when silane appears in the tail pipe, the amount of silane deposition can be effectively controlled to avoid excessive deposition leading to the appearance of floating silicon on the surface.

[0134] It can be seen from Example 1 and Comparative Examples 6-7 that the amount of silane deposited in Comparative Example 6 within the same time period is significantly lower than that in Example 1, and Comparative Example 6 cannot effectively control the silane deposition position, resulting in surface floating silicon, which leads to a significant increase in the resistivity of the material; only by appropriately extending the deposition time can a deposition amount equivalent to that in Example 1 be achieved, but as in Comparative Example 7, the floating silicon phenomenon is more obvious at this time. In addition to the increase in resistivity, it also has a serious impact on the cycle stability of the material, shortening the battery life.

[0135] The lithium-ion battery assembled from the silicon-carbon negative electrode material prepared by the present invention has excellent cycle stability. The capacity retention rate after 100 cycles is as high as over 90%, and can reach up to 96% at the highest. The capacity retention rate after 500 cycles is as high as over 80%, and can reach up to 87% at the highest. The powder resistance is low, less than 8Ω·cm, and has both high reversible specific capacity and first coulombic efficiency.

[0136] The above description is only an optional embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A negative electrode material, characterized in that: The negative electrode material comprises a porous substrate, silicon elements distributed in the pores of the porous substrate, and carbon coated on the surface of the porous substrate, wherein the silicon content in the negative electrode material is 30wt%-80wt%, the resistivity is less than 5Ω·cm, and the value of W is greater than 8, wherein W=silicon content / resistivity, the unit of silicon content is wt%, and the unit of resistivity is Ω·cm; The silicon element distributed in the pores of the porous substrate is obtained by low-temperature adsorption and high-temperature decomposition steps, wherein: Low temperature adsorption, placing the porous substrate in an environment containing silicon source gas and adsorbing the silicon source gas; the low temperature adsorption temperature is 25℃-200℃, and the pressure is 0.0001KPa-0.3KPa; High-temperature pyrolysis is performed by heating the porous substrate adsorbed with silicon source gas to decompose the silicon source gas, thereby obtaining a porous substrate with nano-silicon loaded in the pore structure; the high-temperature pyrolysis step is performed in a high-temperature pyrolysis device, and the high-temperature pyrolysis step ends when the exhaust gas discharged from the tail gas outlet of the high-temperature pyrolysis device does not contain hydrogen during the high-temperature pyrolysis, and the high-temperature pyrolysis step maintains continuous nitrogen flow.

2. The negative electrode material according to claim 1, characterized in that The specific surface area of ​​the negative electrode material is 4 m 2 / g-9m 2 / g; And / or, the D50 of the negative electrode material is 1 μm-15 μm; And / or, the tap density of the negative electrode material is 0.7 g / cm 3 -1.5g / cm 3 .

3. A method for preparing the negative electrode material according to claim 1, characterized in that: include: Low temperature adsorption, placing the porous substrate in an environment containing a silicon source gas and adsorbing the silicon source gas; High-temperature pyrolysis, heating the porous substrate adsorbing the silicon source gas to decompose the silicon source gas, thereby obtaining a porous substrate with nano-silicon loaded in the pore structure; The coating treatment forms a carbon coating layer on the porous substrate loaded with nano-silicon in the pore structure to obtain the negative electrode material.

4. The method for preparing the negative electrode material according to claim 3, characterized in that: The low temperature adsorption step is carried out in a low temperature adsorption device. During the low temperature adsorption, when the silicon source gas is discharged from the tail gas outlet of the low temperature adsorption device, the low temperature adsorption step ends; the low temperature adsorption step satisfies at least one of the following ac: a. Low temperature adsorption temperature is 25℃-200℃, pressure is 0.0001KPa-0.3KPa, and time is 1h-30h; b, the silicon source is selected from at least one of monosilane, disilane, dichlorosilane and trichlorosilane; c. The silicon source-containing gas also includes an inert gas, wherein the volume fraction of the silicon source is 50 vol%-99 vol%.

5. The method for preparing the negative electrode material according to claim 3, characterized in that: The high-temperature pyrolysis step is carried out in a high-temperature pyrolysis device. During the high-temperature pyrolysis, when the exhaust gas from the tail gas outlet of the high-temperature pyrolysis device does not contain hydrogen, the high-temperature pyrolysis step is terminated; The high temperature pyrolysis temperature is 300℃-800℃, the pressure is 0.01Kpa-5Kpa, and the time is 1h-50h.

6. The method for preparing the negative electrode material according to claim 3, characterized in that: The porous substrate satisfies at least one of the following A and B: A. SPAN value <1.5; B. Dv50 is 2μm-20μm C. The specific surface area of ​​the porous substrate is 400 m 2 / g-2000m 2 / g, optionally 900m 2 / g-2000m 2 / g; D. Average pore size is 1.2nm-7.0nm, optionally 1.5nm-5.0nm; E. Pore volume is 0.3 cm 3 / g-2.0cm 3 / g, optionally 0.5cm 3 / g-1.8cm 3 / g; F, pore size concentration is 0.3-6.0, calculated as (P V 90-P V 10) / P V 50, optionally 0.3-8: G. The porous substrate is selected from at least one of porous carbon, porous metal oxide, coordination polymer, porous metal and porous ceramic, and is optionally porous carbon.

7. The method for preparing the negative electrode material according to claim 3, characterized in that: The coating treatment comprises introducing a carbon-containing gas source into a reactor in which a porous substrate loaded with nano-silicon is placed in the pore structure to perform carbon deposition to form a carbon coating layer; the coating treatment step satisfies at least one of the following (1)-(4): (1) The temperature of carbon deposition is 300℃-1300℃, and the carbon deposition time is 1h-10h; (2) The carbon-containing gas source includes a carbon source gas, and the carbon source gas is selected from an alkane gas whose cracking temperature is within the carbon deposition temperature range; (3), the carbon-containing gas source also includes an inert gas; (4) The volume fraction of the carbon source gas in the carbon-containing source gas is 50 vol%-99 vol%.

8. A negative electrode plate, characterized in that: The invention comprises the negative electrode material according to claim 1 or 2 or the negative electrode material prepared by any one of the methods of claims 3-7.

9. A secondary battery, characterized in that: Including the negative electrode sheet as described in claim 8.

10. An electrical equipment, characterized in that: A secondary battery comprising the secondary battery according to claim 9.