Highly stable modified supported metal catalyst and preparation method and application thereof

By modifying niobium oxide, SnO2 or TiO2 on the water-gas transformation catalyst, the interaction between metal oxides and single-atom clusters is enhanced, the problem of insufficient catalyst stability and activity is solved, and efficient water-gas transformation reaction performance is achieved.

CN118437322BActive Publication Date: 2024-12-03UNIV OF CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410517644.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-12-03
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The existing Fe-based and Cu-based catalysts have poor stability in water-gas transformation reactions, high loading of precious metals and high cost, and single-atom catalysts have poor stability in high reduction atmospheres, making it difficult to improve their activity and stability at the same time.

Method used

Niobium oxide, SnO2 or TiO2 metal oxides are modified on the supported metal catalyst by atomic layer deposition method, enhancing the interaction between single atomic/subnano clusters and metal oxides and electron interactions, forming high stability and high activity modified supported metal catalyst.

Benefits of technology

A catalyst with good low-temperature activity, high selectivity and strong stability in water-gas transformation reaction is realized, reducing the load of precious metals and preparation costs, and improving the overall performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118437322B_ABST
    Figure CN118437322B_ABST
Patent Text Reader

Abstract

The present invention discloses a highly stable modified supported metal catalyst and its preparation method and application, and relates to the field of catalyst technology. The technical scheme is as follows: comprising the following steps: S1 preparing a metal oxide carrier; S2 uniformly dispersing the metal oxide carrier powder of step S1 on a frosted glass sheet, and performing noble metal deposition by atomic layer deposition to obtain a single atom / sub-nanometer cluster supported catalyst; S3 performing niobium oxide, SnO2 or TiO2 metal oxide deposition on the supported catalyst obtained in step S2 again by atomic layer deposition to obtain a metal oxide modified supported metal catalyst. The present invention modifies the single atom / sub-nanometer cluster of the supported metal catalyst with a thin atomic layer of niobium oxide, SnO2, or TiO2 metal oxide, which can achieve the simultaneous improvement of the stability and catalytic activity of the single atom / metal cluster.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a highly stable modified supported metal catalyst and a preparation method and application thereof. Background Art

[0002] Hydrogen is considered the cleanest energy source. When hydrogen is burned, it only produces water, without producing toxic gases or CO. 2 . The energy density of hydrogen (140MJ / kg) is three times that of oil and 4.5 times that of coal, making it an ideal substitute for fossil fuels. In addition, hydrogen can also be used as a storage medium for fluctuating energy sources such as wind, light, and hydropower, reducing the phenomenon of wind, light, and water abandonment. As an energy carrier, hydrogen and hydrogen fuel cells are expected to be widely used in automobiles, portable power generation, and fixed power stations. Hydrogen can also be used in industrial fields such as metal refining, hydroprocessing of petroleum products, and chemical synthesis. As the global demand for hydrogen increases, catalytic hydrogen production has great potential in meeting the growing demand for hydrogen.

[0003] The water-gas shift (WGS) reaction plays a vital role in industrial hydrogen production and fuel cell feed stream purification. It is also an important reaction in the process of synthesis gas conversion (such as methanol synthesis and Fischer-Tropsch synthesis). The chemical equation of the water-gas shift (WGS) process is as follows:

[0004] WGS: CO(g)+H 2 O(g)→CO 2 (g)+H 2 (g)

[0005] WGS is an exothermic reaction Lower temperatures are conducive to higher CO conversion rates, but high temperatures can increase the reaction rate. Therefore, in industry, WGS is carried out in a two-stage catalytic converter with high temperature (320-450°C) and low temperature (150-250°C). The commercial catalyst in the high temperature stage is mainly Fe-Cr catalyst, in which Fe 3 O 4 It is an active phase. Cr can prevent the recrystallization of magnetite and act as a stabilizer. 2 O 3 The catalyst has been commercialized, and studies have shown that Cu + It is the active center, Al 2 O 3 However, Fe-based and Cu-based catalysts have poor stability and are easily affected by thermal sintering and chemical poisoning.

[0006] Supported metal catalysts (mainly precious metals Pt, Au and Ir catalysts) show excellent catalytic activity in low-temperature WGS (LT-WGS) reactions. The amount of precious metals used in existing LT-WGS catalysts greatly affects their preparation costs, and the stability of single-component precious metals also needs to be improved. Previous studies have shown that single-atom catalysts can greatly improve the catalytic efficiency of catalysts and greatly reduce the amount of precious metal loading, achieving the dual goals of improving hydrogen production efficiency and reducing catalyst costs. However, single-atom catalysts have poor stability under reaction conditions of highly reducing atmospheres. Therefore, there are huge challenges in how to simultaneously improve the activity and stability of single-atom / sub-nano cluster catalysts. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art, provide a highly stable modified supported metal catalyst and its preparation method and application, and convert a thin atomic layer of niobium oxide, SnO 2 、TiO 2 Metal oxides are modified on single atoms / sub-nanoclusters of supported metal catalysts. Through the strong interaction and electronic interaction between metal oxide additives and single atoms / metal clusters, the stability and catalytic activity of single atoms / metal clusters can be improved simultaneously.

[0008] The technical solution of the present invention is:

[0009] In a first aspect, the present invention provides a method for preparing a highly stable modified supported metal catalyst, comprising the following steps:

[0010] S1 prepares a metal oxide support;

[0011] S2: uniformly dispersing the metal oxide support powder of step S1 on a frosted glass sheet, and performing noble metal deposition by atomic layer deposition to obtain a single atom / sub-nano cluster supported catalyst;

[0012] S3: The supported catalyst obtained in step S2 is again subjected to atomic layer deposition (ALD) to form niobium oxide, SnO 2 or TiO 2 The metal oxide is deposited to obtain a supported metal catalyst modified with the metal oxide.

[0013] The supported catalyst prepared by the present invention contains an active phase dispersed at the level of single atoms or sub-nano clusters, and the further modified single atoms or sub-nano cluster active phase is partially coated with a metal oxide with a thickness of an atomic layer, which can significantly adjust the electronic structure of the active phase and play a role in confining and stabilizing the active phase. Therefore, the modified supported catalyst prepared by the ALD method can show advantages such as good low-temperature activity, high selectivity, and strong stability in the catalytic hydrogen production reaction.

[0014] Preferably, in step S1, the metal oxide support is prepared by a hydrothermal synthesis method.

[0015] Preferably, in step S1, the metal oxide carrier is CeO 2 、TiO 2 or iron oxide carrier.

[0016] Preferably, in step S2, the noble metal is Pt, Au or Ir.

[0017] Preferably, in step S2, the noble metal is deposited 2-20 times, and the loading amount of the noble metal is 0.5-2% of the mass of the metal oxide carrier.

[0018] Preferably, in step S3, the number of depositions of the metal oxide is 2-15 times, and the loading amount of the metal oxide is 0.5-5% of the mass of the metal oxide carrier.

[0019] In a second aspect, the present invention provides a highly stable modified supported metal catalyst prepared by the above preparation method. The water-gas shift hydrogen production catalyst prepared by the present invention has a mesoporous structure of 5-100 nm and a specific surface area of ​​50-200 m 2 / g.

[0020] In a third aspect, the present invention provides the use of a highly stable modified supported metal catalyst prepared by the above preparation method in water-gas shift hydrogen production.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention uses atomic layer deposition (ALD) technology to deposit thin atomic layers of niobium oxide, SnO 2 、TiO 2 Metal oxides are modified on single atoms / sub-nano clusters of supported metal catalysts. Through the strong interaction and electronic interaction between metal oxide additives and single atoms / metal clusters, the stability and catalytic activity of single atoms / metal clusters can be improved simultaneously. ALD technology can overcome the shortcomings of existing catalyst preparation technologies, such as uneven loading of precious metals and excessive coverage of additives, which completely covers the active sites of precious metals. It provides a method for preparing atomic-level modified supported catalysts, thereby achieving high catalytic activity and high stability in catalytic hydrogen production reactions. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is the XRD spectra of different catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2.

[0024] Figure 2 The different TiO prepared in Example 1 2Doping amount of Pt / CeO 2 Catalyst and TiO prepared in Comparative Example 1 2 / CeO 2 Water-gas shift activity diagram of the catalyst, the reaction inlet atmosphere is 2% CO + 8% H 2 O / N 2 .

[0025] Figure 3 The xTiO prepared in Example 1 2 -Pt / CeO 2 (x=2, 6) Stability evaluation results of the catalyst for catalytic water-gas shift hydrogen production at 240°C. DETAILED DESCRIPTION

[0026] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0027] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0028] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0029] Example 1

[0030] The preparation method of the highly stable modified supported metal catalyst of this embodiment comprises the following steps:

[0031] S1 used the hydrothermal synthesis method to prepare the metal oxide support: 1.302 g of cerium nitrate was added to 7.5 mL of deionized water and stirred until completely dissolved to obtain solution A; 14.4 g of sodium hydroxide was added to 52.5 mL of deionized water and stirred until completely dissolved to obtain solution B; solution B was added dropwise to solution A and precipitated under stirring for 30 min; the suspension was transferred to a hydrothermal reactor and hydrothermally reacted at 100 ° C for 24 h; filtered and washed, the obtained sample was dried overnight, and then calcined in a muffle furnace at 500 ° C for 4 h to obtain CeO 2 Carrier;

[0032] S2 uses ALD technology to prepare CeO 2 Supported platinum catalyst Pt / CeO 2 First, 20 mg of CeO prepared in step S1 was added to 2 The carrier was dispersed on a quartz glass sheet, dried at room temperature, and then transferred to an ALD reactor. The ALD process took place in a high-temperature, closed chamber. The deposition of Pt was carried out in the form of (trimethyl)methylcyclopentadienylplatinum (IV) (MeCpPtMe 3 ) and O3 As precursor, Ar as carrier gas, 2 deposition cycles were performed at 250 °C; MeCpPtMe 3 The pulse, breath holding and purge times were 0.5 s, 15 s and 25 s respectively; 3 The pulse, breath-hold and purge times were 1 s, 10 s and 25 s respectively;

[0033] S3 uses ALD technology to prepare TiO 2 Modified Pt / CeO 2 Catalyst: Pt / CeO prepared in step S2 2 Catalyst TiO 2 Atomic deposition, TiO 2 The deposition of titanium tetraisopropoxide (C 12 H 28 O 4 Ti) and H 2 O was used as the precursor and Ar was used as the carrier gas. TiO 2 Sedimentation cycle; C 12 H 28 O 4 The pulse, breath holding and purge times of Ti were 0.5 s, 8 s and 25 s respectively; H 2 The pulse, holding and purge times of O were 0.1 s, 8 s and 25 s respectively; the prepared TiO 2 Modified Pt / CeO 2 The catalyst is represented by 2TiO 2 -Pt / CeO 2 , 6TiO 2 -Pt / CeO 2 , 12TiO 2 -Pt / CeO 2 .

[0034] Example 2

[0035] The difference from Example 1 is that step S3 uses ALD technology to prepare Nb 2 O 5 Modified Pt / CeO 2 Catalyst: Pt / CeO prepared in step S2 2 Catalyst for Nb 2 O 5 Atomic deposition, 6 times Nb at 150 °C 2 O 5 Deposition cycle, the prepared Nb 2 O 5 Modified Pt / CeO 2 The catalyst is represented by 6Nb 2 O 5-Pt / CeO 2 .

[0036] Example 3

[0037] The difference from Example 1 is that step S3 uses ALD technology to prepare SnO 2 Modified Pt / CeO 2 Catalyst: Pt / CeO prepared in step S2 2 Catalyst SnO 2 Atomic deposition, 6 passes of SnO at 150 °C 2 Deposition cycle, the prepared SnO 2 Modified Pt / CeO 2 The catalyst is represented by 6SnO 2 -Pt / CeO 2 .

[0038] Comparative Example 1

[0039] The preparation method of the supported metal catalyst of Comparative Example 1 comprises the following steps:

[0040] S1 used the hydrothermal synthesis method to prepare the metal oxide support: 1.302 g of cerium nitrate was added to 7.5 mL of deionized water and stirred until completely dissolved to obtain solution A; 14.4 g of sodium hydroxide was added to 52.5 mL of deionized water and stirred until completely dissolved to obtain solution B; solution B was added dropwise to solution A and precipitated under stirring for 30 min; the suspension was transferred to a hydrothermal reactor and hydrothermally reacted at 100 ° C for 24 h; filtered and washed, the obtained sample was dried overnight, and then calcined in a muffle furnace at 500 ° C for 4 h to obtain CeO 2 Carrier;

[0041] S2 uses ALD technology to prepare CeO 2 Supported titanium oxide catalyst TiO 2 / CeO 2 First, 20 mg of CeO prepared in step S1 was added to 2 The carrier is dispersed on a quartz glass sheet. After drying at room temperature, the quartz glass sheet is transferred to the ALD reactor. The ALD process takes place in a high-temperature, closed chamber. 2 The deposition of titanium tetraisopropoxide (C 12 H 28 O 4 Ti) and H 2 O was used as the precursor and Ar was used as the carrier gas. Six deposition cycles were performed at 150 °C. 12 H 28 O 4 The pulse, breath holding and purge times of Ti were 0.5 s, 8 s and 25 s respectively; H2 The pulse, breath-hold, and purge times of O were 0.1 s, 8 s, and 25 s, respectively.

[0042] Comparative Example 2

[0043] The preparation method of the supported metal catalyst of Comparative Example 2 comprises the following steps:

[0044] S1 used the hydrothermal synthesis method to prepare the metal oxide support: 1.302 g of cerium nitrate was added to 7.5 mL of deionized water and stirred until completely dissolved to obtain solution A; 14.4 g of sodium hydroxide was added to 52.5 mL of deionized water and stirred until completely dissolved to obtain solution B; solution B was added dropwise to solution A and precipitated under stirring for 30 min; the suspension was transferred to a hydrothermal reactor and hydrothermally reacted at 100 ° C for 24 h; filtered and washed, the obtained sample was dried overnight, and then calcined in a muffle furnace at 500 ° C for 4 h to obtain CeO 2 Carrier;

[0045] S2 uses ALD technology to prepare CeO 2 Supported niobium oxide catalyst Nb 2 O 5 / CeO 2 First, 20 mg of CeO prepared in step S1 was added to 2 The carrier is dispersed on a quartz glass sheet. After drying at room temperature, the quartz glass sheet is transferred to the ALD reactor. The ALD process takes place in a high-temperature, closed chamber. 2 O 5 The deposition of cyclopentadienyl niobium tetrachloride (C 5 H 5 Cl 4 Nb) and H 2 O was used as the precursor and Ar was used as the carrier gas. Six deposition cycles were performed at 150 °C. 5 H 5 Cl 4 The pulse, breath holding and purge times of Nb were 0.5 s, 8 s and 25 s respectively; H 2 The pulse, breath-hold, and purge times of O were 0.1 s, 8 s, and 25 s, respectively.

[0046] Comparative Example 3

[0047] The preparation method of the supported metal catalyst of Comparative Example 3 comprises the following steps:

[0048] S1 used the hydrothermal synthesis method to prepare the metal oxide support: 1.302 g of cerium nitrate was added to 7.5 mL of deionized water and stirred until completely dissolved to obtain solution A; 14.4 g of sodium hydroxide was added to 52.5 mL of deionized water and stirred until completely dissolved to obtain solution B; solution B was added dropwise to solution A and precipitated under stirring for 30 min; the suspension was transferred to a hydrothermal reactor and hydrothermally reacted at 100 ° C for 24 h; filtered and washed, the obtained sample was dried overnight, and then calcined in a muffle furnace at 500 ° C for 4 h to obtain CeO 2 Carrier;

[0049] S2 uses ALD technology to prepare CeO 2 Supported tin oxide catalyst SnO 2 / CeO 2 First, 20 mg of CeO prepared in step S1 was added to 2 The carrier is dispersed on a quartz glass sheet. After drying at room temperature, the quartz glass sheet is transferred to the ALD reactor. The ALD process takes place in a high-temperature, closed chamber. 2 The deposition of butyl stannoic acid (C 4 H 10 O 2 Sn) and H 2 O was used as the precursor and Ar was used as the carrier gas. Six deposition cycles were performed at 150 °C. 4 H 10 O 2 The pulse, breath holding and purge times of Sn were 0.5 s, 8 s and 25 s respectively; 2 The pulse, breath-hold, and purge times of O were 0.1 s, 8 s, and 25 s, respectively.

[0050] Comparative Example 4

[0051] Comparative Example 4 The preparation method of the modified supported metal catalyst comprises the following steps:

[0052] S1 used the hydrothermal synthesis method to prepare the metal oxide support: 1.302 g of cerium nitrate was added to 7.5 mL of deionized water and stirred until completely dissolved to obtain solution A; 14.4 g of sodium hydroxide was added to 52.5 mL of deionized water and stirred until completely dissolved to obtain solution B; solution B was added dropwise to solution A and precipitated under stirring for 30 min; the suspension was transferred to a hydrothermal reactor and hydrothermally reacted at 100 ° C for 24 h; filtered and washed, the obtained sample was dried overnight, and then calcined in a muffle furnace at 500 ° C for 4 h to obtain CeO 2 Carrier;

[0053] S2 uses ALD technology to prepare CeO 2 Supported titanium oxide catalyst TiO2 / CeO 2 First, 20 mg of CeO prepared in step S1 was added to 2 The carrier is dispersed on a quartz glass sheet. After drying at room temperature, the quartz glass sheet is transferred to the ALD reactor. The ALD process takes place in a high-temperature, closed chamber. 2 The deposition of titanium tetraisopropoxide (C 12 H 28 O 4 Ti) and H 2 O was used as the precursor and Ar was used as the carrier gas. Six deposition cycles were performed at 150 °C. 12 H 28 O 4 The pulse, breath holding and purge times of Ti were 0.5 s, 8 s and 25 s respectively; H 2 The pulse, breath-hold, and purge times of O were 0.1 s, 8 s, and 25 s, respectively;

[0054] S3 Preparation of Pt-modified TiO by ALD technology 2 / CeO 2 Catalyst: TiO prepared in step S2 2 / CeO 2 The catalyst was used for Pt atomic deposition. The Pt deposition was carried out in the form of (trimethyl)methylcyclopentadienylplatinum(IV) (MeCpPtMe 3 ) and O 3 As precursor, Ar as carrier gas, 2 deposition cycles were performed at 250 °C; MeCpPtMe 3 The pulse, breath holding and purge times were 0.5 s, 15 s and 25 s respectively; 3 The pulse, gas holding and purge times were 1 s, 10 s and 25 s respectively. The prepared catalyst was denoted as Pt-6TiO 2 / CeO 2 .

[0055] Comparative Example 5

[0056] Comparative Example 5 Preparation of TiO by Traditional Impregnation Method 2 -Pt@CeO 2 Catalyst: prepared by equal volume impregnation method with 6TiO 2 -Pt / CeO 2 TiO with the same Ti and Pt loading 2 -Pt@CeO 2 The catalyst used isopropyl titanate and chloroplatinic acid as the Ti source and Pt source respectively. The specific steps are as follows: CeO 2The carrier was mixed with chloroplatinic acid / ethanol solution, stirred and evaporated at 60 °C, and then heated to 400 °C at a heating rate of 5 °C / min and calcined in air for 4 h to obtain Pt@CeO 2 Catalyst; then burn the Pt@CeO 2 The catalyst was mixed with isopropyl titanate / ethanol solution, and the above evaporation and calcination process was repeated to obtain TiO 2 -Pt@CeO 2 catalyst.

[0057] Comparative Example 6

[0058] The difference from Example 1 is that in step S3, TiO 2 The deposition times were 60 times and the loading amount was CeO 2 18.4% of the carrier mass.

[0059] Catalyst performance evaluation

[0060] The performance evaluation method of the catalyst-catalyzed water-gas shift hydrogen production is as follows: a small fixed-bed continuous flow reaction evaluation device is used, and the reactants and products are analyzed using a GC-7920 gas chromatograph (Beijing Zhongjiao Jinyuan Technology Co., Ltd.), which is equipped with a hydrogen flame ionization detector (FID) for detecting CO and CO 2 (Converted into CH by built-in nickel furnace 4 A thermal conductivity detector (TCD) is also used to detect H 2 During the test, 20 mg of the catalyst and 80 mg of quartz sand were mixed and placed in a quartz tube (inner diameter 6 mm) after sieving the tablets. The reaction temperature was controlled by a temperature-programmed reactor. A mass flow meter was used to control the reaction gas flow, which consisted of 2% CO, 8 vol.% water vapor, and N as the balance gas. 2 The catalyst was introduced into the reaction bed at a total flow rate of 25 mL / min and the space velocity (GHSV) was 75000 mL·g -1 ·h -1 ; In the reaction gas atmosphere, in-situ activation was carried out at 300℃ for 0.5h; then the temperature was lowered to room temperature, and the same reaction gas composition as in the pretreatment was continued to be introduced, the reaction temperature was 180-300℃, and each temperature point was stabilized for at least 30min before sampling and analysis. Stability measurement was carried out at 2% CO and 8vol.%H 2 O / N 2 , total flow rate 30mL / min, GHSV = 90000mL·g -1 ·h -1 , the reaction temperature is 240℃ and 280℃.

[0061] The performance evaluation results of the catalysts of Examples 1-3 and Comparative Examples 1-6 are shown in Table 1:

[0062] Table 1 Evaluation results of water-gas shift activity of catalysts of Examples 1-3 and Comparative Examples 1-6 under different conditions

[0063]

[0064] From Table 1 and Figure 1 It can be seen that compared with Example 1, the TiO 2 / CeO 2 , Nb 2 O 5 / CeO 2 and SnO 2 / CeO 2 The CO conversion rate of the catalyst in water-gas shift hydrogen production is extremely low, which indicates that TiO 2 , Nb 2 O 5 SnO 2 and CeO 2 The 6TiO2 itself has almost no catalytic activity for the water-gas shift reaction. 2 -Pt / CeO 2 、6Nb 2 O 5 -Pt / CeO 2 、6Nb 2 O 5 -Pt / CeO 2 The catalyst is better than the unassisted Pt / CeO 2 The catalyst exhibited higher water-gas shift activity due to the presence of TiO 2 , Nb 2 O 5 SnO 2 The addition of metal oxide additives modified Pt-CeO 2 interface, regulates the metal-support interaction, and changes the electronic state of Pt single atoms / clusters, making it more favorable for CO and H 2 O activation, thereby increasing the Pt / CeO 2 Water-gas shift activity of catalysts.

[0065] Comparative Example 4 Compared with Example 1, the Pt and TiO 2 The deposition sequence of Pt-6TiO 2 / CeO 2 Catalyst ratio 6TiO 2 -Pt / CeO 2The low catalyst activity further indicates that the role of the metal oxide additive is to modify the metal-support interface. Different deposition orders result in different interfaces. 2 It is more conducive to improving the water-gas shift activity of the catalyst. Compared with Example 1, the TiO 2 -Pt@CeO 2 The catalyst activity is poor because the Pt and metal oxide additives obtained by the ALD method can be more evenly and highly dispersed on the support surface, and the ALD technology also helps to construct the interface structure more accurately.

[0066] also, Figure 2 Comparison of different TiO 2 Doping amount of Pt / CeO 2 The water-gas shift activity of the catalyst can be seen from the figure. When TiO 2 When the number of ALD depositions of TiO increases from 2 to 6, the CO conversion rate in the low temperature section (T<240℃) increases significantly. 2 When the number of ALD depositions continued to increase to 12, the CO conversion rate in the low temperature section was lower than that of 6TiO 2 -Pt / CeO 2 catalyst, but still higher than that of Pt / CeO without additive 2 Catalyst. As can be seen from Table 1, the 60TiO 2 -Pt / CeO 2 The catalyst activity is much lower than that of Pt / CeO without additives. 2 catalyst, this is because the excess TiO 2 The Pt active sites are covered, resulting in a decrease in catalyst activity.

[0067] The catalyst stability evaluation results of Example 1 are shown in Tables 2 and Figure 3 As shown:

[0068] Table 2 Stability evaluation results of the catalyst of Example 1 in the water-gas shift reaction

[0069]

[0070] From Table 2 and Figure 3 It can be seen that xTiO 2 -Pt / CeO 2 (x=2, 6) The catalyst has extremely high stability. -1 ·h -1 The catalytic activity did not decrease significantly after continuous reaction for 28 h at a high space velocity.

Claims

1. A method for preparing a highly stable modified supported metal catalyst, characterized in that: The following steps are involved: S1 prepares a metal oxide support; S2: uniformly dispersing the metal oxide support powder of step S1 on a frosted glass sheet, and performing noble metal deposition by atomic layer deposition to obtain a single atom or sub-nano cluster supported catalyst; S3: The supported catalyst obtained in step S2 is again subjected to atomic layer deposition to deposit niobium oxide, SnO2 or TiO2 metal oxide to obtain a supported metal catalyst modified with a metal oxide; In step S1, the metal oxide carrier is CeO2, TiO2 or an iron oxide carrier; In step S3, the number of depositions of the metal oxide is 2-15 times, and the loading amount of the metal oxide is 0.5-5% of the mass of the metal oxide carrier.

2. The method for preparing a highly stable modified supported metal catalyst according to claim 1, characterized in that: In step S1, a metal oxide support is prepared by a hydrothermal synthesis method.

3. The method for preparing a highly stable modified supported metal catalyst according to claim 1, characterized in that: In step S2, the noble metal is Pt, Au or Ir.

4. The method for preparing a highly stable modified supported metal catalyst according to claim 1, characterized in that: In step S2, the noble metal is deposited 2-20 times, and the loading amount of the noble metal is 0.5-2% of the mass of the metal oxide carrier.

5. A highly stable modified supported metal catalyst prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the highly stable modified supported metal catalyst prepared by the preparation method according to any one of claims 1 to 4 in water gas shift hydrogen production.