A lightweight, highly flame-retardant, high-speed fragment-proof composite layer and preparation method thereof
By adopting a lightweight high flame retardant and high-speed fracture composite layer in special equipment, combined with the specific structure of the shear energy-absorbing layer and the tensile energy-absorbing layer, the problems of large weight of the protective structure and poor thermal insulation and flame-retardant effect are solved, and the problem of The balance of high protection and high flame retardant performance improves the equipment's anti-secondary fracture capability and service life.
Patent Information
- Application Number
- CN202410827236.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-06-25
AI Technical Summary
In the prior art, the protective structure of special equipment must be considered lightweight and has poor thermal insulation and flame retardant effects, which leads to easy combustion or temperature collection during fire strikes, affecting the protective performance and service life, and the weight of the protective structure greatly affects the equipment. Mobility and flexibility.
Adopt lightweight, high flame retardant, high-speed fracture composite layer, including shear energy-absorbing layer and tensile energy-absorbing layer. The shear energy-absorbing layer is obtained by composite lamination of multi-layer aramid plain cloth and epoxy resin, and the tensile energy-absorbing layer is obtained by composite lamination of multi-layer aramid jelly fabric and epoxy resin. The layer is obtained by lamination of aramid fiber and UHMWPE fiber mixed fiber and polyurethane resin. The layer is obtained by combining the specific fiber layer structure and resin to achieve high flame retardant and high protection performance.
It achieves high protection performance and flame retardant performance under low surface density and thin thickness conditions, improves the anti-secondary fragmentation capability of special equipment, extends the service life of the protective structure, and improves the survivability of the equipment.
Smart Images

Figure CN118438754B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite layer structures, and in particular to a lightweight, highly flame-retardant and high-speed fragmentation-resistant composite layer and a preparation method thereof. Background Art
[0002] With the upgrading of modern weapons and equipment, the threats faced by special equipment such as helicopters and armored vehicles during combat have become more complex and diversified; therefore, the requirements for protective devices are also increasing. Reliable and effective protective devices can protect the key parts of the equipment, thereby increasing the survival probability of the equipment and combat personnel.
[0003] At present, for the internal protection of special equipment such as helicopters and armored vehicles, inorganic fiber winding molding or two-dimensional laminated fiber tissue is usually used to form a composite material structure to provide protection for the interior of special equipment such as helicopters and armored vehicles; however, the protection capability of this laminated structure is often closely related to the weight, that is, the laminated structure is heavy and thick, and the protection capability is strong. Conversely, the laminated structure is light and thick, and the protection capability is relatively weak; but an overly heavy protective structure will seriously affect the maneuverability and flexibility of the equipment, reduce the combat capability of the special equipment, and increase the probability of the special equipment being hit by firepower. At the same time, during the fire strike, not only will the special equipment be subjected to high-intensity instantaneous fragment impact, but local high temperature and burning phenomena will also occur, thereby accelerating the aging, damage and falling off of the protective structure, causing the special equipment to lose its internal protective function; however, the current protective structure has poor thermal insulation and flame retardant effects due to the need to consider lightweight, resulting in local combustion or temperature convergence points at the struck points of the protective structure during actual fire strikes, which poses a risk of causing equipment combustion and damage. It also accelerates the aging of the protective structure, reduces the service life of the protective structure, and causes weak points in the entire protective structure, affecting the overall protective performance. Summary of the invention
[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a lightweight, highly flame-retardant and anti-high-speed fragmentation composite layer. The composite layer structure takes into account the requirements of lightweight, high flame retardancy and high protection performance, provides effective secondary fragmentation protection for the interior of special equipment, and avoids the problem of decreased protection capability caused by temperature and flame combustion during fire strikes.
[0005] Another object of the present invention is to provide a method for preparing a lightweight, highly flame-retardant and high-speed fragment-proof composite layer.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A lightweight, highly flame-retardant and high-speed fragmentation-proof composite layer comprises a shear energy absorption layer and a tensile energy absorption layer, wherein encapsulation layers are respectively arranged on the side surfaces of the shear energy absorption layer and the tensile performance layer which are away from each other; the shear energy absorption layer is obtained by composite lamination of multiple layers of aramid plain weave cloth and epoxy resin; the tensile energy absorption layer is obtained by composite lamination of multiple layers of mixed fibers and polyurethane resin, wherein a single layer of mixed fibers is composed of aramid fibers and UHMWPE fibers, and two adjacent layers of the multiple layers of mixed fibers are in an orthogonal stacking form.
[0008] Based on further optimization of the above solution, the thickness of the composite layer is no more than 10 mm.
[0009] Based on the further optimization of the above scheme, the encapsulation layer adopts 1 to 5 layers with a density of 200±30g / m 2 When the encapsulating layer of basalt fiber plain weave fabric is not less than two layers, the fibers between the multiple layers of basalt fiber plain weave fabric are parallel to each other.
[0010] Based on the further optimization of the above scheme, the thickness of the shear energy absorption layer is 2 mm to 4 mm, and the surface density of the single-layer aramid plain fabric is 150 g / m 2 ~230g / m 2 , and the epoxy resin content in the shear energy absorption layer is 20% to 40%.
[0011] Based on further optimization of the above solution, in the shear energy absorption layer, the angle of the aramid fiber bundles (in the warp direction or weft direction) between two adjacent layers of aramid plain weave fabric is 30° to 45°.
[0012] The present application achieves strong impact and shear resistance under fire strikes by combining staggered and stacked aramid plain weave cloth with epoxy resin, which can effectively buffer and offset the impact in layers and reduce the rapid destruction of the shear energy absorption layer under instantaneous strong impact.
[0013] Based on further optimization of the above scheme, the thickness of the tensile energy absorbing layer is 4 mm to 7 mm, the tow ratio of the aramid fiber to the UHMWPE fiber of the single layer of hybrid fiber is 1:2, and the surface density of the single layer of hybrid fiber is 100 g / m 2 ~160g / m 2 ; The content of polyurethane resin in the tensile energy absorbing layer is 15% to 25%.
[0014] This application mixes aramid fibers and UHMWPE fibers of a specific tow ratio into a mixed fiber layer, and at the same time cooperates with polyurethane resin and multiple layers of mixed fiber layers orthogonally distributed. Under the premise of ensuring lightweight, firstly, the tensile energy absorption performance of the fibers is fully utilized and the anti-fragmentation performance of the tensile energy absorption layer is improved; secondly, the impact resistance and flame retardant performance are effectively balanced, and high flame retardant performance is achieved while ensuring high protection performance, thereby effectively offsetting the impact and high temperature under fire strikes, and reducing the problems of composite layer damage and peeling; thirdly, the staggered distribution of mixed fibers can effectively disperse instantaneous impact force and high temperature, avoid the formation of impact convergence points and high temperature convergence points, and provide effective protection for high energy dissipation. In addition, through the cooperation of the shear energy absorption layer and the tensile energy absorption layer, firstly, a stable combination between the two layers is ensured to avoid the weakening of interlayer bonding; secondly, by the method of shearing energy absorption first and then stretching energy absorption, the protection performance and service life of the structure are further improved, and the anti-fragmentation performance of the entire composite layer is effectively improved.
[0015] A method for preparing a lightweight, highly flame-retardant, high-speed fragmentation-resistant composite layer, used for preparing the above-mentioned composite layer structure, comprising:
[0016] Step 1, preparation of shear energy absorption layer: first, weave aramid fiber into aramid plain weave cloth, with the density of warp and weft directions being 9 to 10 strands / cm, to obtain a single-layer aramid plain weave cloth; then, impregnate the single-layer aramid plain weave cloth in epoxy resin to prepare prepreg; finally, stack the prepreg single-layer aramid plain weave cloth in sequence, and perform compression molding to obtain a shear energy absorption layer;
[0017] Step 2: Preparation of a tensile energy absorbing layer: First, aramid fiber and UHMWPE fiber are arranged in a ratio of 1:2 and prepared into a unidirectional prepreg with a formed polyurethane resin film; then, the unidirectional prepregs are orthogonally stacked in sequence and compression molded to obtain a tensile energy absorbing layer;
[0018] Step 3: Composite layer forming: First, lay down basalt fiber plain cloth to form a packaging layer for later use; then, lay down the packaging layer, tensile energy absorption layer, shear energy absorption layer, and packaging layer in sequence, and place a layer of hot melt adhesive film between the two layers to obtain the initial structure; then, place the initial structure in a vacuum bag and pre-vacuum it; finally, perform warm-pressing compounding on the vacuum bag, and take it out when the temperature drops below 40°C to obtain the composite layer structure.
[0019] Based on further optimization of the above scheme, the compression molding in step 1 is carried out under the conditions of 100° C. to 130° C. and 2 MPa to 4 MPa, and the heat preservation and pressure holding time is 90 min to 120 min.
[0020] Based on further optimization of the above scheme, the compression molding in the step 2 is carried out under the conditions of 115° C. to 130° C. and 18 MPa to 22 MPa, and the heat and pressure holding time is 60 min to 80 min.
[0021] Based on further optimization of the above scheme, the vacuum degree of the vacuum bag after pre-vacuuming in step three is 92 kPa to 98 kPa; the temperature of the warm-pressing compound is 100° C. to 120° C., and the insulation time is 120 min to 150 min.
[0022] The present invention has the following technical effects:
[0023] The lightweight, highly flame-retardant and high-speed fragment-proof composite layer structure prepared in the present application has the characteristics of low surface density, thin thickness, high protection, high flame retardancy, high weather resistance, and low cost. Through the specific fiber layer structure distribution, stacking and matching with specific resins, it can effectively balance lightweight, high flame retardancy and high protection performance, so that the surface density is not more than 10kg / m 2 , under the condition that the thickness does not exceed 10mm, the ballistic limit V50 speed reaches more than 700m / s and the flame retardant performance reaches V-0 level. The composite layer structure can be used directly as the floor of the equipment, or a decorative surface layer can be added to the surface of the composite layer as the lining of the equipment. It can greatly improve the ability of existing equipment to prevent secondary fragments, protect the safety of personnel and equipment inside the equipment, and effectively improve the survivability of special equipment such as helicopters and ground armored vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of the composite layer in an embodiment of the present invention.
[0025] Figure 2 Schematic diagram of stacking the shear energy absorbing layer in an embodiment of the present invention.
[0026] Figure 3 Schematic diagram of stacking the stretched energy absorbing layer in an embodiment of the present invention.
[0027] Figure 4 1 is a flow chart for preparing the composite layer in an embodiment of the present invention.
[0028] Figure 5 This is a physical picture of the ballistic limit V50 test of the composite layer in an embodiment of the present invention.
[0029] Among them, 10, shear energy absorption layer; 20, tensile energy absorption layer; 21, aramid fiber; 22, UHMWPE fiber; 30, packaging layer. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0031] Embodiment 1:
[0032] A lightweight, highly flame-retardant, high-speed fragmentation-resistant composite layer, such as Figure 1 As shown: the thickness of the composite layer is not more than 10mm, including a shear energy absorption layer 10 and a tensile energy absorption layer 20, and a packaging layer 30 is respectively arranged on the side of the shear energy absorption layer 10 and the tensile performance layer away from each other; the packaging layer 30 adopts a 1-layer surface density of 230g / m 2 The shear energy absorption layer 10 is obtained by composite lamination of multiple layers of aramid plain weave cloth and epoxy resin; wherein the thickness of the shear energy absorption layer 10 is 2 mm, and the surface density of the single layer of aramid plain weave cloth is 150 g / m 2 The epoxy resin content in the shear energy absorbing layer 10 is 20%. At the same time, in the shear energy absorbing layer 10, the angle of the aramid fiber 21 tows (warp or weft) between two adjacent layers of aramid plain weave fabric is 30° (that is, the warp angle of the two adjacent layers of aramid plain weave fabric is 30°, and the weft angle is 30°, such as Figure 2 The tensile energy absorbing layer 20 is obtained by composite lamination of multiple layers of hybrid fibers and polyurethane resin, and the thickness of the tensile energy absorbing layer 20 is 7 mm; wherein the single layer of hybrid fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the tow ratio of the aramid fibers 21 to the UHMWPE fibers 22 is 1:2 (see Figure 3 As shown), the surface density of the single layer of hybrid fibers is 100g / m 2 , and the content of polyurethane resin in the tensile energy absorbing layer 20 is 15%, and the adjacent two layers of multi-layer hybrid fibers are in an orthogonal stacking form (that is, the tows of the adjacent two layers of single-layer hybrid fiber layers are perpendicular to each other, such as Figure 3 as shown).
[0033] The specific preparation method of the above composite layer is:
[0034] Step 1: Preparation of shear energy absorption layer 10: First, aramid fiber 21 is woven into aramid plain weave cloth with a warp and weft density of 9 strands / cm to obtain a single-layer aramid plain weave cloth with a density of 150 g / m 3; Then, a single layer of aramid plain fabric is impregnated in epoxy resin to prepare a prepreg, wherein the content of the epoxy resin is 20%; finally, the prepreg single layer of aramid plain fabric is stacked in sequence at an angle of 30°, and compression molded at 100°C and 2MPa, and the heat preservation and pressure holding time is 90 minutes, thereby obtaining a shear energy absorption layer 10;
[0035] Step 2, preparation of the tensile energy absorbing layer 20: First, the aramid fiber 21 and the UHMWPE fiber 22 are arranged in a ratio of 1:2 and prepared into a unidirectional prepreg with a formed polyurethane resin film, wherein the content of the polyurethane resin is 15%; then, the unidirectional prepregs are orthogonally stacked in sequence, and compression molded at 115°C and 18MPa, and the heat preservation and pressure holding time is 60min, thereby obtaining the tensile energy absorbing layer 20;
[0036] Step 3, composite layer forming: first, stack basalt fiber plain cloth to form a packaging layer 30 for standby use; then, stack the packaging layer 30, the tensile energy absorption layer 20, the shear energy absorption layer 10, and the packaging layer 30 in sequence, and place a layer of hot melt adhesive film (conventional hot melt adhesive film can be used) between the two layers to obtain an initial structure; then, place the initial structure in a vacuum bag and pre-vacuum it with a vacuum degree of 98 kPa; finally, place the vacuum bag in an environment with a vacuum bag temperature of 100°C and keep it warm for 120 minutes for warm-pressing compounding, and take it out when the temperature drops below 40°C to obtain a composite layer structure.
[0037] Embodiment 2:
[0038] A lightweight, highly flame-retardant, high-speed fragmentation-resistant composite layer, such as Figure 1 As shown: the thickness of the composite layer is not more than 10mm, including a shear energy absorption layer 10 and a tensile energy absorption layer 20, and a packaging layer 30 is respectively arranged on the side away from the shear energy absorption layer 10 and the tensile performance layer; the packaging layer 30 adopts a 3-layer surface with a density of 200g / m 2 The basalt fiber plain weave fabric (the thickness of a single layer of basalt fiber plain weave fabric is 0.35 mm, that is, the thickness of the encapsulation layer 30 in this embodiment is 1.05 mm), and the fibers between the three layers of basalt fiber plain weave fabric are parallel to each other (that is, there is no angle between the warp yarns or weft yarns of adjacent basalt fiber plain weave fabrics). The shear energy absorption layer 10 is obtained by composite lamination of multiple layers of aramid plain weave fabric and epoxy resin; wherein, the thickness of the shear energy absorption layer 10 is 3 mm, and the surface density of the single layer of aramid plain weave fabric is 190 g / m 2 , and the epoxy resin content in the shear energy absorbing layer 10 is 30%. At the same time, in the shear energy absorbing layer 10, the angle of the aramid fiber 21 tows (warp or weft) between two adjacent layers of aramid plain weave cloth is 38° (that is, the warp angle of the two adjacent layers of aramid plain weave cloth is 38°, and the weft angle is 38°, such as Figure 2The tensile energy absorbing layer 20 is obtained by composite lamination of multiple layers of hybrid fibers and polyurethane resin, and the thickness of the tensile energy absorbing layer 20 is 5 mm; wherein the single layer of hybrid fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the tow ratio of the aramid fibers 21 to the UHMWPE fibers 22 is 1:2 (see Figure 3 As shown), the surface density of the single layer of hybrid fibers is 130g / m 2 , and the content of polyurethane resin in the tensile energy absorbing layer 20 is 20%, and the adjacent two layers of multi-layer hybrid fibers are in an orthogonal stacking form (that is, the tows of the adjacent two layers of single-layer hybrid fiber layers are perpendicular to each other, such as Figure 3 as shown).
[0039] The specific preparation method of the above composite layer is:
[0040] Step 1: Preparation of shear energy absorption layer 10: First, aramid fiber 21 is woven into aramid plain weave cloth with a warp and weft density of 10 strands / cm to obtain a single-layer aramid plain weave cloth with a density of 190 g / m 3 ; Then, a single-layer aramid plain fabric is impregnated in epoxy resin to prepare a prepreg, wherein the content of the epoxy resin is 30%; finally, the prepreg single-layer aramid plain fabric is stacked in sequence at an angle of 38°, and compression molded at 115°C and 3MPa, and the heat preservation and pressure holding time is 105min, thereby obtaining a shear energy absorption layer 10;
[0041] Step 2, preparation of the tensile energy absorbing layer 20: First, the aramid fiber 21 and the UHMWPE fiber 22 are arranged in a ratio of 1:2 and prepared into a unidirectional prepreg with a formed polyurethane resin film, wherein the content of the polyurethane resin is 20%; then, the unidirectional prepregs are orthogonally stacked in sequence, and compression molded at 125°C and 20MPa, and the heat preservation and pressure holding time is 70 minutes, thereby obtaining the tensile energy absorbing layer 20;
[0042] Step 3, composite layer forming: first, stack basalt fiber plain cloth to form a packaging layer 30 for standby use; then, stack the packaging layer 30, the tensile energy absorption layer 20, the shear energy absorption layer 10, and the packaging layer 30 in sequence, and place a layer of hot melt adhesive film (conventional hot melt adhesive film can be used) between the two layers to obtain an initial structure; then, place the initial structure in a vacuum bag and pre-vacuum it with a vacuum degree of 95kPa; finally, place the vacuum bag in an environment with a vacuum bag temperature of 110°C and keep it warm for 135 minutes for warm-pressing compounding, and take it out when the temperature drops below 40°C to obtain a composite layer structure.
[0043] Embodiment 3:
[0044] A lightweight, highly flame-retardant, high-speed fragmentation-resistant composite layer, such as Figure 1As shown: the thickness of the composite layer is not more than 10mm, including a shear energy absorption layer 10 and a tensile energy absorption layer 20, and a packaging layer 30 is respectively arranged on the side away from the shear energy absorption layer 10 and the tensile performance layer; the packaging layer 30 adopts a 5-layer surface with a density of 170g / m 2 The basalt fiber plain weave cloth (the thickness of a single layer of basalt fiber plain weave cloth is 0.35 mm, that is, the thickness of the packaging layer 30 in this embodiment is 1.75 mm), if the basalt fiber plain weave cloth of the packaging layer 30 is not less than two layers, the fibers between the multiple layers of basalt fiber plain weave cloth are parallel to each other. The shear energy absorption layer 10 is obtained by composite lamination of multiple layers of aramid plain weave cloth and epoxy resin; wherein, the thickness of the shear energy absorption layer 10 is 4 mm, and the surface density of the single layer of aramid plain weave cloth is 230 g / m 2 , and the epoxy resin content in the shear energy absorbing layer 10 is 40%. At the same time, in the shear energy absorbing layer 10, the angle of the aramid fiber 21 tows (warp or weft) between two adjacent layers of aramid plain weave cloth is 45° (that is, the warp angle of the two adjacent layers of aramid plain weave cloth is 45°, and the weft angle is 45°, such as Figure 2 The tensile energy absorbing layer 20 is obtained by composite lamination of multiple layers of hybrid fibers and polyurethane resin, and the thickness of the tensile energy absorbing layer 20 is 4 mm; wherein the single layer of hybrid fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the tow ratio of the aramid fibers 21 to the UHMWPE fibers 22 is 1:2 (see Figure 3 As shown), the surface density of the single layer of hybrid fibers is 160g / m 2 , and the content of polyurethane resin in the tensile energy absorbing layer 20 is 25%, and the adjacent two layers of multi-layer hybrid fibers are in an orthogonal stacking form (that is, the tows of the adjacent two layers of single-layer hybrid fiber layers are perpendicular to each other, such as Figure 3 as shown).
[0045] The specific preparation method of the above composite layer is:
[0046] Step 1: Preparation of shear energy absorption layer 10: First, aramid fiber 21 is woven into aramid plain weave cloth with a warp and weft density of 10 strands / cm to obtain a single-layer aramid plain weave cloth with a density of 230 g / m 3 ; Then, a single layer of aramid plain fabric is impregnated in epoxy resin to prepare a prepreg, wherein the content of the epoxy resin is 40%; finally, the prepreg single layer of aramid plain fabric is stacked in sequence at an angle of 45°, and compression molded at 130°C and 4MPa, and the heat preservation and pressure holding time is 120min, thereby obtaining a shear energy absorption layer 10;
[0047] Step 2, preparation of the tensile energy absorbing layer 20: First, the aramid fiber 21 and the UHMWPE fiber 22 are arranged in a ratio of 1:2 and prepared into a unidirectional prepreg with a formed polyurethane resin film, wherein the content of the polyurethane resin is 25%; then, the unidirectional prepregs are orthogonally stacked in sequence, and compression molded at 130°C and 22MPa, and the heat preservation and pressure holding time is 80min, thereby obtaining the tensile energy absorbing layer 20;
[0048] Step 3, composite layer forming: first, stack basalt fiber plain weave cloth to form a packaging layer 30 for standby use; then, stack the packaging layer 30, the tensile energy absorption layer 20, the shear energy absorption layer 10, and the packaging layer 30 in sequence, and place a layer of hot melt adhesive film (conventional hot melt adhesive film can be used) between the two layers to obtain an initial structure; then, place the initial structure in a vacuum bag and pre-vacuum it with a vacuum degree of 92 kPa; finally, place the vacuum bag in an environment with a vacuum bag temperature of 120°C and keep it warm for 150 minutes for warm-pressing compounding, and take it out when the temperature drops below 40°C to obtain a composite layer structure.
[0049] Comparative Example 1:
[0050] A composite layer structure, using the same structural layer distribution as in Example 2, the encapsulation layer 30 uses 3 layers with a surface density of 200g / m 2 Basalt fiber plain cloth (the thickness of a single layer of basalt fiber plain cloth is 0.35 mm). The thickness of the shear energy absorption layer 10, the surface density of the single layer of aramid plain cloth, and the epoxy resin content are all consistent with those in Example 2. At the same time, the angle of the aramid fiber 21 bundle (warp or weft) between two adjacent layers of aramid plain cloth is 38°. The tensile energy absorption layer 20 is obtained by composite lamination of multiple layers of mixed fibers and polyurethane resin, and the thickness of the tensile energy absorption layer 20 is 5 mm; wherein, the single layer of mixed fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the bundle ratio of aramid fibers 21 to UHMWPE fibers 22 is 1:1, and the surface density of the single layer of mixed fibers is 130 g / m 2 , and the content of polyurethane resin in the tensile energy absorbing layer 20 is 20%, and the adjacent two layers of the multi-layer hybrid fibers are in an orthogonal stacking form.
[0051] The composite layer structure is prepared by the method described in Example 2, except that during the preparation of the tensile energy absorbing layer 20, the aramid fiber 21 and the UHMWPE fiber 22 are arranged in a ratio of 1:1.
[0052] Comparative Example 2:
[0053] A composite layer structure, using the same structural layer distribution as in Example 2, the encapsulation layer 30 uses 3 layers with a surface density of 200g / m 2Basalt fiber plain cloth (the thickness of a single layer of basalt fiber plain cloth is 0.35 mm). The thickness of the shear energy absorption layer 10, the surface density of the single layer of aramid plain cloth, and the epoxy resin content are all consistent with those in Example 2. At the same time, the angle of the aramid fiber 21 bundle (warp or weft) between two adjacent layers of aramid plain cloth is 38°. The tensile energy absorption layer 20 is obtained by composite lamination of multiple layers of mixed fibers and polyurethane resin, and the thickness of the tensile energy absorption layer 20 is 5 mm; wherein, the single layer of mixed fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the bundle ratio of aramid fibers 21 to UHMWPE fibers 22 is 1:3, and the surface density of the single layer of mixed fibers is 130 g / m 2 , and the content of polyurethane resin in the tensile energy absorbing layer 20 is 20%, and the adjacent two layers of the multi-layer hybrid fibers are in an orthogonal stacking form.
[0054] The composite layer structure is prepared by the method described in Example 2, except that during the preparation of the tensile energy absorbing layer 20, the aramid fibers 21 and the UHMWPE fibers 22 are arranged in a ratio of 1:3.
[0055] Comparative Example 3:
[0056] A composite layer structure, using the same structural layer distribution as in Example 2, the encapsulation layer 30 uses 3 layers with a surface density of 200g / m 2 Basalt fiber plain cloth (the thickness of a single layer of basalt fiber plain cloth is 0.35 mm). The thickness of the shear energy absorption layer 10, the surface density of the single layer of aramid plain cloth, and the epoxy resin content are all consistent with those in Example 2. At the same time, the angle of the aramid fiber 21 bundle (warp or weft) between two adjacent layers of aramid plain cloth is 38°. The tensile energy absorption layer 20 is obtained by composite lamination of multiple layers of mixed fibers and epoxy resin, and the thickness of the tensile energy absorption layer 20 is 5 mm; wherein, the single layer of mixed fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the bundle ratio of aramid fibers 21 to UHMWPE fibers 22 is 1:2, and the surface density of the single layer of mixed fibers is 130 g / m 2 , and the content of epoxy resin in the tensile energy absorbing layer 20 is 20%, and the adjacent two layers of the multi-layer hybrid fibers are in an orthogonal stacking form.
[0057] The above-mentioned composite layer structure is prepared by the method described in Example 2, except that: during the preparation of the tensile energy absorption layer 20, the aramid fiber 21 and the UHMWPE fiber 22 are arranged in a ratio of 1:2 and prepared into a unidirectional prepreg with a molded epoxy resin film, and the epoxy resin content is 20%.
[0058] Comparative Example 4:
[0059] A composite layer structure, using the same structural layer distribution as in Example 2, the encapsulation layer 30 uses 3 layers with a surface density of 200g / m 2 Basalt fiber plain cloth (the thickness of a single layer of basalt fiber plain cloth is 0.35 mm). The thickness of the shear energy absorption layer 10, the surface density of the single layer of aramid plain cloth, and the epoxy resin content are all consistent with those in Example 2. At the same time, the angle of the aramid fiber 21 bundle (warp or weft) between two adjacent layers of aramid plain cloth is 38°. The tensile energy absorption layer 20 is obtained by composite lamination of multiple layers of mixed fibers and polyurethane resin, and the thickness of the tensile energy absorption layer 20 is 5 mm; wherein, the single layer of mixed fibers is composed of aramid fibers 21 and UHMWPE fibers 22, and the bundle ratio of aramid fibers 21 to UHMWPE fibers 22 is 1:2, and the surface density of the single layer of mixed fibers is 130 g / m 2 , and the content of polyurethane resin in the tensile energy absorbing layer 20 is 20%, and the angle of fiber bundles between two adjacent layers of the multi-layer mixed fiber is 45°.
[0060] The composite layer structure is prepared by the method described in Example 2, except that during the preparation of the tensile energy absorbing layer 20, the unidirectional prepregs are stacked in sequence at an angle of 45°.
[0061] Comparative Example 5:
[0062] A composite layer structure, using the same structural layer distribution as in Example 2, the encapsulation layer 30 uses 3 layers with a surface density of 200g / m 2 The thickness of the shear energy absorbing layer 10, the surface density of the single-layer aramid plain cloth, and the epoxy resin content are all consistent with those in Example 2. At the same time, the angle of the aramid fiber 21 tows (warp or weft) between two adjacent layers of aramid plain cloth is 60°. The structure of the tensile energy absorbing layer 20 is completely consistent with that in Example 2.
[0063] The composite layer structure is prepared by the method described in Example 2, except that: during the preparation of the shear energy absorption layer 10, the pre-impregnated single-layer aramid plain fabric is stacked in sequence at an angle of 60°.
[0064] Comparative Example 6:
[0065] A composite layer structure, using the same structural layer distribution as in Example 2, the encapsulation layer 30 uses 3 layers with a surface density of 200g / m 2 The shear energy absorption layer 10 is obtained by composite lamination of multiple layers of aramid plain weave fabric and polyurethane resin; wherein, the thickness of the shear energy absorption layer 10 is 3 mm, and the surface density of the single layer of aramid plain weave fabric is 190 g / m2 , and the polyurethane resin content in the shear energy absorbing layer 10 is 30%. At the same time, in the shear energy absorbing layer 10, the angle of the aramid fiber 21 tow (warp or weft) between two adjacent layers of aramid plain fabric is 38°. The structure of the tensile energy absorbing layer 20 is completely consistent with that in Example 2.
[0066] The composite layer structure is prepared by the method described in Example 2, except that during the preparation of the shear energy absorbing layer 10, a single layer of aramid plain fabric is impregnated in polyurethane resin to prepare a prepreg.
[0067] The composite layers prepared in Example 1, Example 2, and Example 3 and the composite layer structures prepared in Comparative Examples 1 to 6 were respectively subjected to a V50 ballistic limit test and a flame retardant grade test by a vertical combustion method. The test results are shown in the following table:
[0068]
[0069] It can be clearly seen from the above table that when the ratio of aramid fiber 21 to UHMWPE fiber 22 bundles in the stretched energy absorbing layer 20 changes, the ballistic limit and flame retardant grade of the composite layer structure will change differently. It can be seen from Example 2 and Comparative Example 1 that when the ratio of aramid fiber 21 bundles in the single-layer unidirectional prepreg in the stretched energy absorbing layer increases, the ballistic limit V50 (representing the anti-fragmentation performance) of the composite layer structure decreases significantly; it can be seen from Example 2 and Comparative Example 2 that when the ratio of UHMWPE fiber 22 bundles in the single-layer unidirectional prepreg in the stretched energy absorbing layer 20 increases, the flame retardant property is estimated to decrease significantly. At the same time, it can be seen from Example 2 and Comparative Example 3 that when the pull-up energy absorption layer uses epoxy resin to replace polyurethane resin, the ballistic limit V50 (representing the anti-fragmentation performance) of the composite layer structure is significantly reduced; it can be seen from Example 2 and Comparative Example 4 that when the ply angle of the unidirectional prepreg of the stretch energy absorption layer 20 is changed, the ballistic limit V50 (representing the anti-fragmentation performance) and flame retardant performance of the composite layer structure are significantly reduced. In addition, it can be seen from Example 2 and Comparative Example 5 that when the ply angle of the shear energy absorption layer 10 is changed, the ballistic limit V50 (representing the anti-fragmentation performance) and flame retardant performance of the composite layer structure are significantly reduced; it can be seen from Example 2 and Comparative Example 6 that when the epoxy resin in the shear energy absorption layer 10 is replaced by polyurethane resin, the ballistic limit V50 (representing the anti-fragmentation performance) of the composite layer structure is significantly reduced; it proves that the need to simultaneously obtain excellent anti-fragmentation energy absorption and flame retardant performance requires the specific structural coordination of the shear energy absorption layer 10 and the stretch energy absorption layer 20 to achieve.
Claims
1. A lightweight, highly flame-retardant, high-speed fragment-proof composite layer, characterized by: It includes a shear energy absorption layer and a tensile energy absorption layer, and a packaging layer is respectively arranged on the side of the shear energy absorption layer and the tensile performance layer away from each other; the packaging layer adopts 1 to 5 layers with a density of 200±30g / m 2 The shear energy absorption layer is obtained by laminating multiple layers of aramid plain fabric and epoxy resin. The thickness of the shear energy absorption layer is 2 mm to 4 mm, and the surface density of the single-layer aramid plain fabric is 150 g / m 2 ~230g / m 2 , and the epoxy resin content in the shear energy absorption layer is 20% to 40%; in the shear energy absorption layer, the angle of the aramid fiber tow between two adjacent layers of aramid plain fabric is 30° to 45°; the tensile energy absorption layer is obtained by composite lamination of multiple layers of hybrid fibers and polyurethane resin, the single layer of hybrid fibers is composed of aramid fibers and UHMWPE fibers, and the adjacent two layers of the multi-layer hybrid fibers are orthogonally stacked, the thickness of the tensile energy absorption layer is 4 mm to 7 mm, the tow ratio of aramid fibers to UHMWPE fibers in the single layer of hybrid fibers is 1:2, and the surface density of the single layer of hybrid fibers is 100 g / m 2 ~160g / m 2 ; The content of polyurethane resin in the tensile energy absorbing layer is 15% to 25%.
2. The lightweight, highly flame-retardant, high-speed fragment-proof composite layer according to claim 1, characterized in that: The thickness of the composite layer is not greater than 10 mm.
3. The method for preparing a lightweight, highly flame-retardant and high-speed fragment-proof composite layer according to claim 2, characterized in that: include: Step 1, preparation of shear energy absorption layer: first, aramid fiber is woven into aramid plain weave cloth, and the density in warp and weft directions is 9-10 strands / cm, so as to obtain a single-layer aramid plain weave cloth; then, the single-layer aramid plain weave cloth is impregnated in epoxy resin to prepare prepreg; finally, the prepreg single-layer aramid plain weave cloth is stacked in sequence, and compression molded to obtain a shear energy absorption layer; Step 2: Preparation of a tensile energy absorbing layer: First, aramid fiber and UHMWPE fiber are arranged in a ratio of 1:2 and prepared into a unidirectional prepreg with a formed polyurethane resin film; then, the unidirectional prepregs are orthogonally stacked in sequence and compression molded to obtain a tensile energy absorbing layer; Step 3, composite layer forming: first, stack basalt fiber plain cloth to form a packaging layer for use; then, stack the packaging layer, tensile energy absorption layer, shear energy absorption layer, and packaging layer in sequence, and place a layer of hot melt adhesive film between the two layers to obtain an initial structure; then, place the initial structure in a vacuum bag and pre-vacuum it; finally, perform warm-pressing compounding on the vacuum bag, and take it out when the temperature drops below 40°C to obtain the composite layer.
4. The method for preparing a lightweight, highly flame-retardant and high-speed fragment-proof composite layer according to claim 3, characterized in that: The compression molding in the step 1 is carried out at 100° C. to 130° C. and 2 MPa to 4 MPa, and the heat preservation and pressure preservation time is 90 min to 120 min.
5. The method for preparing a lightweight, highly flame-retardant and high-speed fragment-proof composite layer according to claim 3, characterized in that: The compression molding in the step 2 is carried out at 115° C. to 130° C. and 18 MPa to 22 MPa, and the heat preservation and pressure preservation time is 60 min to 80 min.
6. The method for preparing a lightweight, highly flame-retardant and high-speed fragment-proof composite layer according to claim 3, characterized in that: In the step 3, the vacuum degree of the vacuum bag after pre-vacuuming is 92 kPa to 98 kPa; the temperature of the warm-pressing compound is 100° C. to 120° C., and the insulation time is 120 min to 150 min.