A high-frequency, wide-temperature, ultra-low-loss ferrite core and a method for preparing the same

By adding specific dopants and steps to manganese zinc ferrite materials, high frequency wide temperature ultra-low loss ferrite cores are prepared, which solves the problem of high frequency loss of existing materials and achieves lower losses and better losses Wide operating temperature.

CN118439862BActive Publication Date: 2024-11-12HUBEI HUACI ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410505171.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-12
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

The power loss of existing manganese-zeb ferrite materials is still relatively high under high frequency conditions, especially at 100KHz, 200mT, and 80℃, which is 240kW/m3, which is difficult to further reduce.

Method used

The main formula is composed of Fe2O3, MnO, ZnO, and by adding CaCO3, CoSn(OH)6, Bi2O3, nano SiO2, composite dopants and YBCO, the composite dopants are prepared by using the method of preparation of composite dopants, including ball milling, pre-firing, and pelletization. and the sintering step, high frequency, wide temperature, ultra-low loss ferrite cores are prepared.

Benefits of technology

It effectively reduces high-frequency losses, improves the heat resistance and magnetic properties of the material, significantly reduces hysteresis losses, and widens the working temperature range of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004810053840000091
    Figure BDA0004810053840000091
Patent Text Reader

Abstract

The present invention belongs to the technical field of ferrite materials. The present invention provides a high-frequency, wide-temperature, ultra-low-loss ferrite core, including a main formula and a dopant formula, wherein the main formula components and proportions are: Fe2O3 70-72mol%, MnO 20-22mol%, ZnO 6-10mol%, and the proportions of each main formula total 100mol%; relative to the weight of the main formula, the components and weight percentages in the dopant formula are: CaCO3 1-1000PPM, CoSn(OH)6 100-150PPM, Bi2O3 50-100PPM, nano-SiO2 50-100PPM, and composite dopant 80-130PPM. The present invention studies and develops a manganese-zinc ferrite core with a wide operating temperature and ultra-low loss, which is of great significance to the development of the high-end product market of high-frequency ultra-low-loss ferrite cores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferrite materials, and in particular relates to a high-frequency, wide-temperature, ultra-low-loss ferrite core and a preparation method thereof. Background Art

[0002] Ferrite core is mainly composed of three metal elements: iron (Fe), manganese (Mn), and zinc (Zn), and is usually called manganese-zinc ferrite. In order to develop independent high-frequency, wide-temperature, ultra-low power loss soft magnetic ferrite materials, the applicant has previously applied for a Chinese authorized invention patent with the authorization announcement number CN114685154B, entitled A high-frequency, wide-temperature, ultra-low loss ferrite material and its preparation process. By adding Co2O3 to the dopant, the metal ion doping in Co2O3 will replace the Fe at the B position of the MnZn ferrite. 3+ and Mn 3+ , thereby increasing the AB super exchange effect, improving the heat resistance of the material, broadening the working temperature of the material, and increasing the Curie temperature of the material, which will also increase the density of the sintered ferrite and effectively increase the saturation magnetic induction intensity of the material. Although the high-frequency loss has been reduced to a certain extent, there is still room for reduction. For example, the manganese-zinc power ferrite material produced by foreign research has a power loss value of only 199kW / m at 100KHz, 200mT, and 80℃. 3 In this invention patent, the power loss value under the conditions of 100KHz, 200mT, and 80℃ is 240kW / m 3 ,Therefore, it is necessary to develop a ferrite core with lower high-frequency loss. Summary of the invention

[0003] The purpose of the present invention is to provide a high-frequency, wide-temperature, ultra-low-loss ferrite core and a preparation method thereof, which has the effect of low high-frequency loss.

[0004] The above technical objectives of the present invention are achieved through the following technical solutions: A high-frequency, wide-temperature, ultra-low-loss ferrite core, comprising a main formula and a dopant formula, wherein the main formula components and proportions are:

[0005] Fe2O3 70~72mol%

[0006] MnO 20~22mol%

[0007] ZnO 6~10mol%

[0008] The total proportion of each main formula is 100 mol%;

[0009] The components and weight percentages of the adulterated formulations relative to the weight of the main formulation are:

[0010] CaCO3 1~1000PPM

[0011] CoSn(OH)6 100~150PPM

[0012] Bi2O3 50~100PPM

[0013] Nano-SiO2 50~100PPM

[0014] Composite dopants 80~130PPM.

[0015] The composite dopant preparation method is as follows: CCTO thin film coated TiO2 is crushed to obtain the composite dopant, and the weight ratio of CCTO to TiO2 is 5:1.

[0016] The present invention is further configured as follows: the preparation method of the composite dopant is as follows: take a CCTO film, heat it up and keep it at 350°C, sprinkle it with TiO2 powder, and then coat a layer of CCTO film, and do this multiple times so that the TiO2 powder is between two adjacent CCTO film layers.

[0017] The present invention is further configured as follows: the dopant formula further includes 30-45 PPM of YBCO in terms of weight percentage.

[0018] The present invention is further configured as follows: wherein the components and proportions of the main formula are:

[0019] Fe2O3 72mol%

[0020] MnO 22mol%

[0021] ZnO 6mol%

[0022] The total proportion of each main formula is 100 mol%.

[0023] The present invention is further configured as follows: relative to the total amount of the main formula, the components and weight percentages in the dopant formula are respectively:

[0024] CaCO3 600PPM

[0025] CoSn(OH)6 110PPM

[0026] Bi2O3 70PPM

[0027] Nano-SiO2 70PPM

[0028] Composite dopant 100PPM.

[0029] The present invention also provides a method for preparing the above-mentioned high-frequency, wide-temperature, ultra-low-loss ferrite core, which is characterized by comprising the following steps:

[0030] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO powder and CoSn(OH)6 according to the ratio requirements, and mix them uniformly;

[0031] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;

[0032] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain pre-sintered powder;

[0033] Step S4: secondary batching: adding CaCO3, Bi2O3, nano-SiO2, composite dopant, and YBCO to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture;

[0034] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;

[0035] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;

[0036] Step S7: pressing and molding: pressing the granulated small particles into annular green billets on a pressing device;

[0037] Step S8: Secondary sintering: Sintering the annular green billet in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

[0038] The present invention is further configured as follows: the pre-burning temperature in step S3 is 800°C to 900°C.

[0039] The present invention is further configured as follows: the polysiloxane in step S4 is PSX700.

[0040] The present invention is further configured as follows: step S5' is further included between step S5 and step S6: rapid high-temperature impurity removal: placing the mixture after the secondary ball milling in an oven and heating it for 20-30 minutes.

[0041] The present invention is further configured as follows: the mixture is placed in an oven and heated to 400° C.-500° C.

[0042] The beneficial effects of the present invention are:

[0043] 1. In the prior art, after SnO2 enters the manganese-zinc ferrite, Sn 4+ Ions can replace part of the Fe 3+ The ions enter the spinel lattice of the ferrite. Sn 4+ Will be with Fe2+ Combination to form ion pairs, Fe 2+ ions to bind Fe 2+ Ions do not participate in the electron hopping mechanism, thus reducing high-frequency losses. 4+ As a commonly used dopant in the prior art, although it is helpful to reduce the loss of ferrite, the reduction is limited.

[0044] Sn 4+ Inevitably, a portion of the ferrite will remain at the grain boundary, promoting the growth of ferrite grains. Therefore, the present invention uses CoSn(OH)6, which can provide Sn during the sintering process. 4+ ions and Co 3+ ions, and pre-sinter them with the raw materials of the main formula in advance to reduce Sn at the grain boundaries 4+ The amount of ions is increased so that they can enter the crystal lattice as much as possible, which is conducive to obtaining smaller uniform grains, and can achieve better magnetic properties while further reducing high-frequency losses.

[0045] 3. Although TiO2 is a commonly used dopant to reduce losses, 4+ Mainly enter the lattice and replace part of Fe 3+ Ions enter the spinel lattice of ferrite and also react with Sn 4+ Will be with Fe 2+ Combining to form ion pairs to reduce high-frequency loss, but according to the law of charge conservation, it will inevitably produce a considerable amount of Fe 2+ , too much Fe 2+ This will cause the ferrite resistivity to decrease and the energy consumption to increase. 4+ Compared with CCTO in the prior art, the present invention ingeniously coats it with TiO2. When CCTO is enriched at the ferrite grain boundary, the TiO2 ions it coats can remain at the grain boundary, making Ti 4+ Not only will it enter the crystal lattice, but it will also remain at the grain boundary, working together with CCTO to significantly increase the grain boundary resistivity and further reduce high-frequency losses. 4+ , Ti 4+ Will not promote grain growth.

[0046] 4. Co of the present invention 3+It can improve the heat resistance of the material and expand the working temperature of the material, but it is easy to cause discontinuous growth and irregular crystallization of the soft magnet microstructure, and produce bubbles in various areas inside the crystal, thereby affecting the initial magnetic permeability and power loss performance of the material. Therefore, the added YBCO can be sintered. YBCO has a low melting point and can be melted and penetrated first to improve the connection between the grains, so that the material crystal growth is continuous, effectively reducing the generation of pores in the material, effectively reducing the hysteresis loss of the material, and reducing Co 3+ The adverse effects caused.

[0047] 5. The present invention studies and develops a manganese-zinc ferrite core with a wide operating temperature range and ultra-low loss, which is of great significance for opening up the high-end product market of high-frequency ultra-low loss ferrite cores. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Embodiment 1: A high-frequency, wide-temperature, ultra-low-loss ferrite core, wherein the components and proportions of the main formula are:

[0050] Fe2O3 72mol%

[0051] MnO 22mol%

[0052] ZnO 6mol%

[0053] The total proportion of each main formula is 100 mol%.

[0054] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:

[0055] CaCO3 600PPM

[0056] CoSn(OH)6 110PPM

[0057] Bi2O3 70PPM

[0058] Nano-SiO2 70PPM

[0059] Composite dopant 100PPM

[0060] YBCO 30PPM.

[0061] The preparation method of the composite dopant is as follows: take a CCTO film, heat it up and keep it at 350°C, sprinkle TiO2 powder on it, and then coat a layer of CCTO film, and do this multiple times so that the TiO2 powder is between two adjacent CCTO films. The weight ratio of CCTO to TiO2 is 5:1.

[0062] The method for preparing the high-frequency, wide-temperature, ultra-low-loss ferrite core comprises the following steps:

[0063] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO powder and CoSn(OH)6 according to the ratio requirements, and mix them uniformly;

[0064] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;

[0065] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain a pre-sintered powder; the pre-sintering temperature is 800°C to 900°C;

[0066] Step S4: secondary batching: adding CaCO3, Bi2O3, nano-SiO2, composite dopant, and YBCO to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture; the polysiloxane is PSX700;

[0067] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;

[0068] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;

[0069] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;

[0070] Step S7: pressing and molding: pressing the granulated small particles into annular green billets on a pressing device;

[0071] Step S8: Secondary sintering: Sintering the annular green billet in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

[0072] Embodiment 2: A high-frequency, wide-temperature, ultra-low-loss ferrite core, wherein the components and proportions of the main formula are:

[0073] Fe2O3 70mol%

[0074] MnO 20mol%

[0075] ZnO 10mol%

[0076] The total proportion of each main formula is 100 mol%.

[0077] Relative to the total amount of the main formula, the components and weight percentages in the dopant formula are:

[0078] CaCO3900PPM

[0079] CoSn(OH)6 140PPM

[0080] Bi2O3 100PPM

[0081] Nano-SiO2 100PPM

[0082] Composite dopant 120PPM

[0083] YBCO 45PPM.

[0084] The preparation method of the composite dopant is as follows: take a CCTO film, heat it up and keep it at 350°C, sprinkle TiO2 powder on it, and then coat a layer of CCTO film, and do this multiple times so that the TiO2 powder is between two adjacent CCTO films. The weight ratio of CCTO to TiO2 is 5:1.

[0085] The method for preparing the high-frequency, wide-temperature, ultra-low-loss ferrite core comprises the following steps:

[0086] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO powder and CoSn(OH)6 according to the ratio requirements, and mix them uniformly;

[0087] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;

[0088] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain a pre-sintered powder; the pre-sintering temperature is 800°C to 900°C;

[0089] Step S4: secondary batching: adding CaCO3, Bi2O3, nano-SiO2, composite dopant, and YBCO to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture; the polysiloxane is PSX700;

[0090] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;

[0091] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;

[0092] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;

[0093] Step S7: pressing and molding: pressing the granulated small particles into annular green billets on a pressing device;

[0094] Step S8: Secondary sintering: Sintering the annular green billet in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

[0095] Comparative Example 1: A high-frequency, wide-temperature, ultra-low-loss ferrite core, wherein the components and proportions of the main formula are:

[0096] Fe2O3 72mol%

[0097] MnO 22mol%

[0098] ZnO 6mol%

[0099] The total proportion of each main formula is 100 mol%.

[0100] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:

[0101] CaCO3 600PPM

[0102] SnO4 110PPM

[0103] Bi2O3 70PPM

[0104] Nano-SiO2 70PPM

[0105] Composite dopant 100PPM

[0106] YBCO 30PPM.

[0107] The preparation method of the composite dopant is as follows: take a CCTO film, heat it up and keep it at 350°C, sprinkle TiO2 powder on it, and then coat a layer of CCTO film, and do this multiple times so that the TiO2 powder is between two adjacent CCTO films. The weight ratio of CCTO to TiO2 is 5:1.

[0108] The method for preparing the high-frequency, wide-temperature, ultra-low-loss ferrite core comprises the following steps:

[0109] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO powder and CoSn(OH)6 according to the ratio requirements, and mix them uniformly;

[0110] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;

[0111] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain a pre-sintered powder; the pre-sintering temperature is 800°C to 900°C;

[0112] Step S4: secondary batching: adding CaCO3, Bi2O3, nano-SiO2, composite dopant, and YBCO to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture; the polysiloxane is PSX700;

[0113] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;

[0114] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;

[0115] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;

[0116] Step S7: pressing and molding: pressing the granulated small particles into annular green billets on a pressing device;

[0117] Step S8: Secondary sintering: Sintering the annular green billet in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

[0118] Comparative Example 2: A high-frequency, wide-temperature, ultra-low-loss ferrite core, wherein the components and proportions of the main formula are:

[0119] Fe2O3 72mol%

[0120] MnO 22mol%

[0121] ZnO 6mol%

[0122] The total proportion of each main formula is 100 mol%.

[0123] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:

[0124] CaCO3 600PPM

[0125] CoSn(OH)6 110PPM

[0126] Bi2O3 70PPM

[0127] Nano-SiO2 70PPM

[0128] CCTO 100PPM

[0129] YBCO 30PPM.

[0130] The method for preparing the high-frequency, wide-temperature, ultra-low-loss ferrite core comprises the following steps:

[0131] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO powder and CoSn(OH)6 according to the ratio requirements, and mix them uniformly;

[0132] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;

[0133] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain a pre-sintered powder; the pre-sintering temperature is 800°C to 900°C;

[0134] Step S4: secondary batching: adding CaCO3, Bi2O3, nano-SiO2, composite dopant, and YBCO to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture; the polysiloxane is PSX700;

[0135] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;

[0136] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;

[0137] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;

[0138] Step S7: pressing and molding: pressing the granulated small particles into annular green materials on a pressing device;

[0139] Step S8: Secondary sintering: Sintering the annular green billet in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

[0140] Comparative Example 3: A high-frequency, wide-temperature, ultra-low-loss ferrite core, wherein the components and proportions of the main formula are:

[0141] Fe2O3 72mol%

[0142] MnO 22mol%

[0143] ZnO 6mol%

[0144] The total proportion of each main formula is 100 mol%.

[0145] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:

[0146] CaCO3 600PPM

[0147] CoSn(OH)6 110PPM

[0148] Bi2O3 70PPM

[0149] Nano-SiO2 70PPM.

[0150] The method for preparing the high-frequency, wide-temperature, ultra-low-loss ferrite core comprises the following steps:

[0151] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO powder and CoSn(OH)6 according to the ratio requirements, and mix them uniformly;

[0152] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;

[0153] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain a pre-sintered powder; the pre-sintering temperature is 800°C to 900°C;

[0154] Step S4: secondary batching: adding CaCO3, Bi2O3, nano-SiO2, composite dopant, and YBCO to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture; the polysiloxane is PSX700;

[0155] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;

[0156] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;

[0157] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;

[0158] Step S7: pressing and molding: pressing the granulated small particles into annular green billets on a pressing device;

[0159] Step S8: Secondary sintering: Sintering the annular green billet in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

[0160] The power loss test was conducted on the standard ring samples of the soft ferrite materials prepared in Examples 1-2 and Comparative Examples 1-3, with an outer diameter of 25× an inner diameter of 15× a height of 7.5. The results are shown in Table 1:

[0161] Table 1 Test results

[0162]

Claims

1. A high frequency, wide temperature and ultra-low loss ferrite core. Features: It includes a main formula and an adulterant formula, wherein the components and proportions of the main formula are: Faith 2 THE 3 70~72mol% MnO 20~22mol% ZnO 6~10mol% The total ratio of each main formula is 100 mol%; The components and weight percentages of the adulterated formulations relative to the weight of the main formulation are: CaCO 3 1~1000PPM CoSn(OH) 6 100~150PPM Bi 2 O 3 50~100PPM Nano-SiO 2 50~100PPM Composite dopant 80~130PPM The preparation method of composite dopant is as follows: CCTO film is coated with TiO 2 After crushing, CCTO and TiO 2 The weight ratio is 5:

1.

2. According to the high frequency, wide temperature and ultra-low loss ferrite core of claim 1, Features: The preparation method of the composite dopant is as follows: take a CCTO film, heat it up and keep it at 350°C, sprinkle TiO 2 After the powder is applied, a CCTO film is coated, and this process is repeated many times to make TiO 2 The powder is located between two adjacent CCTO films.

3. The high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 1, Features: By weight percentage, the dopant formula also includes 30-45 PPM of YBCO.

4. The high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 1, Features: The components and proportions of the main formula are: Faith 2 THE 3 72mol% MnO 22mol% ZnO 6mol% The total proportion of each main formula is 100 mol%.

5. The high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 1, Features: The components and weight percentages of the dopant formula relative to the total amount of the main formula are: CaCO 3 600PPM CoSn(OH) 6 110PPM <h2 style=";text-align:left;direction:ltr">Bi<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 70PPM Nano-SiO 2 70PPM Composite dopant 100PPM.

6. A method for preparing a high-frequency, wide-temperature, ultra-low-loss ferrite core according to any one of claims 1 to 5, Features: The following steps are included: Step S1: Primary batching: Weigh the materials required to prepare the main formula raw material Fe according to the ratio requirements 2 O 3 , MnO, ZnO powder and CoSn(OH) 6 , initially mix evenly; Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder; Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain pre-sintered powder; Step S4: Secondary batching: Adding CaCO to the pre-sintered powder 3 、Bi 2 O 3 、Nano-SiO 2 , the composite dopant, and YBCO are stirred and mixed to form a mixture, and polysiloxane is added to the mixture and stirred and mixed to form a mixture; Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling; Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve; Step S7: pressing and molding: pressing the granulated small particles into annular green materials on a pressing device; Step S8: Secondary sintering: Sinter the annular green material in an air atmosphere to obtain the target high-frequency, wide-temperature, ultra-low-loss ferrite core.

7. The method for preparing a high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 6, Features: The pre-burning temperature in step S3 is 800°C to 900°C.

8. The method for preparing a high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 6, Features: The polysiloxane in step S4 is PSX700.

9. The method for preparing a high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 6, Features: The method further includes step S5' between step S5 and step S6: rapid high-temperature impurity removal: placing the mixture after the second ball milling in an oven and heating it for 20-30 minutes.

10. The method for preparing a high-frequency, wide-temperature, ultra-low-loss ferrite core according to claim 9, Features: The mixture is placed in an oven and heated to 400°C-500°C.