A method for preparing spinning-grade poly(p-phenylene terephthalamide) polymer and fiber thereof
By using prepolymerization and stabilizers to form a prepolymerization system in the preparation of para-aramid fibers, the problems of discoloration and mechanical properties of the fibers under sunlight are solved, and the light stability and mechanical properties of the fibers are significantly improved.
Patent Information
- Application Number
- CN202410573047.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-10
AI Technical Summary
The existing para-aramid fibers are prone to discoloration under sunlight and their mechanical properties are reduced. The molecular weight decreases when dissolving in sulfuric acid to prepare spinning coatings, resulting in a decrease in the retention rate of the fiber's heat resistance strength. It is difficult for existing anti-ultraviolet agents and capping agents to be Completely solve these problems.
Prepolymerization is used to add a stabilizer to form a prepolymerization system, and then polymerize. The stabilizer forms a metastable structure with the terminal amine group, maintains the activity of the amine group and forms a physical barrier in the polymer, and improves the photostability and mechanical properties of the fiber. .
The fiber's photostability and mechanical properties are significantly improved, the polymer aggregation is reduced, and the fiber's stability and resistance to UV aging intensity retention rate is improved.
Smart Images

Figure BDA0004831479390000031 
Figure BDA0004831479390000121 
Figure BDA0004831479390000122
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aromatic polyamide polymers, in particular to a method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer and its fiber. Background Art
[0002] Para-aramid has excellent comprehensive properties, including excellent mechanical properties, heat resistance, electrical insulation, and excellent high temperature acid and alkali resistance. However, para-aramid also has the common problem of all aromatic polyamides, namely poor light stability. Under the irradiation of sunlight, the color of para-aramid fiber will change significantly, and the mechanical properties will also decrease to a certain extent. Studies have found that the main reason for the discoloration of aromatic polyamide polymers, fibers and products is the oxidation of the amine end groups at the ends. In addition, when the aromatic polyamide polymer is dissolved in sulfuric acid to prepare the spinning dope, there is a problem of reduced molecular weight of the polymer, significantly reduced intrinsic viscosity, and reduced heat resistance strength retention of the spun fiber. Studies have found that the main reason is that the carboxyl end groups at the ends are decomposed under acidic conditions. Therefore, both the terminal amine group and the terminal carboxyl group will affect the performance of aramid fiber.
[0003] In response to these problems, researchers have proposed different solutions in recent years, such as treating the surface of para-aramid with an anti-ultraviolet agent (patents CN106592216A, CN112877858A, CN103225210A, CN108642862B, CN105085902A, JPS53126312A, US3888821), or controlling the type of aromatic polyamide end groups (patents JP2007154355A, KR101287323B1, KR101345071B1), or adding a UV-resistant coating to the surface of the polyamide. After the polymerization, a capping agent is added for end-capping treatment (patents CN109575279A, CN113881037A, JP2007154355A, KR101140468B1). However, for para-aramid, there is currently no very effective anti-ultraviolet agent that can completely solve this problem; the end-capping agent is used to cap the aromatic polyamide, which is generally applied to meta-aramid or heterocyclic aramid polymers. Such polymers themselves are still dissolved in the solvent after the polymerization is completed, presenting a stock solution state, and the capping agent can be fully dispersed to achieve good end-capping. The para-aramid industry uses a dry-jet wet spinning process for spinning. First, para-aramid polymer (poly(p-phenylene terephthalamide)) is prepared. This polymer precipitates in the solvent in the late stage of polymerization to form a solid. It is difficult to fully disperse in the solid phase after adding the capping agent. Summary of the invention
[0004] In view of the problems in the prior art, the purpose of the present invention is to provide a method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer and its fiber. The poly(p-phenylene terephthalamide) polymer is obtained by a two-step method of prepolymerization, adding a stabilizer to form a prepolymerization system, and then polymerizing. The prepared aromatic polymer and its fiber overcome the defects of existing aromatic polyamide products such as discoloration when exposed to light and decreased mechanical properties.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] The first aspect of the present invention provides a method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer, and the specific technical scheme is as follows:
[0007] A method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0008] Step 1, dissolving p-phenylenediamine in a solvent system to form a premix; adding part of terephthaloyl chloride to perform prepolymerization to form a prepolymer, and then adding a stabilizer to the prepolymer to continue prepolymerization to obtain a prepolymer system; the stabilizer can form a metastable structure with the terminal amine group of the prepolymer, which can not only maintain the activity of the terminal amine group so that it can continue to polymerize later, but also stabilize the terminal amine group of the final polymer;
[0009] Step 2, adding the remaining terephthaloyl chloride into the prepolymerization system to carry out polymerization to obtain a polymerization product;
[0010] Step 3: neutralize, wash and dry the obtained polymer product to obtain spinning-grade poly(p-phenylene terephthalamide) polymer.
[0011] In some embodiments of the present invention, the stabilizer is a halogen-containing alkane and / or an organic halogenated silane; the general formula of the halogen-containing alkane is: CnH2nR1R2, wherein 3≤n≤9, and R1 and R2 are independently selected from any one of -Br, -Cl, and -F; the general formula of the organic halogenated silane is: X-Si(R)3, wherein X is Br or Cl, and R is selected from any one of C1~C18 alkyl, cycloalkyl, alkoxy, and aryl.
[0012] In some embodiments of the present invention, the stabilizer is selected from any one or more of 1,4-dichlorobutane, trimethylchlorosilane, and trimethoxychlorosilane.
[0013] In some embodiments of the present invention, the solvent system in step 1 is a N-methylpyrrolidone-calcium chloride mixed solvent, wherein the mass proportion of calcium chloride in the mixed solvent is 5wt% to 10wt%.
[0014] In some embodiments of the present invention, the mass fraction of p-phenylenediamine in the premix in step 1 is 1% to 10%.
[0015] In some embodiments of the present invention, the molar amount of the partial terephthaloyl chloride in step 1 is 60% to 85% of the total molar amount of terephthaloyl chloride.
[0016] In some embodiments of the present invention, the stabilizer in step 1 is added at 0.01% to 0.05% of the mass of the spinning-grade poly(p-phenylene terephthalamide) polymer.
[0017] In some embodiments of the present invention, the polymerization in step 2 is continuous polymerization.
[0018] The second aspect of the present invention provides a method for preparing poly(p-phenylene terephthalamide) polymer fiber, using the poly(p-phenylene terephthalamide) polymer prepared by the above preparation method as raw material, and 96wt% to 100wt% concentrated sulfuric acid as solvent to prepare a spinning solution, and adopting a dry-jet wet spinning process to prepare the poly(p-phenylene terephthalamide) polymer fiber.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention adds a stabilizer to the prepolymer, and the stabilizer forms a metastable structure with the terminal amine group of the prepolymer, which can not only maintain the activity of the terminal amine group so that it can continue to polymerize later, but also stabilize the terminal amine group of the final polymer, thereby improving the light stability and chemical stability of the final fiber. At the same time, the addition of the stabilizer can not only interact with the PPTA molecules in a supramolecular chemical manner, but also be inserted into the PPTA prepolymer molecules to form a physical barrier, thereby reducing the aggregation of the prepolymer and improving the stability of the prepolymer.
[0021] 2. The present invention prepares a polymer with fully end group protection by adding a stabilizer to the prepolymer. The fiber end group structure obtained by using this polymer through slurry preparation and dry-jet wet spinning is more stable, and the optical stability and mechanical stability of the fiber are significantly improved. DETAILED DESCRIPTION
[0022] The preparation method of the spinning-grade poly(p-phenylene terephthalamide) polymer and its fiber of the present invention is described in detail below.
[0023] The first aspect of the present invention provides a method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer, and the specific technical scheme is as follows:
[0024] A method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0025] Step 1, dissolving p-phenylenediamine in a solvent system to form a premix; adding part of terephthaloyl chloride to perform prepolymerization to form a prepolymer, and then adding a stabilizer to the prepolymer to continue prepolymerization to obtain a prepolymer system; the stabilizer can form a metastable structure with the terminal amine group of the prepolymer, which can not only maintain the activity of the terminal amine group so that it can continue to polymerize later, but also stabilize the terminal amine group of the final polymer;
[0026] Step 2, adding the remaining terephthaloyl chloride into the prepolymerization system to carry out polymerization to obtain a polymerization product;
[0027] Step 3: neutralize, wash and dry the obtained polymer product to obtain spinning-grade poly(p-phenylene terephthalamide) polymer.
[0028] Poly(p-phenylene terephthalamide) is also known as aramid 1414. Because its molecular structure has an amide group in the para position (1,4) of the benzene ring, it is a fully para-polyaramid formed by the condensation polymerization of p-phenylenediamine and terephthaloyl chloride. The molecular formula is (C 14 H 10 O2N2) n , the chemical structure is as follows:
[0029]
[0030] The stabilizer described in the present invention can form a metastable structure with the terminal amine group of the prepolymer, which can not only maintain the activity of the terminal amine group so that it can continue to polymerize later, but also stabilize the terminal amine group of the final polymer, thereby improving the light stability and chemical stability of the final fiber. At the same time, the addition of the stabilizer can not only interact with the PPTA molecules in a supramolecular chemical manner, but also be inserted into the PPTA prepolymer molecules to form a physical barrier, thereby reducing the aggregation of the prepolymer and improving the stability of the prepolymer.
[0031] In some embodiments of the present invention, the stabilizer is a halogen-containing alkane and / or an organic halogenated silane; the halogen-containing alkane has a general formula of: CnH2nR1R2, wherein 3≤n≤9, R1 and R2 are independently selected from any one of -Br, -Cl, and -F, and can be 1,2-dibromopropane, 1,3-dibromopropane, 1,2-dibromobutane, 1,3-dibromobutane, 1,4-dibromobutane, 1,2-dichloro Propane, 1,3-dichloropropane, 1,2-dichlorobutane, 1,3-dichlorobutane, 1,4-dichlorobutane, etc.; the general formula of the organic halogenated silane is: X-Si(R)3, wherein X is Br or Cl, and R is selected from any one of C1-C18 alkyl, cycloalkyl, alkoxy, and aryl groups, and can be trimethylbromosilane, trimethylchlorosilane, triethylchlorosilane, trimethoxychlorosilane, triethoxychlorosilane, triphenylchlorosilane, etc. The working principle of the stabilizer: halogen can produce hydrogen bonds with the amide of PPTA, and also has a strong coordination complexation effect, and can also produce hydrogen bonds with amine groups, thereby achieving stabilization of the amine groups. However, this supramolecular chemical interaction will not affect the subsequent reaction of the amine groups, so the stability and chemical reaction of the amine groups can be taken into account.
[0032] In some embodiments of the present invention, the stabilizer is selected from any one or more of 1,4-dichlorobutane, trimethylchlorosilane, and trimethoxychlorosilane.
[0033] In the present invention, the term "alkyl" generally refers to a saturated aliphatic group, which may be a straight chain or a branched chain. For example, C1-C18 alkyl generally refers to an alkyl group including 1, 2, 3, 4 ... 18 carbon atoms, and the alkyl group may specifically be methyl, ethyl, propyl, n-propyl, isopropyl, butyl, n-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, etc.
[0034] In the present invention, the term "alkoxy" generally refers to an alkyl-O-group, wherein alkyl is as defined above. For example, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy and heptoxy, etc. The bond to the parent moiety is through the ether oxygen.
[0035] In the present invention, the term "epoxy" generally refers to a CC cycloalkyl group, and includes fused, spiro and bridged bicyclic groups, for example, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, bicyclo[3.1.0]hexyl, bicyclo[2.1.1]hexyl and the like.
[0036] In the present invention, the term "phenyl" generally refers to an unsubstituted phenyl group.
[0037] The solvent in the solvent system in step 1 of the present invention is selected from dimethylacetamide, N-methylpyrrolidone, tetramethylurea, etc., and the solvent system generally also includes a cosolvent, which is selected from calcium chloride, lithium chloride, etc. In some embodiments of the present invention, the solvent system in step 1 is an N-methylpyrrolidone-calcium chloride mixed solvent, N-methylpyrrolidone is the solvent, and calcium chloride acts as a cosolvent in the mixed solvent, wherein the mass proportion of calcium chloride in the mixed solvent is 5% to 10%, which can be 5% to 6%, 6% to 7%, 7% to 8%, 8% to 9%, or 9% to 10%.
[0038] In some embodiments of the present invention, the temperature of the prepolymerization in step one is -10 to 15°C, which can be -10 to -8°C, -8 to -6°C, -6 to -4°C, -4 to -2°C, -2 to 0°C, 0 to 2°C, 2 to 5°C, 5 to 10°C, or 10 to 15°C, preferably -10 to 0°C.
[0039] In some embodiments of the present invention, in step one, the mass fraction of p-phenylenediamine in the premix is 1% to 10%, which can be 1% to 2%, 2% to 3%, 3% to 4%, 4% to 5%, 5% to 6%, 6% to 7%, 7% to 8%, 8% to 9%, or 9% to 10%.
[0040] In some embodiments of the present invention, the stabilizer in step one is added at 0.01% to 0.05% of the mass of the spinning-grade poly(p-phenylene terephthalamide) polymer, which can be 0.01% to 0.02%, 0.02% to 0.03%, 0.03% to 0.04%, or 0.04% to 0.05%.
[0041] In some embodiments of the present invention, the molar amount of the part of terephthaloyl chloride in step 1 is 60% to 85% of the total molar amount of terephthaloyl chloride, and can be 60% to 65%, 65% to 70%, 70% to 75%, 75% to 80%, or 80% to 85%, preferably 70%.
[0042] In some embodiments of the present invention, the polymerization temperature in step 2 is 0-60°C, which can be 0-5°C, 5-10°C, 10-15°C, 15-20°C, 20-25°C, 25-30°C, 30-35°C, 35-40°C, 40-45°C, 45-50°C, 50-55°C, or 55-60°C, preferably 10-30°C.
[0043] In some embodiments of the present invention, the drying in step three is specifically drying at 100-180°C until the moisture content is less than 1wt%, which can be 100-110°C, 110-120°C, 120-130°C, 130-140°C, 140-150°C, 150-160°C, 160-170°C, or 170-180°C.
[0044] The polymerization production process in the present invention is not particularly limited, and can be intermittent polymerization or continuous polymerization.
[0045] The second aspect of the present invention provides a method for preparing poly(p-phenylene terephthalamide) polymer fiber, using the poly(p-phenylene terephthalamide) polymer prepared by the above preparation method as a raw material, using 96wt% to 100wt% concentrated sulfuric acid as a solvent, preparing a spinning solution, and adopting a dry-jet wet spinning process to prepare the poly(p-phenylene terephthalamide) polymer fiber. In some embodiments of the present invention, the solid content of the poly(p-phenylene terephthalamide) polymer in the spinning solution is 5wt% to 15wt%, which can be 5wt% to 6wt%, 6wt% to 7wt%, 7wt% to 8wt%, 8wt% to 9wt%, 9wt% to 10wt%, 10wt% to 11wt%, 11wt% to 12wt%, 12wt% to 13wt%, 13wt% to 14wt%, or 14wt% to 15wt%.
[0046] In the present invention, the dry-jet wet spinning process is not particularly limited, and a process commonly used in the art can be used. In some embodiments of the present invention, the dry-jet wet spinning process specifically includes: passing the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation, and the coagulated fibers are washed, neutralized, dried, and oiled before being wound into products.
[0047] The specific embodiments of the present invention are further described in detail below in conjunction with preferred embodiments. When the embodiments provide numerical ranges, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, as those skilled in the art grasp the prior art and record the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0048] Example 1
[0049] In this embodiment, 1,4-dichlorobutane is selected as the stabilizer. In this polymerization reaction, terephthaloyl chloride (TPC) and p-phenylenediamine (PPDA) react at a molar ratio of 0.99:1, and the polymerization method adopts intermittent polymerization.
[0050] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0051] S1. Dissolve calcium chloride in NMP solvent in a reactor to form 10 kg of NMP-CaCl2 mixed solvent, wherein calcium chloride accounts for 9 wt% of the mixed solvent; dissolve 0.526 kg of PPDA in the mixed solvent to form a PPDA-NMP-CaCl2 premix, wherein PPDA accounts for 5 wt%.
[0052] S2. The solvent temperature was controlled below 0°C, 0.684 kg of TPC was added and the reaction was continued for 2 minutes, the reaction temperature was controlled below 5°C, and then 0.00058 kg of 1,4-dichlorobutane was added into the reactor and the reaction was continued for 2 minutes.
[0053] S3. Add 0.293 kg of TPC and continue stirring for 10 minutes, controlling the polymerization temperature to be no higher than 30° C. until the reaction is terminated.
[0054] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0055] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0056] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0057] (2) The dry-jet wet spinning process is adopted to pass the spinning solution through the spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried and oiled, and then wound into products to obtain poly(p-phenylene terephthalamide) fibers.
[0058] Example 2
[0059] The amount of stabilizer 1,4-dichlorobutane was adjusted to 0.00043 kg, and the rest was the same as in Example 1 to obtain poly(p-phenylene terephthalamide) polymer and poly(p-phenylene terephthalamide) fiber.
[0060] Example 3
[0061] In this embodiment, 1,4-dichlorobutane is used as the stabilizer. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine react at a molar ratio of 0.99:1, and the polymerization method adopts continuous polymerization.
[0062] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0063] S1. Prepare a solvent with NMP and calcium chloride in a certain ratio, and distill out water to continuously obtain a NMP-CaCl2 mixed solvent with a calcium chloride concentration of 9 wt%.
[0064] S2. Use a chemical pump and a flow meter to pump the NMP-CaCl2 mixed solvent at a rate of 10 tons / hour and the molten PPDA at a rate of 0.526 tons / hour into a continuous mixing kettle for thorough mixing to continuously obtain a PPDA-NMP-CaCl2 premix.
[0065] S3. Use a chemical pump and a flow meter to pump the PPDA-NMP-CaCl2 premix at a rate of 10.526 tons / hour and the molten TPC at a rate of 0.684 tons / hour into a continuous prepolymerization reactor, and simultaneously use a precision feeder to add 1,4-dichlorobutane to the outlet of the prepolymerization reactor at a rate of 0.58 kg / hour. The prepolymer with the stabilizer added and the molten TPC at 0.293 tons / hour enter the twin-screw reactor together, control the reaction temperature below 30°C, and finally obtain a polymer at the outlet of the twin-screw reactor.
[0066] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0067] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0068] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0069] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain poly(p-phenylene terephthalamide) fibers.
[0070] Comparative Example 1
[0071] In this comparative example, no stabilizer is added. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine are reacted at a molar ratio of 0.99:1, and the polymerization method adopts intermittent polymerization.
[0072] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0073] S1. Dissolve calcium chloride in NMP solvent in a reactor to form 10 kg of NMP-CaCl2 mixed solvent, wherein calcium chloride accounts for 9 wt% of the mixed solvent; dissolve 0.526 kg of PPDA in the mixed solvent to form a PPDA-NMP-CaCl2 premix, wherein PPDA accounts for 5 wt%.
[0074] S2. The solvent temperature is controlled below 0°C, 0.684 kg of TPC is added and reacted for 2 minutes, and the reaction temperature is controlled below 5°C.
[0075] S3. Add 0.293 kg of TPC and continue stirring for 10 minutes, controlling the polymerization temperature to be no higher than 30° C. until the reaction is terminated.
[0076] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0077] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0078] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0079] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain conventional poly(p-phenylene terephthalamide) fibers.
[0080] Comparative Example 2
[0081] In this embodiment, no stabilizer is added. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine react at a molar ratio of 0.99:1, and the polymerization method adopts continuous polymerization.
[0082] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0083] S1. Prepare a solvent with NMP and calcium chloride in a certain ratio, and distill out water to continuously obtain a NMP-CaCl2 mixed solvent with a calcium chloride concentration of 9 wt%.
[0084] S2. Use a chemical pump and a flow meter to pump the NMP-CaCl2 mixed solvent at a rate of 10 tons / hour and the molten PPDA at a rate of 0.526 tons / hour into a continuous mixing kettle for thorough mixing to continuously obtain a PPDA-NMP-CaCl2 premix.
[0085] S3. Use a chemical pump and a flow meter to pump the PPDA-NMP-CaCl2 premix at a rate of 10.526 tons / hour and the molten TPC at a rate of 0.684 tons / hour into a continuous prepolymerization reactor. After the prepolymer is generated, the prepolymer and 0.293 tons / hour of molten TPC enter a twin-screw reactor together, control the reaction temperature below 30°C, and finally obtain a polymer at the outlet of the twin-screw reactor.
[0086] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0087] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0088] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0089] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain conventional poly(p-phenylene terephthalamide) fibers.
[0090] Example 4
[0091] In this embodiment, trimethylsilyl chloride is used as a stabilizer. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine react at a molar ratio of 0.995:1, and the polymerization method adopts intermittent polymerization.
[0092] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0093] S1. Dissolve calcium chloride in NMP solvent in a reactor to form 10 kg of NMP-CaCl2 mixed solvent, wherein calcium chloride accounts for 9 wt% of the mixed solvent; dissolve 0.526 kg of PPDA in the mixed solvent to form a PPDA-NMP-CaCl2 premix, wherein PPDA accounts for 5 wt%.
[0094] S2. The solvent temperature was controlled below 0°C, 0.657 kg of TPC was added and the reaction was continued for 2 minutes, the reaction temperature was controlled below 5°C, and then 0.00056 kg of trimethylsilyl chloride was added into the reactor and the reaction was continued for 2 minutes.
[0095] S3. Add 0.327 kg of TPC and continue stirring for 10 minutes, controlling the polymerization temperature to be no higher than 30° C. until the reaction is terminated.
[0096] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0097] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0098] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0099] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain poly(p-phenylene terephthalamide) fibers.
[0100] Example 5
[0101] The stabilizer was replaced by trimethoxysilyl chloride, and the rest was the same as in Example 4 to prepare poly(p-phenylene terephthalamide) polymer and poly(p-phenylene terephthalamide) fiber.
[0102] Example 6
[0103] The amount of the stabilizer trimethylchlorosilane was adjusted to 0.00042 kg, and the rest was the same as in Example 4 to obtain poly(p-phenylene terephthalamide) polymer and poly(p-phenylene terephthalamide) fiber.
[0104] Example 7
[0105] In this embodiment, trimethylsilyl chloride is used as a stabilizer. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine react at a molar ratio of 0.995:1, and the polymerization method adopts continuous polymerization.
[0106] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0107] S1. Prepare a solvent with NMP and calcium chloride in a certain ratio, and distill out water to continuously obtain a NMP-CaCl2 mixed solvent with a calcium chloride concentration of 9 wt%.
[0108] S2. Use a chemical pump and a flow meter to pump the NMP-CaCl2 mixed solvent at a rate of 10 tons / hour and the molten PPDA at a rate of 0.526 tons / hour into a continuous mixing kettle for thorough mixing to continuously obtain a PPDA-NMP-CaCl2 premix.
[0109] S3. Use a chemical pump and a flow meter to pump the PPDA-NMP-CaCl2 premix at a rate of 10.526 tons / hour and the molten TPC at a rate of 0.657 tons / hour into a continuous prepolymerization reactor, and simultaneously use a precision feeder to add trimethylchlorosilane to the outlet of the prepolymerization reactor at a rate of 0.56 kg / hour. The prepolymer with the stabilizer added and the molten TPC of 0.327 tons / hour enter the twin-screw reactor together, control the reaction temperature below 30°C, and finally obtain a polymer at the outlet of the twin-screw reactor.
[0110] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0111] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0112] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0113] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain poly(p-phenylene terephthalamide) fibers.
[0114] Comparative Example 3
[0115] In this comparative example, no stabilizer is added. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine are reacted at a molar ratio of 0.995:1, and the polymerization method adopts intermittent polymerization.
[0116] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0117] S1. Dissolve calcium chloride in NMP solvent in a reactor to form 10 kg of NMP-CaCl2 mixed solvent, wherein calcium chloride accounts for 9 wt% of the mixed solvent; dissolve 0.526 kg of PPDA in the mixed solvent to form a PPDA-NMP-CaCl2 premix, wherein PPDA accounts for 5 wt%.
[0118] S2. The solvent temperature is controlled below 0°C, 0.657 kg of TPC is added and reacted for 2 minutes, and the reaction temperature is controlled below 5°C.
[0119] S3. Add 0.327 kg of TPC and continue stirring for 10 minutes, controlling the polymerization temperature to be no higher than 30° C. until the reaction is terminated.
[0120] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0121] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0122] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0123] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain conventional poly(p-phenylene terephthalamide) fibers.
[0124] Comparative Example 4
[0125] In this embodiment, no stabilizer is added. In this polymerization reaction, terephthaloyl chloride and p-phenylenediamine react at a molar ratio of 0.995:1, and the polymerization method adopts continuous polymerization.
[0126] The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer comprises the following steps:
[0127] S1. Prepare a solvent with NMP and calcium chloride in a certain ratio, and distill out water to continuously obtain a NMP-CaCl2 mixed solvent with a calcium chloride concentration of 9 wt%.
[0128] S2. Use a chemical pump and a flow meter to pump the NMP-CaCl2 mixed solvent at a rate of 10 tons / hour and the molten PPDA at a rate of 0.526 tons / hour into a continuous mixing kettle for thorough mixing to continuously obtain a PPDA-NMP-CaCl2 premix.
[0129] S3. Use a chemical pump and a flow meter to pump the PPDA-NMP-CaCl2 premix at a rate of 10.526 tons / hour and the molten TPC at a rate of 0.657 tons / hour into a continuous prepolymerization reactor. After the prepolymer is generated, the prepolymer and 0.327 tons / hour of molten TPC enter a twin-screw reactor together, control the reaction temperature below 30°C, and finally obtain a polymer at the outlet of the twin-screw reactor.
[0130] S4, neutralizing the obtained polymer to neutrality, washing it clean, and drying it at 100° C. until the moisture content is less than 1%, thereby obtaining a pure and dry poly(p-phenylene terephthalamide) polymer.
[0131] The preparation method of p-phenylene terephthalamide polymer fiber comprises the following steps:
[0132] (1) using the poly(p-phenylene terephthalamide) polymer as a raw material and 100 wt % concentrated sulfuric acid as a solvent to prepare a spinning solution (polymer solid content 10 wt %);
[0133] (2) The same dry-jet wet spinning process as in Example 1 is used to pass the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation. The coagulated fibers are washed, neutralized, dried, and oiled, and then wound into a product to obtain conventional poly(p-phenylene terephthalamide) fibers.
[0134] Performance Testing
[0135] 1. Color changes of polymers and fibers
[0136] The color is characterized by the L value measured by KURABO's COLOR-7X. The initial color is the test value before light aging, represented by L0; the color after the QUV ultraviolet light accelerated aging test is represented by L1, and the color change ΔL = L1-L0. The ultraviolet light accelerated aging test uses ultraviolet light with an irradiance of 0.89W / m at 340nm to expose the blackboard temperature at 60℃ for 8h, followed by a cycle of condensation at a blackboard temperature of 50℃ for 4h for 1 week to test the color changes of polymers and aramid fibers before and after light aging.
[0137] 2. Changes in polymer viscosity and fiber light aging strength retention
[0138] QUV accelerated aging test uses ultraviolet light with an irradiance of 0.89W / m at 340nm to expose the material for 8h at a blackboard temperature of 60℃, and then cycles for 1 week at a blackboard temperature of 50℃ for 4h to test the viscosity change of the polymer before and after light aging.
[0139] Polymer viscosity test: Using concentrated sulfuric acid as solvent, the logarithmic viscosity of the polymer is tested with an Ubbelohde capillary viscometer. The test value before light aging is represented by η0; the color after QUV ultraviolet accelerated aging test is represented by η1, and the viscosity change rate Δη=η1-η0. The ultraviolet accelerated aging test uses ultraviolet light with an irradiance of 0.89W / m at 340nm to expose the blackboard temperature at 60℃ for 8h, and then condenses for 4h at a blackboard temperature of 50℃ for 1 week to test the change in polymer viscosity before and after light aging.
[0140] Fiber strength (SF n ) characterizes the mechanical properties of the fiber, namely the breaking strength per unit linear density (LD), which is defined by the following formula (1). In addition, the light aging strength retention rate of the fiber is expressed by the following formula (2), where SF0 is the strength of the fiber before heat treatment; SF n It is the intensity after being exposed to ultraviolet light with an irradiance of 0.89 W / m at 340 nm at a blackboard temperature of 60°C for 8 hours, followed by condensation at a blackboard temperature of 50°C for 4 hours for one week.
[0141] Fiber breaking strength SF n (cN / dtex) = F n (N)×100 / LD(dtex) (1)
[0142] Light aging strength retention rate SF (%) = (SF n -SF0)×100 / SF0 (2)
[0143] Table 1 below shows the test results of the color, viscosity and viscosity change rate of the polymers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 before and after light aging treatment.
[0144] Table 1 Polymer color and viscosity changes
[0145]
[0146] Table 2 below shows the test results of fiber color change, fiber strength before and after light aging treatment, and strength retention rate of the aramid fibers prepared in Examples 1 to 3 and Comparative Examples 1 to 2.
[0147] Table 2 Changes in fiber color and fiber strength
[0148]
[0149] As can be seen from Table 1 and Table 2, in Examples 1 to 3, when an appropriate amount of stabilizer is added to the prepolymer, the color change of the polymer and the aramid fiber is significantly reduced, and the light stability is significantly improved. The viscosity of the polymer is less affected, and at the same time, the light aging strength retention rate is about 90%, so the strength after light aging treatment is well maintained. In contrast, the strength retention rate of conventional fibers (Comparative Example 1, Comparative Example 2) manufactured by conventional methods after light aging is about 85%.
[0150] Table 3 below shows the test results of the color, viscosity and viscosity change rate of the polymers prepared in Examples 4 to 7 and Comparative Examples 3 to 4 before and after light aging treatment.
[0151] Table 3 Changes in polymer color and viscosity
[0152]
[0153] Table 4 below shows the test results of fiber color change, fiber strength before and after light aging treatment, and strength retention rate of the aramid fibers prepared in Examples 4 to 7 and Comparative Examples 3 to 4.
[0154] Table 4 Changes in fiber color and fiber strength
[0155]
[0156] As can be seen from Table 3 and Table 4, in Examples 4 to 7, when an appropriate amount of stabilizer is added to the prepolymer, the color change of the polymer and the aramid fiber is significantly reduced, and the light stability is significantly improved. The viscosity of the polymer has a small effect, and at the same time, the light aging strength retention rate is about 90%, so the strength after light aging treatment is well maintained. In contrast, the strength retention rate of conventional fibers (Comparative Examples 3 and 4) manufactured by conventional methods after light aging is about 85%.
[0157] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer, characterized in that: The following steps are involved: Step 1, dissolving p-phenylenediamine in a solvent system to form a premix; adding part of terephthaloyl chloride to perform prepolymerization to form a prepolymer, then adding a stabilizer to the prepolymer, continuing prepolymerization to obtain a prepolymer system; the stabilizer can form a metastable structure with the terminal amine group of the prepolymer, which can not only maintain the activity of the terminal amine group so that it can continue to polymerize later, but also stabilize the terminal amine group of the final polymer; the stabilizer is a halogen-containing alkane and / or an organic halogenated silane; the halogen-containing alkane has a general formula of: C n H 2n R1R2, wherein 3≤n≤9, R1 and R2 are independently selected from any one of -Br, -Cl, and -F; the general formula of the organohalosilane is: X-Si(R)3, wherein X is Br or Cl, and R is selected from any one of C1~C18 alkyl, cycloalkyl, alkoxy, and aryl; Step 2, adding the remaining terephthaloyl chloride into the prepolymerization system to carry out polymerization to obtain a polymerization product; Step 3: neutralize, wash and dry the obtained polymer product to obtain spinning-grade poly(p-phenylene terephthalamide) polymer.
2. The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer according to claim 1, characterized in that: The stabilizer is selected from any one or more of 1,4-dichlorobutane, trimethylchlorosilane and trimethoxychlorosilane.
3. The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer according to claim 1, wherein: Includes one or more of the following characteristics: (1) The molar amount of the partial terephthaloyl chloride in step 1 is 60% to 85% of the total molar amount of terephthaloyl chloride; (2) In step 1, the solvent system is a N-methylpyrrolidone-calcium chloride mixed solvent, wherein the mass proportion of calcium chloride in the mixed solvent is 5% to 10%; (3) In step 1, the prepolymerization temperature is -10~15°C; (4) In step 1, the mass fraction of p-phenylenediamine in the premix is 1% to 10%; (5) In step 1, the stabilizer is added at 0.01% to 0.05% of the mass of the spinning-grade poly(p-phenylene terephthalamide) polymer.
4. The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer according to claim 1, wherein: In step 2, the polymerization temperature is 0-60°C.
5. The method for preparing a spinning-grade poly(p-phenylene terephthalamide) polymer according to claim 1, characterized in that: In step 3, the drying is specifically drying at 100-180° C. until the moisture content is less than 1 wt %.
6. A method for preparing poly(p-phenylene terephthalamide) polymer fiber, characterized in that: The poly(p-phenylene terephthalamide) polymer prepared by the preparation method according to any one of claims 1 to 5 is used as a raw material, 96wt% to 100wt% concentrated sulfuric acid is used as a solvent to prepare a spinning solution, and a dry-jet wet spinning process is adopted to prepare the poly(p-phenylene terephthalamide) polymer fiber.
7. The method for preparing poly(p-phenylene terephthalamide) polymer fiber according to claim 6, characterized in that: The dry-jet wet spinning process specifically includes: passing the spinning solution through a spinneret to form primary filaments, which are then put into a coagulation bath for coagulation and forming; the coagulated fibers are washed, neutralized, dried and oiled, and then wound into products.
8. The method for preparing poly(p-phenylene terephthalamide) polymer fiber according to claim 6, characterized in that: The solid content of the poly(p-phenylene terephthalamide) polymer in the spinning solution is 5wt%-15wt%.