A rubber flame retardant material for underground conveyor belts in coal mines and a preparation method thereof
By using a combination of powder flame retardant filler and surfactant silane coupling agent in underground conveyor belts of coal mines, the problem of difficulty in taking into account both flame retardant and mechanical properties is solved, and excellent flame retardant and mechanical properties are achieved, and the quality of flame retardant and mechanical properties is reduced. production costs.
Patent Information
- Application Number
- CN202410778938.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-17
AI Technical Summary
The flame retardant performance and mechanical properties of existing coal mine underground conveyor belts are difficult to take into account. Neoprene-based flame retardant conveyor belts have problems such as easy crystallization, poor processing performance, high cost and the addition of a large number of powder flame retardants, resulting in the decline in mechanical properties.
The rubber flame retardant material containing powder flame retardant filler and surfactant silane coupling agent is adopted. The surfactant silane coupling agent is made of siloxane, hydroxyl, long carbon chain alkyl, carboxyl, sodium sulfonate groups and Quaternary ammonium groups provide flame retardant and surfactant effects, synergistically improve flame retardant properties and promote catalytic carbon formation, reducing the negative impact of powder flame retardant filler addition on mechanical properties.
The coal mine underground conveyor belt has achieved a balance of flame retardant performance and mechanical properties, reduced production costs, and met the needs of coal mine underground conveyor belts through good dispersion of inorganic components and organic components.
Smart Images

Figure CN118440410B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of flame-retardant conveyor belts for underground coal mines, and more specifically, to a rubber flame-retardant material for underground coal mine conveyor belts and a preparation method thereof. Background Art
[0002] Coal is the main support of my country's energy structure. In order to improve the transportation efficiency of coal, people usually use mechanical equipment for transportation, such as conveyors. The main component of the conveyor is the conveyor belt composed of covering rubber, rubber core layer and skeleton material.
[0003] Although conveyors can effectively improve the efficiency of coal transportation, as the conveyor capacity, transportation distance and load increase, the tensile stress on the conveyor belt increases significantly. At the same time, due to the irregular shape, heavy weight and sharp surface of minerals, the minerals can easily cause serious damage and wear to the conveyor belt. Even if the conveyor belt rubs and produces sparks during transportation, it can easily lead to fire, resulting in significant loss of life and property. In response to this, the state requires coal mine conveyor belts to have flame retardant properties and meet the requirements of MT / T668.
[0004] At present, flame-retardant conveyor belts are basically based on chloroprene rubber, and a large amount of flame retardants or flame retardant fillers are used to improve the flame retardant properties of the conveyor belts. However, chloroprene rubber has the disadvantages of easy crystallization, poor processing performance, unstable performance, difficult storage, and high cost. At the same time, the addition of a large amount of powder flame retardant will lead to a decrease in the mechanical properties of the conveyor belt. Therefore, there is an urgent need for a material with both excellent flame retardant and mechanical properties for use in coal conveyor belts. Summary of the invention
[0005] In order to improve the defect that conventional chloroprene rubber-based flame-retardant conveyor belts are difficult to have both flame-retardant properties and mechanical properties, the present application provides a rubber flame-retardant material for underground conveyor belts in coal mines and a preparation method thereof.
[0006] In the first aspect, the present application provides a rubber flame retardant material for a conveyor belt in a coal mine, which adopts the following technical solution:
[0007] A rubber flame retardant material for a coal mine underground conveyor belt, the rubber flame retardant material for a coal mine underground conveyor belt comprising a powder flame retardant filler and a surface active silane coupling agent;
[0008] The molecular structural formula of the surface active silane coupling agent is:
[0009] .
[0010] The surface active silane coupling agent in the present application contains siloxane groups, hydroxyl groups, long carbon chain alkyl groups, carboxyl groups, sodium sulfonate groups, quaternary ammonium salt groups and flame retardant element silicon at the same time, wherein the siloxane groups and hydroxyl groups can play the role of silane coupling agents, the long carbon chain alkyl groups, carboxyl groups, sodium sulfonate groups and quaternary ammonium salt groups play the role of surfactants, surface dispersion and surface modification, and at the same time, the sodium sulfonate group also plays the role of a catalyst, thereby promoting catalytic carbonization and improving the thermal stability and flame retardant properties of the material; and the presence of elemental silicon provides excellent flame retardant properties.
[0011] In summary, when the rubber flame retardant material for underground conveyor belts in coal mines contains powder flame retardant fillers and surfactant silane coupling agents, the powder flame retardant fillers and surfactant silane coupling agents will have a synergistic flame retardant effect. At the same time, the surfactant silane coupling agent can also help the powder flame retardant filler to be evenly dispersed in the rubber matrix, thereby reducing the problem of decreased mechanical properties of the conveyor belt caused by the addition of powder flame retardant fillers.
[0012] That is, when the rubber flame retardant material for underground conveyor belts in coal mines contains powder flame retardant fillers and surface active silane coupling agents, the rubber flame retardant material for underground conveyor belts in coal mines will have both excellent flame retardant properties and mechanical properties.
[0013] Preferably, the preparation method of the surface active silane coupling agent comprises the following steps:
[0014] S1. First, N-octadecyl-1,3-propylene diamine and 3-glycidyloxypropyltrimethoxysilane are mixed and reacted in isopropanol to obtain a reaction intermediate I. The structural formula of the reaction intermediate I is:
[0015] ;
[0016] S2, adding acrylic acid to the intermediate I, mixing and reacting to obtain a reaction intermediate II, the structural formula of the reaction intermediate II is:
[0017] ;
[0018] S3, adding the aqueous solution of sodium 3-chloro-2-hydroxypropyl sulfonate to the reaction intermediate II, mixing and reacting, and obtaining a surface active silane coupling agent.
[0019] Preferably, the reaction equations of each step of the preparation method of the surface active silane coupling agent are:
[0020] S1:
[0021] ;
[0022] S2:
[0023] ;
[0024] S3:
[0025] .
[0026] Preferably, the molar ratio of N-octadecyl-1,3-propylene diamine, 3-glycidyloxypropyltrimethoxysilane, acrylic acid, and sodium 3-chloro-2-hydroxypropyl sulfonate is 1: (1.0-1.2): (2.0-2.2): (2.0-2.3).
[0027] Preferably, the mass ratio of the N-octadecyl-1,3-propylene diamine to isopropanol is 1:(1.3-3.3).
[0028] Preferably, in the aqueous solution of sodium 3-chloro-2-hydroxypropyl sulfonate, the mass fraction of sodium 3-chloro-2-hydroxypropyl sulfonate is 25wt%-40wt%.
[0029] Preferably, in S1, the reaction temperature is 65-82°C and the reaction time is 3-5h.
[0030] Preferably, in S2, the reaction temperature is 65-82°C and the reaction time is 2-4h.
[0031] Preferably, in S3, the reaction temperature is 65-82° C., and the reaction time is 4-6 h.
[0032] Preferably, the preparation method of the surface active silane coupling agent comprises the following steps:
[0033] S1. First, N-octadecyl-1,3-propylene diamine and isopropanol are added to a reactor, and then 3-glycidyloxypropyltrimethoxysilane is added, heated and stirred, and reacted at a temperature of 65-82° C. for 3-5 hours to obtain a reaction intermediate I. The structural formula of the reaction intermediate I is:
[0034] ;
[0035] S2. Add acrylic acid to reaction I, and mix and react at a temperature of 65-82° C. for 2-4 hours to obtain reaction intermediate II, the structural formula of which is:
[0036] ;
[0037] S3. Add 25wt%-40wt% of 3-chloro-2-hydroxypropyl sodium sulfonate aqueous solution to the reaction intermediate II, mix and react at a temperature of 65-82° C. for 4-6 hours to obtain a surface active silane coupling agent.
[0038] Preferably, the rubber flame retardant material for underground conveyor belts in coal mines comprises the following raw materials in parts by mass: 40-60 parts of natural rubber, 40-60 parts of butadiene rubber, 40-50 parts of reinforcing agent, 4-6 parts of activating agent, 0-3 parts of stearic acid, 4-6 parts of aromatic oil, 1.5-3.5 parts of antioxidant, 0.8-2.8 parts of accelerator, 20-30 parts of chlorinated paraffin, 12-26 parts of powdered flame retardant filler, 0.1-0.8 parts of surface active silane coupling agent and 1-4 parts of vulcanizing agent;
[0039] The powder flame retardant filler is composed of 2-6 parts of antimony trioxide and 10-20 parts of aluminum hydroxide.
[0040] Antimony trioxide and aluminum hydroxide are both inorganic flame retardants with excellent flame retardant effects. Among them, the flame retardant mechanism of antimony trioxide mainly includes three aspects: gas phase flame retardant, solid phase flame retardant and chemical reaction flame retardant. Specifically, antimony trioxide can release antimony pentoxide at high temperature, and antimony pentoxide can react with free radicals in the fuel to inhibit the combustion. At the same time, antimony trioxide can also form a dense isolation layer at high temperature, thereby hindering combustion and heat conduction and slowing down the spread of flames. In addition, antimony trioxide can also react chemically with free radicals and active substances in the flame propagation chain reaction, thereby blocking the chain reaction and achieving a flame retardant effect.
[0041] The flame retardant mechanism of aluminum hydroxide mainly includes three aspects: dehydration, dilution and isolation. Specifically, at high temperature, aluminum hydroxide can decompose water, thereby absorbing heat, reducing the surface temperature of the fuel, and inhibiting the formation and spread of flames. At the same time, the generation of water vapor will also dilute the oxygen concentration, thereby inhibiting the formation and spread of flames. In addition, when burning, aluminum hydroxide can form an isolation layer of aluminum oxide, thereby hindering combustion and heat conduction and slowing down the spread of flames.
[0042] When antimony trioxide and aluminum hydroxide are used together, they will synergistically flame retard in different aspects, and with the cooperation of the surface active silane coupling agent, a better flame retardant effect can be obtained.
[0043] Preferably, the reinforcing agent is carbon black N220.
[0044] Preferably, the active agent is zinc oxide and magnesium oxide, or a mixture of both.
[0045] Preferably, the antioxidant is one or a mixture of antioxidant 4010 (N-cyclohexyl-N'-phenyl-p-phenylenediamine), antioxidant 4020 (N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine) and antioxidant RD (2,2,4-trimethyl-1,2-dihydroquinoline polymer).
[0046] Preferably, the accelerator is one or a mixture of DM (2,2'-dibenzothiazole disulfide) and CZ (N-cyclohexyl-2-benzothiazole sulfenamide).
[0047] Preferably, the vulcanizing agent is sulfur.
[0048] In a second aspect, the present application provides a method for preparing a rubber flame retardant material for a conveyor belt in a coal mine, using the following technical solution:
[0049] A method for preparing a rubber flame retardant material for a conveyor belt in an underground coal mine comprises the following steps:
[0050] Step 1: Mix 4-6 parts of an active agent, 2-6 parts of antimony trioxide, 10-20 parts of aluminum hydroxide and 0.1-0.8 parts of a surface-active silane coupling agent, stir evenly, and dry at a temperature of 40-60° C. to obtain component A;
[0051] Step 2: 40-60 parts of natural rubber and 40-60 parts of butadiene rubber are put into an internal mixer at a rotor speed of 30-35 r / min and a top bolt pressure of 2.5-4.0 bar, and mixed for 20-30 seconds to obtain component B;
[0052] Step 3: Add component A, 20-30 parts of chlorinated paraffin 70, 0-3 parts of stearic acid, 4-6 parts of aromatic oil, 1.5-3.5 parts of antioxidant and 0.8-2.8 parts of accelerator to component B, and continue mixing for 60-90 seconds to obtain component C;
[0053] Step 4: Add 40-50 parts of reinforcing agent to component C, continue mixing for 100-120 seconds, control the debonding temperature ≤130°C, debond; further mix on the open mill (cut off twice and turn over three times), then roll down the sheet, pass through the release agent tank, and enter the wind room to cool to room temperature to obtain component D;
[0054] Step 5: After the D component is parked for 6-8 hours, it is put into an internal mixer, 1-4 parts of vulcanizer are added, the rotor speed is 20-25r / min, the top bolt pressure is 2.5-4.0bar, mixing is performed for 90-120s, and the discharge temperature is controlled to be ≤95°C, and the rubber is discharged; after further mixing in the open mixer, the sheet is calendered, and after passing through the isolation agent tank, it enters the wind room to cool to room temperature to obtain the rubber flame retardant material for underground conveyor belts in coal mines.
[0055] In summary, this application has the following beneficial effects:
[0056] 1. The surface active silane coupling agent in the present application contains siloxane groups, hydroxyl groups, long carbon chain alkyl groups, carboxyl groups, sodium sulfonate groups, quaternary ammonium salt groups and flame retardant element silicon at the same time, wherein the siloxane groups and hydroxyl groups can play the role of silane coupling agents, the long carbon chain alkyl groups, carboxyl groups, sodium sulfonate groups and quaternary ammonium salt groups play the role of surfactants, surface dispersion and surface modification, and at the same time, the sodium sulfonate group also plays the role of a catalyst, thereby promoting catalytic carbonization and improving the thermal stability and flame retardant properties of the material; and the presence of elemental silicon provides excellent flame retardant properties;
[0057] That is, when the rubber flame retardant material for underground conveyor belts in coal mines contains powder flame retardant fillers and surface active silane coupling agents, the rubber flame retardant material for underground conveyor belts in coal mines will have both excellent flame retardant properties and mechanical properties.
[0058] 2. The method of the present application has a simple production process, low cost and is easy to promote and apply.
[0059] 3. The inorganic components and organic components in the rubber flame retardant material for underground conveyor belts in coal mines of the present application have strong mutual dispersibility and coupling, are environmentally friendly, have good dispersibility and mechanical properties, and can meet the needs of underground conveyor belts in coal mines. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is an infrared spectrum analysis chart of the surface active silane coupling agent in Example 1. DETAILED DESCRIPTION
[0061] The following combination Figure 1 , Examples 1-5 and Comparative Examples 1-2 further illustrate the present application in detail.
[0062] raw material
[0063] Octadecyl-1,3-propylenediamine; 3-glycidyloxypropyltrimethoxysilane; isopropanol; acrylic acid; sodium 3-chloro-2-hydroxypropylsulfonate; natural rubber standard No. 1; butadiene rubber BR9000; reinforcing agent carbon black N220; activator zinc oxide CAS: 1314-13-2; stearic acid; aromatic oil; antioxidant RD 2,2,4-trimethyl-1,2-dihydroquinoline polymer; antioxidant 4010 N-cyclohexyl-N'-phenyl-p-phenylenediamine; accelerator CZ N-cyclohexyl-2-benzothiazolesulfonamide; accelerator DM 2,2'-dithiodibenzothiazole; chlorinated paraffin 70; antimony trioxide CAS: 1309-64-4; aluminum hydroxide ATH-8; vulcanizing agent-sulfur CAS: 7704-34-9.
[0064] Example
[0065] Example 1
[0066] A rubber flame retardant material for an underground conveyor belt in a coal mine, comprising the following raw materials: 50kg natural rubber, 50kg butadiene rubber, 45kg carbon black N220, 5kg zinc oxide, 2kg stearic acid, 5kg aromatic oil, 1.5kg antioxidant RD, 1.0kg antioxidant CZ, 1.3kg accelerator CZ, 0.5g accelerator DM, 25kg chlorinated paraffin 70, 19kg powder flame retardant filler, 0.3kg surfactant silane coupling agent and 2kg vulcanizing agent-sulfur; the powder filler is composed of 4kg antimony trioxide and 15kg aluminum hydroxide ATH-8.
[0067] The preparation method of the rubber flame retardant material for underground conveyor belts in coal mines comprises the following steps:
[0068] Step 1: Mix 15 kg of aluminum hydroxide and 0.3 kg of a surface-active silane coupling agent, stir evenly, and dry at 50° C. to obtain component A;
[0069] Step 2: 50 kg of natural rubber and 50 kg of butadiene rubber are put into an internal mixer at a rotor speed of 33 r / min and a top bolt pressure of 3.5 bar, and mixed for 25 seconds to obtain component B;
[0070] Step 3, add component A, 25kg chlorinated paraffin 70, 5kg zinc oxide, 4kg antimony trioxide, 2kg stearic acid, 5kg aromatic oil, 1.5kg antioxidant RD, 1.0kg antioxidant CZ, 1.3kg accelerator CZ and 0.5g accelerator DM to component B, and continue mixing for 80s to obtain component C;
[0071] Step 4: Add 45 kg of reinforcing agent carbon black N220 to component C, continue mixing for 110 seconds, control the debonding temperature to ≤130°C, and debond; further mix on an open mixer (cut off twice and turn over three times), then calender the sheet, pass through a release agent tank, and then enter a wind room to cool to room temperature to obtain component D;
[0072] Step 5: After the D component is parked for 8 hours, it is put into an internal mixer, 2 kg of sulfur vulcanizer is added, the rotor speed is 22 r / min, the top bolt pressure is 3.5 bar, and the mixing is performed for 110 seconds. The discharge temperature is controlled to be ≤95°C, and the rubber is discharged; after further mixing in the open mixer, the lower sheet is calendered, and after passing through the isolation agent tank, it enters the wind room to cool to room temperature, and a rubber flame retardant material for underground conveyor belts in coal mines is obtained.
[0073] Among them, the molecular structure formula of the surface active silane coupling agent is:
[0074] .
[0075] The preparation method of the surface active silane type coupling agent comprises the following steps:
[0076] S1. At a temperature of 70°C, 326.0 g of N-octadecyl-1,3-propylene diamine (1 mol) was dissolved in 750 g of isopropanol, and then 245.8 g of 3-glycidyloxypropyltrimethoxysilane (1.04 mol) was gradually added, and the reaction was stirred at a temperature of 70°C for 4 hours to obtain a reaction intermediate I. The structural formula of the reaction intermediate I is:
[0077] ;
[0078] S2. Add 147.0 g of acrylic acid (2.04 mol) to the intermediate I, and stir the mixture at 70° C. for 3 h to obtain a reaction intermediate II. The structural formula of the reaction intermediate II is:
[0079] ;
[0080] S3. Dissolve 421.2 g of sodium 3-chloro-2-hydroxypropyl sulfonate (2.1 mol, purity 98%) in 842 g of water to obtain an aqueous solution of sodium 3-chloro-2-hydroxypropyl sulfonate, and add the aqueous solution to the reaction intermediate II. Stir the reaction at 70° C. for 5 h to obtain a surface-active silane coupling agent.
[0081] The reaction equations of each step of the preparation method of the surface active silane coupling agent are:
[0082] S1:
[0083] ;
[0084] S2:
[0085] ;
[0086] S3:
[0087] .
[0088] Infrared spectrum analysis of surface active silane coupling agent Figure 1 shown.
[0089] Depend on Figure 1 It can be seen that:
[0090] 3386 cm-1 (peak 1) is the OH stretching vibration absorption peak;
[0091] 2920 cm-1 (peak 2) is the asymmetric stretching vibration absorption peak of methylene;
[0092] 2852 cm-1 (peak 3) is the peak of symmetric stretching vibration of methylene;
[0093] 1714 cm-1 (peak 4) is the stretching vibration peak of carboxylic acid C=O;
[0094] 1469 cm-1 (peak 5) is the asymmetric bending vibration of methylene;
[0095] 1394 cm-1 (peak 6) is the symmetric bending vibration of methylene;
[0096] 1197 cm-1 (peak 7) is the symmetric stretching vibration absorption peak of sulfonic acid group S=O;
[0097] 1041 cm-1 (peak 8) is the asymmetric stretching vibration absorption peak of sulfonic acid group S=O;
[0098] 817cm-1 (peak 9) is the Si-C stretching vibration absorption peak;
[0099] 721 cm-1 (peak 10) is the in-plane rocking vibration of the methylene group;
[0100] 487 cm-1 (peak 11) is the Si-O absorption peak.
[0101] Example 2
[0102] The difference from Example 1 is that the added amount of the surface active silane coupling agent is adjusted from 0.3 kg to 0.75 kg.
[0103] Example 3
[0104] The difference from Example 1 is that the added amount of the surface active silane coupling agent is adjusted from 0.3 kg to 1.5 kg.
[0105] Example 4
[0106] The difference from Example 1 is that the components and preparation method of the rubber flame retardant material for underground conveyor belts in coal mines are slightly different, as follows.
[0107] A rubber flame retardant material for an underground conveyor belt in a coal mine, comprising the following raw materials: 50kg natural rubber, 50kg butadiene rubber, 45kg carbon black N220, 5kg zinc oxide, 0kg stearic acid, 5kg aromatic oil, 1.5kg antioxidant RD, 1.0kg antioxidant CZ, 1.3kg accelerator CZ, 0.5g accelerator DM, 25kg chlorinated paraffin 70, 19kg powder flame retardant filler, 0.24kg surfactant silane coupling agent and 2kg vulcanizing agent-sulfur; the powder filler is composed of 4kg antimony trioxide and 15kg aluminum hydroxide ATH-8.
[0108] The preparation method of the rubber flame retardant material for underground conveyor belts in coal mines comprises the following steps:
[0109] Step 1: 5 kg zinc oxide, 4 kg antimony trioxide, 15 kg aluminum hydroxide and 0.24 kg surface active silane coupling agent are mixed, stirred evenly, and dried at a temperature of 50° C. to obtain component A;
[0110] Step 2: 50 kg of natural rubber and 50 kg of butadiene rubber are put into an internal mixer at a rotor speed of 33 r / min and a top bolt pressure of 3.5 bar, and mixed for 25 seconds to obtain component B;
[0111] Step 3: Add component A, 25kg chlorinated paraffin 70, 0kg stearic acid, 5kg aromatic oil, 1.5kg antioxidant RD, 1.0kg antioxidant CZ, 1.3kg accelerator CZ and 0.5g accelerator DM to component B, and continue mixing for 80s to obtain component C;
[0112] Step 4: Add 45 kg of reinforcing agent carbon black N220 to component C, continue mixing for 110 seconds, control the debonding temperature to ≤130°C, and debond; further mix on an open mixer (cut off twice and turn over three times), then calender the sheet, pass through a release agent tank, and then enter a wind room to cool to room temperature to obtain component D;
[0113] Step 5: After the D component is parked for 8 hours, it is put into an internal mixer, 2 kg of sulfur vulcanizer is added, the rotor speed is 22 r / min, the top bolt pressure is 3.5 bar, and the mixing is performed for 110 seconds. The discharge temperature is controlled to be ≤95°C, and the rubber is discharged; after further mixing in the open mixer, the lower sheet is calendered, and after passing through the isolation agent tank, it enters the wind room to cool to room temperature, and a rubber flame retardant material for underground conveyor belts in coal mines is obtained.
[0114] Example 5
[0115] The difference from Example 4 is that the amount of the surface active silane coupling agent added was adjusted from 0.24 kg to 0.48 kg.
[0116] Comparative Example
[0117] Comparative Example 1
[0118] The difference from Example 1 is that no surface active silane coupling agent is added.
[0119] Comparative Example 2
[0120] The difference from Example 4 is that no surface active silane coupling agent is added.
[0121] Performance testing
[0122] Detection Methods
[0123] Three samples were taken from Examples 1-5 and Comparative Examples 1-2 respectively, and then the various properties of the samples were tested with reference to MT / T914-2019 "Fabric Core Flame-Retardant Conveyor Belts for Coal Mines" and GB / T10707-2008 "Determination of Rubber Combustion Performance", and the average values were taken.
[0124] The test data are shown in Tables 1 and 2.
[0125] Table 1 Performance test table of Examples 1-3 and Comparative Example 1
[0126]
[0127] Referring to Examples 1-3 and Comparative Example 1 and in combination with Table 1, it can be seen that, relative to Comparative Example 1, the tensile strength and elongation of Example 1 are significantly improved, while the oxygen index of Example 1 does not change much, which indicates that the addition of a surface active silane coupling agent can significantly improve the mechanical properties of the conveyor belt rubber material without affecting its flame retardant properties.
[0128] The reason may be that the surface active silane coupling agent in the present application contains siloxane group, hydroxyl group, long carbon chain alkyl group, carboxyl group, sodium sulfonate group, quaternary ammonium salt group and flame retardant element silicon at the same time, among which siloxane group and hydroxyl group can play the role of silane coupling agent, long carbon chain alkyl group, carboxyl group, sodium sulfonate group and quaternary ammonium salt group play the role of surfactant, surface dispersion and surface modification, thereby improving the negative effects caused by poor dispersibility of powder flame retardant filler.
[0129] Compared with Example 1, the tensile strength and elongation of Example 2 are slightly decreased, and the tensile strength and elongation of Example 3 are further decreased, especially the elongation of Example 3 is even lower than that of Comparative Example 1. This shows that although the addition of the surfactant silane coupling agent can enable the conveyor belt rubber material to obtain extremely good mechanical properties and flame retardant properties, excessive addition of the surfactant silane coupling agent will lead to a decrease in the mechanical properties of the conveyor belt rubber material.
[0130] Table 2 Performance test table of Examples 4-5 and Comparative Example 2
[0131]
[0132] With reference to Comparative Example 2, Example 4 and Example 1 and in combination with Table 1-2, it can be seen that, relative to Comparative Example 2, the tensile strength and elongation of Example 4 are significantly improved, and at the same time, the oxygen index of Example 4 is also significantly improved, and the mean and maximum values of the alcohol burner flame combustion test in Example 4 are also significantly reduced. This shows that the addition of the surfactant silane coupling agent can not only significantly improve the mechanical properties of the conveyor belt rubber material, but also actually improve its flame retardant properties under certain conditions.
[0133] The reason is that the sodium sulfonate group in the surfactant silane coupling agent also acts as a catalyst, thereby promoting catalytic carbonization and improving the thermal stability and flame retardant properties of the material; and the presence of elemental silicon provides excellent flame retardant properties.
[0134] Compared with Example 4, the tensile strength, elongation and oxygen index of Example 1 are significantly reduced. The reason may be that the addition of stearic acid has a negative effect on the flame retardant and mechanical properties of the surfactant silane coupling agent, or in step 1, compared with only mixing aluminum hydroxide with the surfactant silane coupling agent, the operation of mixing zinc oxide, antimony trioxide and aluminum hydroxide with the surfactant silane coupling agent can obtain better mechanical properties and flame retardant properties.
[0135] Referring to Examples 4-5 and in combination with Table 2, it can be seen that, relative to Example 4, although the tensile strength and oxygen index of Example 5 are substantially unchanged, the elongation of Example 5 is significantly reduced, even lower than that of Comparative Example 2, and the mean and maximum values of the alcohol burner flame combustion test are also improved, which indicates that the addition amount of the surface active silane coupling agent is relatively good between 0.24 and 0.3, that is, the surface active silane coupling agent only needs a very low addition amount to obtain a good effect.
[0136] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A flame retardant rubber material for underground conveyor belts in coal mines, characterized in that: The rubber flame retardant material for underground conveyor belts in coal mines contains a powder flame retardant filler and a surface active silane coupling agent; The rubber flame retardant material for underground conveyor belts in coal mines comprises the following raw materials in parts by mass: 40-60 parts of natural rubber, 40-60 parts of butadiene rubber, 40-50 parts of reinforcing agent, 4-6 parts of activating agent, 0-3 parts of stearic acid, 4-6 parts of aromatic oil, 1.5-3.5 parts of antioxidant, 0.8-2.8 parts of accelerator, 20-30 parts of chlorinated paraffin, 12-26 parts of powdered flame retardant filler, 0.1-0.8 parts of surface active silane coupling agent and 1-4 parts of vulcanizing agent; The powder flame retardant filler is composed of 2-6 parts of antimony trioxide and 10-20 parts of aluminum hydroxide; The molecular structural formula of the surface active silane coupling agent is: ; The preparation method of the surface active silane type coupling agent comprises the following steps: S1. First, N-octadecyl-1,3-propylene diamine and 3-glycidyloxypropyltrimethoxysilane are mixed and reacted in isopropanol to obtain a reaction intermediate I. The structural formula of the reaction intermediate I is: ; S2, adding acrylic acid to the intermediate I, mixing and reacting to obtain a reaction intermediate II, the structural formula of the reaction intermediate II is: ; S3, adding the aqueous solution of sodium 3-chloro-2-hydroxypropyl sulfonate to the reaction intermediate II, mixing and reacting, and obtaining a surface active silane coupling agent.
2. The flame retardant rubber material for underground conveyor belts in coal mines according to claim 1, characterized in that: The molar ratio of the N-octadecyl-1,3-propylene diamine, 3-glycidyloxypropyltrimethoxysilane, acrylic acid, and sodium 3-chloro-2-hydroxypropyl sulfonate is 1: (1.0-1.2): (2.0-2.2): (2.0-2.3).
3. The flame retardant rubber material for underground conveyor belts in coal mines according to claim 2, characterized in that: The mass ratio of the N-octadecyl-1,3-propylene diamine to isopropanol is 1:(1.3-3.3).
4. The flame retardant rubber material for underground conveyor belts in coal mines according to claim 1, characterized in that: In S1, the reaction temperature is 65-82°C and the reaction time is 3-5h; In S2, the reaction temperature is 65-82°C and the reaction time is 2-4h; In S3, the reaction temperature is 65-82°C and the reaction time is 4-6h.
5. The flame retardant rubber material for underground conveyor belts in coal mines according to claim 1, characterized in that: The active agent is one of zinc oxide and magnesium oxide or a mixture of both.
6. The flame retardant rubber material for underground conveyor belts in coal mines according to claim 1, characterized in that: The antioxidant is one of antioxidant 4010, antioxidant 4020 and antioxidant RD, or a mixture of several thereof.
7. The flame retardant rubber material for underground conveyor belts in coal mines according to claim 1, characterized in that: The accelerator is one of DM and CZ or a mixture of both.
8. A method for preparing the flame-retardant rubber material for underground conveyor belts in coal mines according to any one of claims 5 to 7, characterized in that: The following steps are involved: Step 1: Mix 4-6 parts of an active agent, 2-6 parts of antimony trioxide, 10-20 parts of aluminum hydroxide and 0.1-0.8 parts of a surface-active silane coupling agent, stir evenly, and dry at a temperature of 40-60° C. to obtain component A; Step 2: 40-60 parts of natural rubber and 40-60 parts of butadiene rubber are put into an internal mixer at a rotor speed of 30-35 r / min and a top bolt pressure of 2.5-4.0 bar, and mixed for 20-30 seconds to obtain component B; Step 3: Add component A, 20-30 parts of chlorinated paraffin 70, 0-3 parts of stearic acid, 4-6 parts of aromatic oil, 1.5-3.5 parts of antioxidant and 0.8-2.8 parts of accelerator to component B, and continue mixing for 60-90 seconds to obtain component C; Step 4: Add 40-50 parts of reinforcing agent to component C, continue mixing for 100-120 seconds, control the debonding temperature ≤130°C, debond; further mix on the open mill (cut off twice and turn over three times), then roll down the sheet, pass through the release agent tank, and enter the wind room to cool to room temperature to obtain component D; Step 5: After the D component is parked for 6-8 hours, it is put into an internal mixer, 1-4 parts of vulcanizer are added, the rotor speed is 20-25r / min, the top bolt pressure is 2.5-4.0bar, mixing is performed for 90-120s, and the discharge temperature is controlled to be ≤95°C, and the rubber is discharged; after further mixing in the open mixer, the sheet is calendered, and after passing through the isolation agent tank, it enters the wind room to cool to room temperature to obtain the rubber flame retardant material for underground conveyor belts in coal mines.