A high and low temperature resistant, super strong adhesive silicone sealant and preparation method thereof

By introducing terminal alkenyl polyurea resin and terminal hydrogen silicone oil crosslinking agent into silicone sealant to form a three-dimensional crosslinking network, the problems of adhesive strength and temperature resistance of silicone sealant under extreme temperatures are solved, and higher tensile strength and hardness are achieved.

CN118440665BActive Publication Date: 2024-11-12DONGGUAN XINYI ELECTRONIC MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410673060.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-11-12
Estimated Expiration
2044-05-28

AI Technical Summary

Technical Problem

Silicone sealants have poor temperature resistance, low bonding strength, and poor mechanical properties in extreme climates.

Method used

α,ω-vinyl polydimethylsiloxane is used as the main adhesive and terminal alkenyl polyurea resin is used as the modifier. By introducing terminal hydrogen silicone oil as a crosslinking agent, a chemically stable three-dimensional crosslinking network is formed, which improves the bonding performance and temperature resistance.

Benefits of technology

The cross-linked network maintains stability at low temperatures of -20℃ and high temperatures of 80℃, which improves the tensile strength and hardness of the silicone sealant, resulting in better adhesion and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118440665B_ABST
    Figure CN118440665B_ABST
Patent Text Reader

Abstract

The invention discloses a high and low temperature resistant, super strong adhesive organosilicon sealant and a preparation method thereof, wherein α,ω-vinyl polydimethylsiloxane is used as the main glue of the sealant, and terminal olefin polyurea resin is used as a modifier, and an organosilicon structure is introduced into the main chain of the polyurea resin, which has a good structural similarity with the main glue α,ω-vinyl polydimethylsiloxane in the organosilicon sealant, and the compatibility of the polyurea resin in the organosilicon sealant matrix can be improved. At the same time, two alkenyl groups are introduced at both ends of the polyurea resin, and terminal hydrogen silicone oil is used as a cross-linking agent, which can react with the alkenyl groups of α,ω-vinyl polydimethylsiloxane and the alkenyl groups of the polyurea resin to form a cross-linking reaction, thereby improving the cross-linking degree of the organosilicon sealant, forming a three-dimensional cross-linked network of chemical stability, and making the organosilicon sealant show higher bonding tensile properties, hardness, tensile strength and temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealants, in particular to an organosilicon sealant resistant to high and low temperatures and having super strong adhesion and a preparation method thereof. Background Art

[0002] Organic silicone adhesives have excellent weather resistance, UV resistance, water resistance and other properties. They can be used as building joint sealants and are widely used in building materials such as concrete and cement mortar. Traditional organic silicone adhesives have problems such as poor temperature resistance, low bonding strength, and poor mechanical properties. This limits the practical application of organic silicone sealants in building materials in extreme climates such as severe cold and heat. The development of high-performance organic silicone sealants has important applications.

[0003] Polyurea resin has high mechanical strength and good heat resistance, and can maintain good performance in harsh environments such as extreme climates. By compounding polyurea resin with organosiloxane, silicone rubber, etc., a composite material with excellent performance can be obtained, which has broad application prospects in the fields of adhesives, coatings, etc. Chinese patent CN114479741B discloses a one-component silicone modified sealant that can be quickly and deeply cured at low temperature and a preparation method thereof. The silicone modified sealant obtained uses trimethoxysilane-terminated polyurea resin, reinforcing fillers, functional fillers, plasticizers, etc. as raw materials, and has the advantages of good low-temperature curing performance and excellent mechanical properties. However, the amount of functional fillers and plasticizers added in this patent is relatively large, the preparation method is relatively complicated, and the tensile strength of the silicone modified sealant obtained is relatively low. It is not conducive to the practical application of silicone sealants. Summary of the invention

[0004] The technical problem solved by the invention is to solve the problems of poor high and low temperature resistance, low bonding strength and poor mechanical properties of organic silicon sealant.

[0005] The technical solution provided by the present invention is: a high and low temperature resistant and super-strong adhesive silicone sealant, comprising 80-93 parts by weight of α,ω-vinyl polydimethylsiloxane, 5-12 parts by weight of terminal hydrogen silicone oil, 2-8 parts by weight of terminal olefin silicon-containing polyurea resin, 0.25-0.32 parts by weight of 1-acetylene cyclohexanol inhibitor, and 0.12-0.2 parts by weight of Castaplatin catalyst.

[0006] The preparation method of the terminal olefin-containing silicon-containing polyurea resin is as follows:

[0007] (1) Nitrogen is introduced into a reaction vessel, and polyetheramine and isophorone diisocyanate are added to carry out a reaction.

[0008] (2) Then, a chain extender, bis(4-aminophenoxy)dimethylsilane, was added to the reaction vessel to carry out a reaction.

[0009] (3) Finally, add the structural formula 2-amino-1,3-propanediacrylate is reacted to obtain a terminal olefin-containing silicon-containing polyurea resin.

[0010] Furthermore, the molar ratio of polyetheramine, isophorone diisocyanate, bis(4-aminophenoxy)dimethylsilane and 2-amino-1,3-propanediacrylate is 1:(2.3-2.6):(1-1.1)(2.1-2.2).

[0011] Furthermore, the reaction temperature in (1) is 50-65°C, and the reaction time is 3-4h.

[0012] Furthermore, the reaction temperature in (2) is 50-65° C., and the reaction time is 1-1.5 h.

[0013] Furthermore, the reaction temperature in (3) is 35-50°C, and the reaction time is 20-40 min.

[0014] Furthermore, the preparation method of 2-amino-1,3-propanediacrylate in (3) is as follows: dichloromethane, N-Boc-serinol, acryloyl chloride and triethylamine in a molar ratio of 1:(2.3-2.8):(2.3-2.8) are added to a reaction container at -5 to 0°C, and then the mixture is stirred for reaction at room temperature for 6-10 hours, distilled water is added for extraction and separation, the organic phase is dried and concentrated, and the product is added to a dichloromethane solution of trifluoroacetic acid, wherein the volume ratio of trifluoroacetic acid to dichloromethane is (0.4-0.5):1, the mixture is stirred for reaction at room temperature for 2-3 hours, and the mixture is concentrated under reduced pressure, saturated sodium bicarbonate and ethyl acetate are added for extraction and separation, and the organic phase is dried and concentrated to obtain 2-amino-1,3-propanediacrylate.

[0015] Furthermore, the preparation method of the silicone sealant is as follows: α, ω-vinyl polydimethylsiloxane, terminal olefin silicon-containing polyurea resin, 1-ethynyl cyclohexanol inhibitor, and castaplatin catalyst are stirred and mixed, terminal hydrogen silicone oil is added, and vacuum degassing is performed after mixing to obtain a silicone sealant that is resistant to high and low temperatures and has super strong adhesion.

[0016] The technical effect produced by the present invention is as follows: the present invention uses polyetheramine D2000 and isophorone diisocyanate as polymerization monomers, bis(4-aminophenoxy)dimethylsilane as a chain extender, and 2-amino-1,3-propanediacrylate as a capping agent to prepare a novel terminal olefin polyurea resin containing organic siloxane in the main chain.

[0017] The present invention uses α,ω-vinyl polydimethylsiloxane as the main glue of the sealant and terminal olefinic polyurea resin as the modifier. The polyurea resin itself has excellent bonding performance, mechanical properties and temperature resistance, and an organic siloxane structure is introduced into the main chain of the polyurea resin, which has good structural similarity with the main glue α,ω-vinyl polydimethylsiloxane in the silicone sealant, and can improve the compatibility of the polyurea resin in the silicone sealant matrix. At the same time, two alkenyl groups are introduced at both ends of the polyurea resin, and terminal hydrogen silicone oil is used as a crosslinking agent, which can react with the alkenyl groups of α,ω-vinyl polydimethylsiloxane and the alkenyl groups of the polyurea resin to crosslink the polyurea resin, thereby grafting the polyurea resin into the α,ω-vinyl polydimethylsiloxane molecular chain, improving the crosslinking degree of the silicone sealant, forming a three-dimensional crosslinking network with chemical stability, and making the silicone sealant show higher bonding tensile properties, hardness and tensile strength. In addition, the chemically stable cross-linked network has good temperature resistance. The sealant can maintain a stable cross-linked network even when treated at low temperature of -20°C or high temperature of 80°C, allowing the sealant to maintain good tensile strength and hardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The invention is a reaction route for preparing 2-amino-1,3-propanediacrylate.

[0019] Figure 2 This is a reaction route for preparing terminal olefin-containing silicon-containing polyurea resin. DETAILED DESCRIPTION

[0020] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. Without departing from the scope or spirit of the present invention, various improvements and changes can be made to the specific embodiments of the present invention specification, which will be apparent to those skilled in the art. Other embodiments obtained from the description of the present invention will be apparent to the technician. This application description and examples are exemplary only.

[0021] Example 1

[0022] (1) At -5°C, 8 mL of dichloromethane, 5 mmol of N-Boc-serinol, 11.5 mmol of acryloyl chloride, and 11.5 mmol of triethylamine were added to a reaction container, and then stirred at room temperature for 10 h. Distilled water was added for extraction and separation. The organic phase was dried and concentrated. The product was added to a dichloromethane solution containing 2 mL of trifluoroacetic acid. The volume of the dichloromethane solution was 5 mL. The reaction was stirred at room temperature for 3 h. The reaction was concentrated under reduced pressure. Saturated sodium bicarbonate and ethyl acetate were added for extraction and separation. The organic phase was dried and concentrated to obtain 2-amino-1,3-propanediacrylate.

[0023] (2) nitrogen was introduced into the reaction vessel, 30 mmol polyetheramine D2000 and 69 mmol isophorone diisocyanate were added, and the reaction was carried out at 60°C for 4 h; then 30 mmol chain extender bis(4-aminophenoxy)dimethylsilane (structural formula: ), react at 50°C for 1h; finally, add 66mmol 2-amino-1,3-propanediacrylate, react at 50°C for 20min to obtain terminal olefin-containing silicon-containing polyurea resin.

[0024] (3) 93 g of α, ω-vinyl polydimethylsiloxane, 2 g of terminal olefin silicon-containing polyurea resin, 0.28 g of 1-ethynyl cyclohexanol inhibitor, and 0.12 g of Castaplatin catalyst were stirred and mixed, and 12 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a high and low temperature resistant and super strong adhesive silicone sealant.

[0025] Example 2

[0026] (1) At 0°C, 10 mL of dichloromethane, 5 mmol of N-Boc-serinol, 14 mmol of acryloyl chloride, and 14 mmol of triethylamine were added to a reaction container, and then stirred at room temperature for 6 h. Distilled water was added for extraction and separation. The organic phase was dried and concentrated. The product was added to a dichloromethane solution containing 2.5 mL of trifluoroacetic acid, the volume of the solution of dichloromethane was 5 mL, and the reaction was stirred at room temperature for 3 h. The mixture was concentrated under reduced pressure, saturated sodium bicarbonate and ethyl acetate were added for extraction and separation, and the organic phase was dried and concentrated to obtain 2-amino-1,3-propanediacrylate.

[0027] (2) nitrogen was introduced into the reaction vessel, 30 mmol polyetheramine D2000 and 75 mmol isophorone diisocyanate were added, and the mixture was reacted at 50°C for 4 h; then 33 mmol chain extender bis(4-aminophenoxy)dimethylsilane was added, and the mixture was reacted at 50°C for 1.5 h; finally 63 mmol 2-amino-1,3-propanediacrylate was added, and the mixture was reacted at 35°C for 40 min to obtain a terminal olefin-containing silicon-containing polyurea resin.

[0028] (3) 88 g of α, ω-vinyl polydimethylsiloxane, 4 g of terminal olefin silicon-containing polyurea resin, 0.32 g of 1-ethynyl cyclohexanol inhibitor, and 0.2 g of Castaplatin catalyst were stirred and mixed, and 10 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a high and low temperature resistant and super strong adhesive silicone sealant.

[0029] Example 3

[0030] (1) At -5°C, 10 mL of dichloromethane, 5 mmol of N-Boc-serinol, 13.2 mmol of acryloyl chloride, and 13.2 mmol of triethylamine were added to a reaction container, and then stirred at room temperature for 10 h. Distilled water was added for extraction and separation. The organic phase was dried and concentrated. The product was added to a dichloromethane solution containing 2 mL of trifluoroacetic acid. The volume of the dichloromethane solution was 5 mL. The reaction was stirred at room temperature for 3 h. The reaction was concentrated under reduced pressure. Saturated sodium bicarbonate and ethyl acetate were added for extraction and separation. The organic phase was dried and concentrated to obtain 2-amino-1,3-propanediacrylate.

[0031] (2) nitrogen was introduced into the reaction vessel, 30 mmol polyetheramine D2000 and 69 mmol isophorone diisocyanate were added, and the mixture was reacted at 50°C for 4 h; then 31 mmol chain extender bis(4-aminophenoxy)dimethylsilane was added, and the mixture was reacted at 50°C for 1.5 h; finally 64 mmol 2-amino-1,3-propanediacrylate was added, and the mixture was reacted at 40°C for 40 min to obtain a terminal olefin-containing silicon-containing polyurea resin.

[0032] (3) 84 g of α, ω-vinyl polydimethylsiloxane, 6 g of terminal olefin silicon-containing polyurea resin, 0.25 g of 1-ethynyl cyclohexanol inhibitor, and 0.15 g of Castaplatin catalyst were stirred and mixed, and 8 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a high and low temperature resistant and super strong adhesive silicone sealant.

[0033] Example 4

[0034] (1) At 0°C, 8 mL of dichloromethane, 5 mmol of N-Boc-serinol, 11.5 mmol of acryloyl chloride, and 11.5 mmol of triethylamine were added to a reaction container, and then stirred at room temperature for 8 h. Distilled water was added for extraction and separation. The organic phase was dried and concentrated. The product was added to a dichloromethane solution containing 2.5 mL of trifluoroacetic acid, the volume of the solution of dichloromethane was 5 mL, and the reaction was stirred at room temperature for 2 h. The mixture was concentrated under reduced pressure, saturated sodium bicarbonate and ethyl acetate were added, and the mixture was extracted and separated. The organic phase was dried and concentrated to obtain 2-amino-1,3-propanediacrylate.

[0035] (2) nitrogen was introduced into the reaction vessel, 30 mmol polyetheramine D2000 and 78 mmol isophorone diisocyanate were added, and the mixture was reacted at 65°C for 3 h; then 33 mmol chain extender bis(4-aminophenoxy)dimethylsilane was added, and the mixture was reacted at 65°C for 1 h; finally 66 mmol 2-amino-1,3-propanediacrylate was added, and the mixture was reacted at 3°C ​​for 30 min to obtain a terminal olefin-containing silicon-containing polyurea resin.

[0036] (3) 80 g of α, ω-vinyl polydimethylsiloxane, 8 g of terminal olefin silicon-containing polyurea resin, 0.32 g of 1-ethynyl cyclohexanol inhibitor, and 0.14 g of Castaplatin catalyst were stirred and mixed, and 5 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a high and low temperature resistant and super strong adhesive silicone sealant.

[0037] Comparative Example 1

[0038] (1) 93 g of α, ω-vinyl polydimethylsiloxane, 0.28 g of 1-ethynyl cyclohexanol inhibitor, and 0.12 g of Castaplatin catalyst were stirred and mixed, and 12 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain an organic silicone sealant.

[0039] Comparative Example 2

[0040] (2) nitrogen was introduced into the reaction vessel, 30 mmol polyetheramine D2000 and 69 mmol isophorone diisocyanate were added, and the mixture was reacted at 60° C. for 4 h; then 30 mmol chain extender bis(4-aminophenoxy)dimethylsilane was added, and the mixture was reacted at 50° C. for 1 h to obtain a silicon-containing polyurea resin.

[0041] (3) 93 g of α, ω-vinyl polydimethylsiloxane, 2 g of silicon-containing polyurea resin, 0.28 g of 1-ethynyl cyclohexanol inhibitor, and 0.12 g of Castaplatin catalyst were stirred and mixed, and 12 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a silicone sealant.

[0042] Comparative Example 3

[0043] (1) Nitrogen was introduced into a reaction vessel, 30 mmol polyetheramine D2000 and 69 mmol isophorone diisocyanate were added, and the mixture was reacted at 60°C for 4 h; then 30 mmol chain extender bis(4-aminophenoxy)dimethylsilane was added, and the mixture was reacted at 50°C for 1 h; finally 66 mmol hydroxyethyl acrylate was added, and the mixture was reacted at 50°C for 20 min to obtain a terminal olefin-containing silicon-containing polyurea resin.

[0044] (2) 93 g of α, ω-vinyl polydimethylsiloxane, 2 g of terminal olefin silicon-containing polyurea resin, 0.28 g of 1-ethynyl cyclohexanol inhibitor, and 0.12 g of Castaplatin catalyst were stirred and mixed, and 12 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a silicone sealant.

[0045] Comparative Example 4

[0046] (1) Nitrogen was introduced into a reaction container, 30 mmol polyetheramine D2000 and 69 mmol isophorone diisocyanate were added, and the mixture was reacted at 60° C. for 4 h; then 30 mmol chain extender ethylenediamine was added, and the mixture was reacted at 50° C. for 1 h; finally 66 mmol 2-amino-1,3-propanediacrylate (prepared according to the method of Example 1) was added, and the mixture was reacted at 50° C. for 20 min to obtain a terminal olefin polyurea resin.

[0047] (2) 93 g of α, ω-vinyl polydimethylsiloxane, 2 g of terminal olefin polyurea resin, 0.28 g of 1-ethynyl cyclohexanol inhibitor, and 0.12 g of Castaplatin catalyst were stirred and mixed, and 12 g of terminal hydrogen silicone oil was added. After mixing, vacuum degassing was performed to obtain a silicone sealant.

[0048] According to JC / T 881-2001 standard, the bonding performance of organic silicon sealant to cement mortar board was tested. The curing conditions of the sealant bonding cement mortar board specimen were 60℃×48h, and then placed at room temperature for 28 days. The bonding performance test is shown in the following table.

[0049] Table 1 Adhesion performance test

[0050]

[0051]

[0052] Pour the silicone sealant into the mold, cure it at 80℃ for 24h, and then place it at 25℃ for 3 days. Test the hardness of the sealant cure according to GB / T 531.1-2009. Test the tensile strength according to GB / T 528-2009.

[0053] The cured sealant is placed at 25°C for 240 hours, or at -20°C for 240 hours, or at 80°C for 240 hours, and then placed at room temperature for 6 hours before testing the hardness and tensile strength of the cured sealant.

[0054] Table 2 Mechanical properties test of sealant

[0055]

[0056] As can be seen from Table 1 and Table 2, the silicone sealants in Examples 1-4 are added with terminal olefinic polyurea resins, and the polyurea resins themselves have excellent bonding properties, mechanical properties and temperature resistance, and an organosiloxane structure is introduced into the main chain of the polyurea resin, which has a good structural similarity with the main resin α,ω-vinyl polydimethylsiloxane in the silicone sealant, and can improve the compatibility of the polyurea resin in the silicone sealant matrix. At the same time, two alkenyl groups are introduced at both ends of the polyurea resin, and terminal hydrogen silicone oil is used as a cross-linking agent, which can react with the alkenyl groups of α,ω-vinyl polydimethylsiloxane and the alkenyl groups of the polyurea resin to undergo cross-linking reactions, thereby grafting the polyurea resin into the α,ω-vinyl polydimethylsiloxane molecular chain, thereby improving the cross-linking degree of the silicone sealant, forming a three-dimensional cross-linked network with chemical stability, and making the silicone sealant exhibit higher bonding tensile properties, hardness and tensile strength. In addition, the chemically stable cross-linked network has good temperature resistance. The sealant can maintain a stable cross-linked network even when treated at low temperature of -20°C or high temperature of 80°C, allowing the sealant to maintain good tensile strength and hardness.

[0057] Compared with Example 1, in Comparative Example 1, no terminal olefin polyurea resin is added, and the tensile bonding performance of the silicone sealant is low, and the tensile strength and hardness are poor.

[0058] The silicon-containing polyurea resin in Comparative Example 2 is not end-capped with 2-amino-1,3-propanediacrylate, and its end position does not contain an olefin group. It cannot be chemically cross-linked with terminal hydrogen silicone oil and α,ω-vinyl polydimethylsiloxane, and a stable three-dimensional cross-linked network is not formed. The silicone sealant has low tensile bonding properties, and poor tensile strength and hardness.

[0059] Comparative Example 3 uses hydroxyethyl acrylate as a capping agent. Compared with Example 1, the terminal alkenyl silicon-containing polyurea resin of Comparative Example 3 has one alkenyl group at each end, which can only be cross-linked with terminal hydrogen silicone oil and α, ω-vinyl polydimethylsiloxane to form a linear structure, and cannot form a stable three-dimensional cross-linked network. The tensile bonding performance of the silicone sealant is low, and the tensile strength and hardness are poor.

[0060] In Comparative Example 4, ethylenediamine is used instead of bis(4-aminophenoxy)dimethylsilane as a chain extender. The main chain of the obtained terminal olefin polyurea resin does not contain a siloxane structure, and the compatibility with α,ω-vinyl polydimethylsiloxane is poor. The tensile bonding performance of the silicone sealant is low, and the tensile strength and hardness are poor.

[0061] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A silicone sealant, characterized in that: The organic silicone sealant comprises 80-93 parts by weight of α,ω-vinyl polydimethylsiloxane, 5-12 parts by weight of terminal hydrogen silicone oil, 2-8 parts by weight of terminal olefin silicon-containing polyurea resin, 0.25-0.32 parts by weight of 1-ethynyl cyclohexanol inhibitor, and 0.12-0.2 parts by weight of Castaplatin catalyst; The preparation method of the terminal olefin-containing silicon-containing polyurea resin is as follows: (1) introducing nitrogen into a reaction vessel, adding polyetheramine and isophorone diisocyanate, and reacting; (2) then adding a chain extender, bis(4-aminophenoxy)dimethylsilane, into the reaction vessel to carry out a reaction; (3) Finally, add the structural formula 2-amino-1,3-propanediacrylate is reacted to obtain a terminal olefin-containing silicon-containing polyurea resin.

2. The organic silicon sealant according to claim 1, characterized in that: The molar ratio of the polyetheramine, isophorone diisocyanate, bis(4-aminophenoxy)dimethylsilane and 2-amino-1,3-propanediacrylate is 1:(2.3-2.6):(1-1.1):(2.1-2.2).

3. The organic silicon sealant according to claim 1, characterized in that: The reaction temperature in (1) is 50-65°C and the reaction time is 3-4h.

4. The organic silicon sealant according to claim 1, characterized in that: The reaction temperature in (2) is 50-65°C and the reaction time is 1-1.5h.

5. The organic silicon sealant according to claim 1, characterized in that: The reaction temperature in (3) is 35-50°C and the reaction time is 20-40 min.

6. The organic silicon sealant according to claim 1, characterized in that: The preparation method of 2-amino-1,3-propanediacrylate in (3) is as follows: dichloromethane, N-Boc-serinol, acryloyl chloride and triethylamine are added to a reaction container at -5 to 0°C, and then the mixture is stirred for reaction for 6-10 hours at room temperature. After extraction and separation, the product is added to a dichloromethane solution of trifluoroacetic acid, and the mixture is stirred for reaction for 2-3 hours at room temperature. The mixture is concentrated under reduced pressure, extracted and separated, and dried to obtain 2-amino-1,3-propanediacrylate.

7. The organic silicon sealant according to claim 6, characterized in that: The molar ratio of the N-Boc-serinol, acryloyl chloride and triethylamine is 1:(2.3-2.8):(2.3-2.8).

8. The organic silicon sealant according to claim 6, characterized in that: The volume ratio of trifluoroacetic acid to dichloromethane is (0.4-0.5):

1.

9. A method for preparing the organosilicon sealant according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: mixing α,ω-vinyl polydimethylsiloxane, terminal olefin silicon-containing polyurea resin, 1-ethynyl cyclohexanol inhibitor and castar platinum catalyst, adding terminal hydrogen silicone oil, mixing and vacuum degassing to obtain the organic silicone sealant.