Thin-film ceramic processing method, device, equipment and readable storage medium

By bonding the ceramic blank to the metal plate and processing and cleaning it multiple times, the problems of accuracy and efficiency in sheet ceramic processing are solved, and high-precision and high-efficiency sheet ceramic production are achieved.

CN118456667BActive Publication Date: 2024-11-22HUIZHOU BEST NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410760020.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-11-22
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The existing thin-sheet ceramic processing technology has problems of low processing efficiency, poor accuracy and high cost, especially under the micron-level requirements of thin-sheet ceramics below 1mm, it is difficult to ensure the accuracy of the product.

Method used

Use wax to bond the ceramic blank to be processed to the preset metal plate, and after initial processing, cleaning and multiple transfers to the metal plates of different sizes for fine processing. Finally, the wax layer is removed by cleaning to ensure the accuracy of the ceramic. and quality.

Benefits of technology

It realizes efficient and high-precision thin-sheet ceramic processing, and mass-produced thin-sheet sheet thickness accuracy is within -0.002 to 0.002, improving production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118456667B_ABST
    Figure CN118456667B_ABST
Patent Text Reader

Abstract

The present application provides a method, device, equipment and readable storage medium for processing thin ceramics. The method provided by the present application can fix the ceramic blank to be processed on a metal plate, and perform primary processing and fine processing on it, so that the precision of the processed thin ceramics can be within ‑0.002 to +0.002, and thin ceramics with finer thickness precision of thin plates can be efficiently mass-produced. Specifically, thin ceramics with a thickness precision of thin plates within ‑0.002 to 0.002 can be mass-processed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of ceramic processing technology, and in particular to a method, device, equipment and readable storage medium for processing thin ceramic slices. Background Art

[0002] In practical applications, thin-film ceramic processing technology is a recently developed advanced process used to process various thin-film ceramic materials, such as alumina, zirconia, and silicon nitride. Thin-film ceramics offer excellent properties such as high strength, high hardness, high-temperature resistance, and corrosion resistance, and have broad application prospects in electronics, machinery, chemicals, and medicine.

[0003] Traditional methods for processing thin ceramics primarily include machining, electro-discharge machining (EDM), and laser machining. While these methods can produce thin ceramic parts, they suffer from low efficiency, poor precision, and high costs. For example, due to the inherent non-conductivity of ceramics, ensuring micron-level precision when processing thin ceramics less than 1 mm has always been a technical challenge. Therefore, there is a pressing need for efficient, high-precision, and low-cost thin ceramic processing technology. Summary of the Invention

[0004] The present application aims to solve at least one of the above-mentioned technical defects. In view of this, the present application provides a thin-film ceramic processing method, device, equipment and readable storage medium to solve the technical defects of mass production of high-precision thin-film ceramics in the existing technology.

[0005] A method for processing thin ceramic slices, comprising:

[0006] Using wax to bond the ceramic blank to be processed onto a first metal plate of a preset first size to obtain a first target ceramic;

[0007] Performing preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate, and marking a first mark on the preliminary processed side to obtain a second target ceramic;

[0008] removing the second target ceramic from the first metal plate and cleaning it using a preset solvent according to a preset cleaning procedure to obtain a third target ceramic;

[0009] Adhere the side of the third target ceramic having the first mark to a second metal plate of a preset second size using wax to obtain a fourth target ceramic;

[0010] processing a surface of the fourth target ceramic that is not adhered to the second metal plate, and marking the processed surface with a second mark to obtain a fifth target ceramic;

[0011] removing the fifth target ceramic from the second metal plate and cleaning it using the preset solvent according to the preset cleaning procedure to obtain a sixth target ceramic;

[0012] Adhere the side of the sixth target ceramic having the second mark to a third metal plate of a preset third size using wax to obtain a seventh target ceramic;

[0013] processing the surface of the seventh target ceramic that is not adhered to the third metal plate to obtain an eighth target ceramic;

[0014] The eighth target ceramic is removed from the third metal plate and cleaned using the preset solvent according to the preset cleaning procedure to obtain a target thin ceramic.

[0015] Preferably, the method further comprises:

[0016] Performing quality inspection on the target ceramic slice according to preset quality inspection requirements;

[0017] Determining whether the target thin-film ceramic is qualified according to a quality inspection result of the target thin-film ceramic;

[0018] If the target thin-film ceramic passes the quality inspection, determining that the processing of the target thin-film ceramic is completed;

[0019] If the target thin-film ceramic fails the quality inspection, a reprocessing procedure for the target thin-film ceramic is initiated.

[0020] Preferably, the preliminary processing of the side of the ceramic blank to be processed that is not adhered to the first metal plate includes:

[0021] According to a preset first processing requirement, performing preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate;

[0022] The preset first processing requirements include the following:

[0023] Cutting and trimming the first target ceramic according to a preset ceramic shape requirement, and ensuring that an error between an actual size of the first target ceramic and a preset ceramic size is within a preset first range, wherein the preset first range is set to [0 mm, 0.01 mm];

[0024] According to the preset ceramic thickness requirement, the side of the first target ceramic that is not adhered to the first metal plate is polished, and the side of the first target ceramic that is not adhered to the first metal plate is ensured to remain flat.

[0025] Preferably, processing the surface of the fourth target ceramic that is not adhered to the second metal plate includes:

[0026] According to a preset second processing requirement, processing a surface of the fourth target ceramic that is not adhered to the second metal plate;

[0027] Among them, the preset second processing requirements include the following:

[0028] According to preset ceramic design requirements, the size, processing accuracy, and smoothness of the fourth target ceramic are processed to ensure that the error between the actual size of the fourth target ceramic and the preset size is within a preset second range, the error between the actual processing accuracy of the fourth target ceramic and the preset processing accuracy is within a preset third range, and the error between the actual smoothness of the fourth target ceramic and the preset smoothness is within a preset fourth range;

[0029] Wherein, the second range is set to [0.3mm, 0.6mm];

[0030] The third range is set to [-0.002, 0.002];

[0031] The fourth range is set to [0, 0.6].

[0032] Preferably, processing the side of the seventh target ceramic that is not adhered to the third metal plate includes:

[0033] According to a preset third processing requirement, processing the surface of the seventh target ceramic that is not adhered to the third metal plate;

[0034] The preset third processing requirements include the following:

[0035] According to a preset ceramic design requirement, the error between the actual size of the surface of the seventh target ceramic that is not adhered to the third metal plate and the preset size is controlled within a preset fifth range;

[0036] The preset fifth range is set to [0 mm, 0.005 mm].

[0037] Preferably,

[0038] The thickness of the wax layer between the first metal plate and the ceramic blank to be processed is a preset first threshold value, and the preset first size is designed according to ceramic processing requirements;

[0039] The thickness of the wax layer between the third target ceramic and the second metal plate is a preset second threshold value, and the preset second size is designed according to ceramic processing requirements;

[0040] The thickness of the wax layer between the third metal plate and the sixth target ceramic is a preset first threshold, and the preset third dimension is designed according to ceramic processing requirements;

[0041] Preferably,

[0042] The preset first size is set to be 150 mm in length and width respectively, and 20 mm in height;

[0043] The preset second size is set to be 150 mm in length and width respectively, and 20 mm in height;

[0044] The preset third size is set to be 100 mm in length and width respectively, and 20 mm in height;

[0045] The value range of the preset first threshold is set to [0.05mm, 0.15mm];

[0046] The value range of the preset second threshold is set to [0.05mm, 0.15mm].

[0047] Preferably, the preset cleaning program includes:

[0048] Dewaxing and cleaning the ceramic removed from the metal plate using a preset solvent at a preset temperature;

[0049] in,

[0050] The preset solvent includes a dewaxing agent;

[0051] The preset temperature range is set to [40° C., 55° C.].

[0052] A thin ceramic processing device, comprising:

[0053] a first processing unit, configured to bond the ceramic blank to be processed onto a first metal plate of a preset first size using wax to obtain a first target ceramic;

[0054] a first processing unit for performing preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate, and marking a first mark on the preliminary processed side to obtain a second target ceramic;

[0055] a first cleaning unit, configured to remove the second target ceramic from the first metal plate and clean it using a preset solvent according to a preset cleaning procedure to obtain a third target ceramic;

[0056] a second processing unit, configured to adhere the side of the third target ceramic having the first mark to a second metal plate of a preset second size using wax to obtain a fourth target ceramic;

[0057] a second processing unit, configured to process a surface of the fourth target ceramic that is not adhered to the second metal plate, and mark the processed surface with a second mark to obtain a fifth target ceramic;

[0058] a second cleaning unit, configured to remove the fifth target ceramic from the second metal plate and clean it using the preset solvent according to the preset cleaning procedure to obtain a sixth target ceramic;

[0059] a third processing unit, configured to adhere the side of the sixth target ceramic having the second mark to a third metal plate of a preset third size using wax to obtain a seventh target ceramic;

[0060] a third processing unit, configured to process a side of the seventh target ceramic that is not adhered to the third metal plate to obtain an eighth target ceramic;

[0061] The third cleaning unit is used to remove the eighth target ceramic from the third metal plate and clean it using the preset solvent according to the preset cleaning procedure to obtain a target thin ceramic.

[0062] A thin-film ceramic processing device includes: one or more processors, and a memory;

[0063] The memory stores computer-readable instructions, and when the computer-readable instructions are executed by the one or more processors, the steps of the thin-film ceramic processing method as described in any one of the above introductions are implemented.

[0064] A readable storage medium stores computer-readable instructions. When the computer-readable instructions are executed by one or more processors, the one or more processors implement the steps of the thin-film ceramic processing method as described in any one of the above descriptions.

[0065] It can be seen from the technical solution introduced above that when thin-film ceramics need to be processed, the method provided in the embodiment of the present application can use wax to bond the ceramic blank to be processed to a first metal plate of a preset first size, thereby obtaining a first target ceramic. The first target ceramic is the ceramic to be processed, wherein, in order to ensure that the processed ceramic can meet the preset design requirements, the thickness of the wax layer between the first metal plate and the ceramic blank to be processed can be a preset first threshold; so that the blank to be processed and the first metal plate can be more tightly bonded to avoid the ceramic blank to be processed from loosening during the processing process and being unable to be processed smoothly; therefore, after the ceramic blank to be processed is fixed on the first metal plate, the side of the ceramic blank to be processed that is not bonded to the first metal plate can be preliminarily processed, and a first mark can be made on the preliminarily processed side, thereby obtaining a second target ceramic; wherein, the preliminarily processing of the ceramic blank to be processed this time is mainly to process the ceramic blank to be processed into the shape required by the target thin-film ceramic so that further fine processing can be performed.

[0066] Therefore, after preliminary processing of the side of the ceramic blank to be processed that is not adhered to the first metal plate, the second target ceramic can be further removed from the first metal plate. Since the unprocessed side of the second target ceramic is adhered to the first metal plate through the wax layer, if the second target ceramic continues to be fine-processed, these residual wax layers may affect the effect of further processing. Therefore, it is necessary to clean the second target ceramic removed from the first metal plate according to the preset cleaning procedure and use a preset solvent to remove the wax layer remaining on the second target ceramic, thereby obtaining the third target ceramic.

[0067] The third target ceramic is continued to be adhered to the second metal plate of a preset second size with wax so as to perform fine processing on the third target ceramic, thereby obtaining a fourth target ceramic, wherein, since the side of the third target ceramic with the first mark is the side that has been preliminarily processed, the side of the third target ceramic with the first mark can be adhered to the second metal plate to process the other side of the third target ceramic, wherein, in order to better fix the third target ceramic and the second metal plate, the thickness of the wax layer between the third target ceramic and the second metal plate can be set to a preset second threshold; then, the side of the fourth target ceramic that is not adhered to the second metal plate can be processed, and the second mark can be marked on the processed side to obtain a fifth target ceramic; since the unprocessed side of the fifth target ceramic is adhered to the second metal plate through the wax layer, if the fifth target ceramic is continued to be finely processed, the residual wax layer may affect the effect of further processing, therefore, the fifth target ceramic needs to be removed from the second metal plate, and the fifth target ceramic removed from the second metal plate is cleaned using a preset solvent according to a preset cleaning procedure to remove the wax layer remaining on the fifth target ceramic, thereby obtaining a sixth target ceramic.

[0068] Use wax to continue to bond the sixth target ceramic to the third metal plate of a preset third size, so that the sixth target ceramic can continue to be fine-processed, thereby obtaining the seventh target ceramic, wherein, since the side of the sixth target ceramic with the second mark has been fine-processed, the side of the sixth target ceramic with the second mark can be bonded to the third metal plate, wherein, in order to better fix the third target ceramic and the second metal plate, the thickness of the wax layer between the third metal plate and the sixth target ceramic can be set to a preset first threshold; and the side of the seventh target ceramic that is not bonded to the third metal plate is processed, thereby obtaining the eighth target ceramic; since the eighth target ceramic is bonded to the second metal plate through the wax layer, these residual wax layers may affect the effect of further quality inspection of the eighth target ceramic, therefore, the eighth target ceramic needs to be removed from the third metal plate, and according to the preset cleaning procedure, the eighth target ceramic removed from the third metal plate is cleaned with a preset solvent to remove the wax layer remaining on the eighth target ceramic, thereby obtaining the ninth target ceramic as the target thin film ceramic.

[0069] From the above introduction, it can be seen that when thin-sheet ceramics need to be processed in batches, the method provided in the embodiment of the present application can efficiently batch-produce thin-sheet ceramics with finer thickness precision of thin plates. Specifically, thin-sheet ceramics with a thickness precision within -0.002 to 0.002 can be batch-processed. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0071] Figure 1 A flowchart of a method for processing thin ceramic sheets provided in an embodiment of the present application;

[0072] Figure 2 This is a schematic diagram of the structure of a thin-film ceramic processing device exemplified in an embodiment of the present application;

[0073] Figure 3 This is a hardware structure block diagram of a thin-film ceramic processing device disclosed in an embodiment of the present application. DETAILED DESCRIPTION

[0074] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0075] Given that most of the current thin-film ceramic processing solutions are difficult to adapt to complex and changing business needs, the applicant has studied a thin-film ceramic processing solution. When batch processing of thin-film ceramics is required, the method provided in the embodiment of the present application can efficiently batch-produce thin-film ceramics with finer thickness precision of thin plates. Specifically, thin-film ceramics with a thickness precision within -0.002 to 0.002 can be batch-processed.

[0076] The methods provided in the embodiments of the present application can be used in a variety of general-purpose or specialized computing device environments or configurations, such as personal computers, server computers, handheld or portable devices, tablet devices, multi-processor devices, and distributed computing environments including any of the above.

[0077] An embodiment of the present application provides a method for processing thin ceramic slices, which can be applied to various ceramic production management systems, and can also be applied to various computer terminals or smart terminals. The execution subject can be the processor or server of the computer terminal or smart terminal.

[0078] The following combination Figure 1 , introduces the process of the thin-film ceramic processing method given in the embodiment of this application, such as Figure 1 As shown, the process can include the following steps:

[0079] Step S101: Using wax, a ceramic blank to be processed is bonded to a first metal plate of a preset first size to obtain a first target ceramic.

[0080] Specifically, in actual application, in order to better process ceramics, ceramic blanks are generally glued to metal plates with wax for processing. First, it can fix the ceramic blanks. Sticking the ceramic blanks to be processed to the metal plate with wax can ensure that the blanks remain stable during the processing and prevent them from moving or shaking, thereby ensuring the processing accuracy and quality. In addition, this method can make the blanks more firmly attached to the metal plate, which is convenient for various processing steps, such as cutting, grinding, engraving, etc., making the processing process smoother, and to a certain extent avoiding damage or defects that may be caused by direct contact between the blanks and the processing equipment, and playing a certain protective role for the ceramic blanks.

[0081] Therefore, when the ceramic blank to be processed needs to be processed, the ceramic blank to be processed can be bonded to a first metal plate of a preset first size using wax, thereby obtaining a first target ceramic.

[0082] in,

[0083] The thickness of the wax layer between the first metal plate and the ceramic blank to be processed can be set to a preset first threshold;

[0084] The preset first size can be designed according to the ceramic processing requirements;

[0085] For example, the preset first size may be set to 150 mm in length and width respectively, and 20 mm in height, that is, 150 mm*150 mm*20 mm.

[0086] The value range of the preset first threshold can be set to [0.05mm, 0.15mm];

[0087] For example, the ceramic blank to be processed can be fixed on a first metal plate of 150mm*150mm*20mm with wax, and the wax can be evenly applied to the first metal plate, ensuring that there is wax everywhere on the first metal plate and the thickness is evenly distributed, so that the thickness of the wax layer between the ceramic blank to be processed and the first metal plate is consistent and the wax is evenly distributed, with a thickness of approximately [0.05mm, 0.15mm].

[0088] In addition, in ceramic processing, in addition to using wax to stick to the metal plate, the following fixing methods can also be used to fix the ceramic or ceramic blank to be processed:

[0089] 1. Use a fixture: A specially designed fixture can be clamped and fixed according to the shape and size of the ceramic blank.

[0090] 2. Adhesive fixation: Use suitable strong glue to fix the ceramics on a specific base or platform.

[0091] 3. Negative pressure adsorption: Use the suction force generated by negative pressure to adsorb the ceramics on the processing table.

[0092] 4. Inlay fixation: The ceramic blank is embedded into a groove or bracket with a matching shape for fixation.

[0093] Step S102 : performing preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate, and marking a first mark on the preliminary processed side to obtain a second target ceramic.

[0094] Specifically, from the above introduction, it can be seen that the method provided in the embodiment of the present application can adhere the ceramic blank to be processed to the first metal plate with wax to fix the ceramic blank to be processed. Therefore, after the ceramic blank to be processed is fixed, the side of the ceramic blank to be processed that is not adhered to the first metal plate can be preliminarily processed according to the preset first processing requirements, so that the ceramic blank to be processed can be trimmed and polished in shape first. In order to better carry out subsequent fine processing procedures, a first mark can be made on the preliminarily processed side so that the side that has been processed can be better marked, thereby obtaining a second target ceramic.

[0095] The preset first processing requirements may include the following:

[0096] The first target ceramic can be cut and trimmed according to a preset ceramic shape requirement, ensuring that the error between the actual size of the first target ceramic and the preset ceramic size is within a preset first range. Furthermore, according to a preset ceramic thickness requirement, the surface of the first target ceramic not adhering to the first metal plate is polished to ensure that the surface of the first target ceramic not adhering to the first metal plate remains flat.

[0097] in,

[0098] The preset first range can be set to [0mm, 0.01mm];

[0099] Among them, the primary processing of the ceramic blank to be processed is mainly to process the ceramic blank to be processed into the shape required by the target thin-film ceramic so that further fine processing can be carried out.

[0100] For example, the first target ceramic can be cut and trimmed according to the ceramic shape design requirements to remove excess material from the ceramic blank to be processed and ensure that the actual size of the first target ceramic is within 0.01 of the preset ceramic size. Furthermore, according to the preset ceramic thickness requirements, the side of the first target ceramic that is not adhered to the first metal plate is polished to ensure that the side of the first target ceramic that is not adhered to the first metal plate remains flat.

[0101] For example, if the preset ceramic size requirement is 0.6mm thickness, the actual measured ceramic size thickness after initial processing needs to be maintained between 0.6mm-0.61mm.

[0102] Step S103 , removing the second target ceramic from the first metal plate, and cleaning it using a preset solvent according to a preset cleaning procedure to obtain a third target ceramic.

[0103] Specifically, as can be seen from the above introduction, the method provided in the embodiment of the present application can perform preliminary processing on the first target ceramic to obtain the second target ceramic. The second target ceramic obtained after the preliminary processing has already taken shape as the designed ceramic prototype. Further, it is necessary to continue to perform fine processing on the second target ceramic. Therefore, after obtaining the second target ceramic, it is necessary to perform fine processing on it. Since the unprocessed side of the second target ceramic is adhered to the first metal plate through the wax layer, if the second target ceramic is further processed, these residual wax layers may affect the effect of further processing. Therefore, it is necessary to remove the second target ceramic from the first metal plate and clean the second target ceramic removed from the first metal plate with a preset solvent according to a preset cleaning procedure to remove the residual wax layer on the second target ceramic, thereby obtaining a third target ceramic.

[0104] Among them, the preset cleaning program may include the following:

[0105] Dewaxing and cleaning the ceramic removed from the first metal plate using a preset solvent at a preset temperature;

[0106] in,

[0107] The preset solvent may include a dewaxing agent; wherein the dewaxing agent may be used as a dewaxing agent 380 for dewaxing treatment.

[0108] The preset temperature range can be set to [40℃, 55℃], among which, when the temperature is 50 degrees Celsius, the dewaxing effect is better.

[0109] Step S104 , using wax to adhere the side of the third target ceramic with the first mark to a second metal plate of a preset second size to obtain a fourth target ceramic.

[0110] Specifically, from the above introduction, it can be seen that the method provided in the embodiment of the present application can remove the second target ceramic from the first metal plate, and according to a preset cleaning procedure, use a preset solvent to clean the second target ceramic removed from the first metal plate to remove the residual wax layer on the second target ceramic, thereby obtaining a third target ceramic.

[0111] Next, the third target ceramic needs to be further fine-processed. In order to better fine-process the third target ceramic, the third target ceramic can be adhered to a second metal plate of a preset second size with wax to obtain a fourth target ceramic.

[0112] Among them, from the above introduction, it can be seen that the side of the third target ceramic with the first mark is the side that has been preliminarily processed. Therefore, the side of the third target ceramic with the first mark can be bonded to the second metal plate. In order to better fix the third target ceramic on the second metal plate, the thickness of the wax layer between the third target ceramic and the second metal plate can be set to a preset second threshold.

[0113] The preset second size is designed according to ceramic processing requirements.

[0114] The preset second size can be set to 150mm in length and width, and 20mm in height;

[0115] The value range of the preset second threshold can be set to [0.05mm, 0.15mm].

[0116] For example, the third target ceramic can be fixed on a second metal plate of 150mm*150mm*20mm with wax, and the wax can be evenly applied to the second metal plate, ensuring that there is wax everywhere on the second metal plate and the thickness is evenly distributed, so that the wax layer between the third target ceramic and the second metal plate has the same thickness and the wax is evenly distributed, with a thickness of approximately [0.05mm, 0.15mm].

[0117] Step S105 , processing the surface of the fourth target ceramic that is not adhered to the second metal plate, and marking the processed surface with a second mark to obtain a fifth target ceramic.

[0118] Specifically, as can be seen from the above description, the method provided in the embodiment of the present application can adhere the third target ceramic to the second metal plate with wax to fix the third target ceramic and obtain the fourth target ceramic. Therefore, after the fourth target ceramic is fixed, the side of the fourth target ceramic that is not adhered to the second metal plate can be processed according to the preset second processing requirements, so that the fourth target ceramic can continue to be finely processed. In order to better carry out the subsequent fine processing steps, a first mark can be placed on the already processed side to better mark the already processed side, thereby obtaining the fifth target ceramic.

[0119] The preset second processing conditions may include the following:

[0120] The size, processing accuracy and smoothness of the fourth target ceramic can be processed according to the preset ceramic design requirements, and it can be ensured that the error between the actual size of the fourth target ceramic and the preset size is within the preset second range, the error between the actual processing accuracy of the fourth target ceramic and the preset processing accuracy is within the preset third range, and the error between the actual smoothness of the fourth target ceramic and the preset smoothness is within the preset fourth range.

[0121] in,

[0122] The second range can be set to [0.3mm, 0.6mm];

[0123] The third range can be set to [-0.002, 0.002];

[0124] The fourth range may be set to [0, 0.6].

[0125] For example, the size, processing accuracy and smoothness of the fourth target ceramic can be processed according to the preset ceramic design requirements, and it can be ensured that the actual size of the fourth target ceramic and the preset size error are within [0.3mm, 0.6mm], the actual processing accuracy of the fourth target ceramic and the preset processing accuracy error are after [-0.002, 0.002], and the actual smoothness of the fourth target ceramic and the preset smoothness error are within [0, 0.6].

[0126] For example, if the preset ceramic size requirement is 0.55mm thickness, the actual measured ceramic size thickness after fine processing needs to be maintained between 0.55mm-0.555mm.

[0127] In ceramic processing, finish primarily refers to the smoothness and glossiness of a ceramic product's surface. Specifically, smoothness reflects the flatness and roughness of the ceramic surface. A smoother surface means fewer microscopic fluctuations and a smoother feel. Glossiness reflects the surface's ability to reflect light; a high-gloss ceramic surface appears brighter and more reflective.

[0128] The smoothness of ceramic products has an important impact on their appearance, feel, and certain properties, such as their anti-pollution ability. Specific measurement methods and standards are usually used to evaluate and describe the smoothness of ceramics.

[0129] Step S106 , removing the fifth target ceramic from the second metal plate, and cleaning it using the preset solvent according to the preset cleaning procedure to obtain a sixth target ceramic.

[0130] Specifically, as can be seen from the above introduction, the method provided in the embodiment of the present application can process the fourth target ceramic to obtain the fifth target ceramic. The fifth target ceramic obtained after secondary processing is more in line with the designed ceramic requirements. Further, it is necessary to continue to fine-process the fifth target ceramic. Therefore, after obtaining the fifth target ceramic, it is necessary to continue to fine-process it. Since the side of the fifth target ceramic that has not been finely processed is adhered to the second metal plate through the wax layer, if the fifth target ceramic is continued to be fine-processed, these residual wax layers may affect the effect of further processing. Therefore, it is necessary to remove the fifth target ceramic from the second metal plate and use a preset solvent to clean the fifth target ceramic removed from the second metal plate according to a preset cleaning procedure to remove the residual wax layer on the fifth target ceramic, thereby obtaining the sixth target ceramic.

[0131] Among them, the preset cleaning program may include the following:

[0132] Dewaxing and cleaning the ceramic removed from the second metal plate using a preset solvent at a preset temperature;

[0133] in,

[0134] The preset solvent may include a dewaxing agent; wherein the dewaxing agent may be used as a dewaxing agent 380 for dewaxing treatment.

[0135] The preset temperature range can be set to [40℃, 55℃], among which, when the temperature is 50 degrees Celsius, the dewaxing effect is better.

[0136] Step S107 , using wax to adhere the side of the sixth target ceramic with the second mark to a third metal plate of a preset third size to obtain a seventh target ceramic.

[0137] Specifically, from the above introduction, it can be seen that the method provided in the embodiment of the present application can remove the fifth target ceramic from the second metal plate, and according to a preset cleaning procedure, use a preset solvent to clean the second target ceramic removed from the second metal plate to remove the residual wax layer on the fifth target ceramic, thereby obtaining the sixth target ceramic.

[0138] Next, the sixth target ceramic needs to be further fine-processed. In order to better fine-process the sixth target ceramic, the sixth target ceramic can be adhered to a third metal plate of a preset third size with wax to obtain a seventh target ceramic.

[0139] Among them, from the above introduction, it can be seen that the side of the sixth target ceramic with the second mark is the side that has undergone the first fine processing. Therefore, the side of the sixth target ceramic with the second mark can be bonded together with the third metal plate. In order to better fix the sixth target ceramic on the third metal plate, the thickness of the wax layer between the sixth target ceramic and the third metal plate can be set to a preset second threshold.

[0140] Among them, the preset third size is designed according to the ceramic processing requirements.

[0141] For example, the preset third size may be set to be 100 mm in length and width respectively, and 20 mm in height.

[0142] For example, the sixth target ceramic can be fixed on a third metal plate of 100mm*100mm*20mm with wax, and the wax can be evenly applied on the third metal plate, ensuring that there is wax everywhere on the third metal plate and the thickness is evenly distributed, so that the thickness of the wax layer between the sixth target ceramic and the third metal plate is consistent and the wax is evenly distributed, with a thickness of approximately [0.05mm, 0.15mm].

[0143] Step S108 , processing the surface of the seventh target ceramic that is not adhered to the third metal plate to obtain an eighth target ceramic.

[0144] Specifically, as described above, the method provided in the embodiments of the present application can adhere the sixth target ceramic to the third metal plate with wax to fix the sixth target ceramic, thereby obtaining the seventh target ceramic. Therefore, after the sixth target ceramic is fixed, the side of the seventh target ceramic that is not adhered to the third metal plate can be processed according to the preset third processing requirements, so that the seventh target ceramic can continue to be finely processed. In order to better perform the subsequent fine processing steps, a first mark can be placed on the already processed side to better mark the already processed side, thereby obtaining the eighth target ceramic.

[0145] The preset third processing requirements may include the following:

[0146] According to the preset ceramic design requirements, the error between the actual size of the surface of the seventh target ceramic that is not adhered to the third metal plate and the preset size can be controlled within a preset fifth range;

[0147] in,

[0148] The preset fifth range may be set to [0 mm, 0.005 mm].

[0149] For example, according to preset ceramic design requirements, the error between the actual size of the surface of the seventh target ceramic that is not adhered to the third metal plate and the preset size can be controlled within [0 mm, 0.005 mm].

[0150] If the preset ceramic size requirement is 0.5mm thickness, the actual measured ceramic size thickness after fine processing needs to be maintained between 0.55mm-0.505mm.

[0151] Step S109 , removing the eighth target ceramic from the third metal plate, and cleaning it using the preset solvent according to the preset cleaning procedure to obtain a target thin ceramic.

[0152] Specifically, as can be seen from the above introduction, the method provided in the embodiment of the present application can obtain the ninth target ceramic after primary processing and fine processing of the first target ceramic. The ninth target ceramic obtained after primary processing and fine processing already has the designed ceramic standard. Further, the ninth target ceramic needs to be sent for inspection. Since the ninth target ceramic is adhered to the third metal plate through the wax layer, these residual wax layers may affect the quality inspection effect of the ninth target ceramic. Therefore, the ninth target ceramic needs to be removed from the third metal plate and cleaned with a preset solvent according to a preset cleaning procedure to remove the residual wax layer on the ninth target ceramic, thereby obtaining the target thin-film ceramic.

[0153] Among them, the preset cleaning program may include the following:

[0154] Dewaxing and cleaning the ceramic removed from the third metal plate using a preset solvent at a preset temperature;

[0155] in,

[0156] The preset solvent may include a dewaxing agent; wherein the dewaxing agent may be used as a dewaxing agent 380 for dewaxing treatment.

[0157] The preset temperature range can be set to [40℃, 55℃], among which, when the temperature is 50 degrees Celsius, the dewaxing effect is better.

[0158] Step S110 : performing quality inspection on the target ceramic slice according to preset quality inspection requirements.

[0159] Specifically, in actual applications, in order to ensure that product quality meets standards and requirements, it is necessary to conduct quality inspections on processed thin-film ceramics. This inspection can reveal possible dimensional deviations, surface defects, insufficient strength, and other problems, thus preventing unqualified products from entering the market.

[0160] Secondly, thin-film ceramics may be used in fields with higher performance requirements. Quality inspection can verify whether they have the required physical, chemical and other properties to meet the needs of specific usage scenarios.

[0161] Furthermore, it helps maintain the company's reputation and brand image. High-quality products help enhance the company's competitiveness and credibility in the market, and quality inspection is a key link in controlling quality and establishing a good reputation.

[0162] Therefore, after the target thin-film ceramics are processed, they can be quality inspected according to preset quality inspection requirements, wherein the preset quality inspection requirements can be set according to the design requirements of the target thin-film ceramics.

[0163] Step S111 : judging whether the target thin-film ceramic is qualified according to the quality inspection result of the target thin-film ceramic.

[0164] Specifically, as can be seen from the above description, the method provided in the embodiments of the present application can perform a quality inspection on a target thin ceramic sheet. Furthermore, based on the quality inspection results of the target thin ceramic sheet, it can be determined whether the target thin ceramic sheet is qualified. If the target thin ceramic sheet passes the quality inspection, step S112 can be executed; if the target thin ceramic sheet fails the quality inspection, step S113 can be executed.

[0165] Step S112: Determine whether the processing of the target ceramic slice is completed.

[0166] Specifically, from the above introduction, it can be seen that the method provided in the embodiment of the present application can judge whether the target thin film ceramics are qualified based on the quality inspection results of the target thin film ceramics. If it is determined that the target thin film quality inspection is qualified, it means that the processed target thin film ceramics can be put into use without the need for reprocessing, and it can be determined that the processing of the target thin film ceramics is completed.

[0167] Step S113: starting a reprocessing procedure for the target ceramic slice.

[0168] Specifically, from the above introduction, it can be seen that the method provided in the embodiment of the present application can determine whether the target thin film ceramics are qualified based on the quality inspection results of the target thin film ceramics. If it is determined that the target thin film quality inspection is unqualified, it means that the processed target thin film ceramics cannot be put into use and needs to be reprocessed, then the reprocessing procedure for the target thin film ceramics can be started.

[0169] Furthermore, the method provided in the embodiment of the present application can also determine the qualified rate and defective rate of each ceramic production batch through a reprocessing procedure.

[0170] For example, in actual applications, experiments have shown that the method provided in the embodiments of this application can be used to process thin ceramic sheets, achieving efficient mass production of ceramic sheets with a length and width of 13mm*13mm, a thickness of 0.3mm-0.6mm, and an accuracy within -0.002 to +0.002, with a single machine capacity of 48,000 pieces in 8 hours. Existing baffle technology cannot guarantee this accuracy, and the single machine capacity is less than 2,000 pieces. Therefore, the method provided in the embodiments of this application can effectively improve the production efficiency of thin ceramic sheets with finer thickness accuracy.

[0171] It can be seen from the technical solutions introduced above that the method provided in the embodiments of the present application can efficiently mass-produce thin-plate ceramics with finer thickness accuracy.

[0172] The following describes a thin-film ceramic processing device provided in an embodiment of the present application. The thin-film ceramic processing device described below and the thin-film ceramic processing method described above can be referenced to each other.

[0173] See also Figure 2 , Figure 2 This is a schematic structural diagram of a thin-film ceramic processing device disclosed in an embodiment of the present application.

[0174] like Figure 2 As shown, the thin-film ceramic processing device may include:

[0175] The first processing unit 101 is used to bond the ceramic blank to be processed onto a first metal plate of a preset first size using wax to obtain a first target ceramic;

[0176] The first processing unit 102 is used to perform preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate, and mark the preliminary processed side with a first mark to obtain a second target ceramic;

[0177] a first cleaning unit 103, configured to remove the second target ceramic from the first metal plate and clean it using a preset solvent according to a preset cleaning procedure to obtain a third target ceramic;

[0178] A second processing unit 104 is configured to adhere the side of the third target ceramic having the first mark to a second metal plate of a preset second size using wax to obtain a fourth target ceramic;

[0179] A second processing unit 105 is used to process the side of the fourth target ceramic that is not adhered to the second metal plate and mark the processed side with a second mark to obtain a fifth target ceramic;

[0180] a second cleaning unit 106 for removing the fifth target ceramic from the second metal plate and cleaning it using the preset solvent according to the preset cleaning procedure to obtain a sixth target ceramic;

[0181] A third processing unit 107 is configured to adhere the side of the sixth target ceramic having the second mark to a third metal plate of a preset third size using wax to obtain a seventh target ceramic;

[0182] a third processing unit 108 for processing a surface of the seventh target ceramic that is not adhered to the third metal plate to obtain an eighth target ceramic;

[0183] The third cleaning unit 109 is used to remove the eighth target ceramic from the third metal plate and clean it using the preset solvent according to the preset cleaning procedure to obtain a target thin ceramic.

[0184] It can be seen from the technical solution introduced above that when thin-film ceramics need to be processed, the device provided in the embodiment of the present application can use wax to bond the ceramic blank to be processed to a first metal plate of a preset first size, thereby obtaining a first target ceramic. The first target ceramic is the ceramic to be processed, wherein, in order to ensure that the processed ceramic can meet the preset design requirements, the thickness of the wax layer between the first metal plate and the ceramic blank to be processed can be a preset first threshold; so that the blank to be processed and the first metal plate can be more tightly bonded to avoid the ceramic blank to be processed from loosening during the processing process and being unable to be processed smoothly; therefore, after the ceramic blank to be processed is fixed on the first metal plate, the side of the ceramic blank to be processed that is not bonded to the first metal plate can be preliminarily processed according to the preset first processing requirements, and a first mark can be marked on the preliminarily processed side, thereby obtaining a second target ceramic; wherein, the preliminarily processing of the ceramic blank to be processed this time is mainly to process the ceramic blank to be processed into the shape required by the target thin-film ceramic so that further fine processing can be performed.

[0185] Therefore, after preliminary processing of the side of the ceramic blank to be processed that is not adhered to the first metal plate, the second target ceramic can be further removed from the first metal plate. Since the unprocessed side of the second target ceramic is adhered to the first metal plate through the wax layer, if the second target ceramic continues to be fine-processed, these residual wax layers may affect the effect of further processing. Therefore, it is necessary to clean the second target ceramic removed from the first metal plate according to the preset cleaning procedure and use a preset solvent to remove the wax layer remaining on the second target ceramic, thereby obtaining the third target ceramic.

[0186] The third target ceramic is further bonded to the second metal plate of a preset second size using wax so as to perform fine processing on the third target ceramic, thereby obtaining a fourth target ceramic. Since the side of the third target ceramic with the first mark is the side that has been preliminarily processed, the side of the third target ceramic with the first mark can be bonded to the second metal plate to process the other side of the third target ceramic. In order to better fix the third target ceramic to the second metal plate, the thickness of the wax layer between the third target ceramic and the second metal plate can be set to a preset second threshold value. Then, according to the preset second processing requirement, the side of the fourth target ceramic that is not bonded to the second metal plate can be processed, and the second mark can be marked on the processed side to obtain a fifth target ceramic. Since the unprocessed side of the fifth target ceramic is bonded to the second metal plate through the wax layer, if the fifth target ceramic is further fine-processed, the residual wax layer may affect the effect of further processing. Therefore, the fifth target ceramic needs to be removed from the second metal plate and cleaned with a preset solvent according to a preset cleaning procedure to remove the wax layer remaining on the fifth target ceramic, thereby obtaining a sixth target ceramic.

[0187] Use wax to continue to adhere the sixth target ceramic to the third metal plate of a preset third size, so that the sixth target ceramic can continue to be fine-processed, thereby obtaining the seventh target ceramic, wherein, since the side of the sixth target ceramic with the second mark has been fine-processed, the side of the sixth target ceramic with the second mark can be adhered to the third metal plate, wherein, in order to better fix the third target ceramic and the second metal plate, the thickness of the wax layer between the third metal plate and the sixth target ceramic can be set to a preset first threshold; and according to the preset third processing requirement, the side of the seventh target ceramic that is not adhered to the third metal plate is processed, thereby obtaining the eighth target ceramic; since the eighth target ceramic is adhered to the second metal plate through the wax layer, these residual wax layers may affect the effect of further quality inspection of the eighth target ceramic, therefore, the eighth target ceramic needs to be removed from the third metal plate, and according to the preset cleaning procedure, the eighth target ceramic removed from the third metal plate is cleaned with a preset solvent to remove the wax layer remaining on the eighth target ceramic, thereby obtaining the ninth target ceramic as the target thin film ceramic.

[0188] From the above introduction, it can be seen that when thin-sheet ceramics need to be processed in batches, the device provided in the embodiment of the present application can efficiently batch-produce thin-sheet ceramics with finer thickness precision of thin plates. Specifically, thin-sheet ceramics with a thickness precision within -0.002 to 0.002 can be batch-processed.

[0189] Among them, the specific processing flow of each unit included in the above-mentioned thin-film ceramic processing device can refer to the relevant introduction of the thin-film ceramic processing method part above, and will not be repeated here.

[0190] The thin-film ceramic processing device provided in the embodiment of the present application can be applied to thin-film ceramic processing equipment, such as terminals: mobile phones, computers, etc. Optionally, Figure 3 The hardware structure diagram of the thin-film ceramic processing equipment is shown. Figure 3 The hardware structure of the thin-film ceramic processing equipment may include: at least one processor 1, at least one communication interface 2, at least one memory 3 and at least one communication bus 4.

[0191] In an embodiment of the present application, the number of processor 1 , communication interface 2 , memory 3 , and communication bus 4 is at least one, and the processor 1 , communication interface 2 , and memory 3 communicate with each other through the communication bus 4 .

[0192] The processor 1 may be a central processing unit (CPU), or an application-specific integrated circuit (ASIC), or one or more integrated circuits configured to implement the embodiments of the present application;

[0193] The memory 3 may include a high-speed RAM memory, and may also include a non-volatile memory, such as at least one disk memory;

[0194] The memory stores a program, and the processor can call the program stored in the memory, wherein the program is used to implement each processing flow in the aforementioned terminal thin-film ceramic processing solution.

[0195] An embodiment of the present application further provides a readable storage medium, which can store a program suitable for execution by a processor, wherein the program is used to implement various processing flows of the aforementioned terminal in the thin-film ceramic processing solution.

[0196] Finally, it should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or device. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of additional identical elements in the process, method, article, or device comprising the element.

[0197] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0198] The above description of the disclosed embodiments is intended to enable those skilled in the art to implement or use the present application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. The various embodiments may be combined with one another. Therefore, the present application is not limited to the embodiments shown herein, but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for processing thin ceramic sheets, characterized in that: include: Using wax to bond the ceramic blank to be processed onto a first metal plate of a preset first size to obtain a first target ceramic; Performing preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate, and marking a first mark on the preliminary processed side to obtain a second target ceramic; The second target ceramic is removed from the first metal plate, and is cleaned using a preset solvent according to a preset cleaning procedure to obtain a third target ceramic; Using wax to adhere the side of the third target ceramic with the first mark to a second metal plate of a preset second size to obtain a fourth target ceramic; Processing a side of the fourth target ceramic that is not adhered to the second metal plate, and marking the processed side with a second mark to obtain a fifth target ceramic; The fifth target ceramic is removed from the second metal plate, and cleaned using the preset solvent according to the preset cleaning procedure to obtain a sixth target ceramic; Using wax to adhere the side of the sixth target ceramic having the second mark to a third metal plate of a preset third size to obtain a seventh target ceramic; Processing the side of the seventh target ceramic that is not adhered to the third metal plate to obtain an eighth target ceramic; The eighth target ceramic is removed from the third metal plate, and is cleaned using the preset solvent according to the preset cleaning procedure to obtain a target thin-sheet ceramic.

2. The method according to claim 1, characterized in that The method further includes: According to the preset quality inspection requirements, the target thin ceramic sheet is quality inspected; Determining whether the target thin-film ceramic is qualified according to the quality inspection result of the target thin-film ceramic; If the target thin-film ceramic passes the quality inspection, it is determined that the processing of the target thin-film ceramic is completed; If the target thin-film ceramic fails the quality inspection, a reprocessing procedure for the target thin-film ceramic is initiated.

3. The method according to claim 1, characterized in that The preliminary processing of the side of the ceramic blank to be processed that is not adhered to the first metal plate comprises: According to a preset first processing requirement, performing preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate; The preset first processing requirement includes the following: According to the preset ceramic shape requirement, the first target ceramic is cut and trimmed, and it is ensured that the error between the actual size of the first target ceramic and the preset ceramic size is within a preset first range, wherein the preset first range is set to [0 mm, 0.01 mm]; According to the preset ceramic thickness requirement, the side of the first target ceramic that is not adhered to the first metal plate is polished, and it is ensured that the side of the first target ceramic that is not adhered to the first metal plate remains flat.

4. The method according to claim 1, characterized in that: The processing of the side of the fourth target ceramic that is not adhered to the second metal plate comprises: According to a preset second processing requirement, processing a side of the fourth target ceramic that is not adhered to the second metal plate; Among them, the preset second processing requirements include the following: According to the preset ceramic design requirements, the size, processing accuracy and smoothness of the fourth target ceramic are processed, and it is ensured that the error between the actual size of the fourth target ceramic and the preset size is within a preset second range, the error between the actual processing accuracy of the fourth target ceramic and the preset processing accuracy is within a preset third range, and the error between the actual smoothness of the fourth target ceramic and the preset smoothness is within a preset fourth range; Wherein, the second range is set to [0.3mm, 0.6mm]; The third range is set to [-0.002, 0.002]; The fourth range is set to [0, 0.6].

5. The method according to claim 1, characterized in that The processing of the side of the seventh target ceramic that is not adhered to the third metal plate comprises: According to a preset third processing requirement, processing is performed on a side of the seventh target ceramic that is not adhered to the third metal plate; The preset third processing requirements include the following: According to the preset ceramic design requirements, the error between the actual size of the side of the seventh target ceramic that is not adhered to the third metal plate and the preset size is controlled within a preset fifth range; Wherein, the preset fifth range is set to [0mm, 0.005mm].

6. The method according to claim 1, characterized in that The wax layer thickness between the first metal plate and the ceramic blank to be processed is a preset first threshold value, and the preset first size is designed according to the ceramic processing requirements; The thickness of the wax layer between the third target ceramic and the second metal plate is a preset second threshold value, and the preset second size is designed according to ceramic processing requirements; The thickness of the wax layer between the third metal plate and the sixth target ceramic is a preset first threshold, and the preset third size is designed according to ceramic processing requirements.

7. The method according to claim 6, characterized in that The preset first size is set to be 150 mm in length and width respectively, and 20 mm in height; The preset second size is set to be 150 mm in length and width respectively, and 20 mm in height; The preset third size is set to be 100 mm in length and width respectively, and 20 mm in height; The value range of the preset first threshold is set to [0.05mm, 0.15mm]; The value range of the preset second threshold is set to [0.05mm, 0.15mm].

8. The method according to claim 1, characterized in that The preset cleaning program includes: Dewaxing and cleaning the ceramic removed from the metal plate using a preset solvent at a preset temperature; in, The preset solvent includes a dewaxing agent; The preset temperature range is set to [40° C., 55° C.].

9. A thin-film ceramic processing device, characterized in that: include: A first processing unit is used to bond the ceramic blank to be processed onto a first metal plate of a preset first size by using wax to obtain a first target ceramic; A first processing unit is used to perform preliminary processing on a side of the ceramic blank to be processed that is not adhered to the first metal plate, and mark the preliminary processed side with a first mark to obtain a second target ceramic; A first cleaning unit is used to remove the second target ceramic from the first metal plate and clean it using a preset solvent according to a preset cleaning procedure to obtain a third target ceramic; a second processing unit, for bonding the side of the third target ceramic having the first mark to a second metal plate of a preset second size using wax to obtain a fourth target ceramic; A second processing unit is used to process the side of the fourth target ceramic that is not adhered to the second metal plate, and mark the processed side with a second mark to obtain a fifth target ceramic; a second cleaning unit, used to remove the fifth target ceramic from the second metal plate, and clean it using the preset solvent according to the preset cleaning procedure to obtain a sixth target ceramic; a third processing unit, configured to adhere the side of the sixth target ceramic having the second mark to a third metal plate of a preset third size using wax to obtain a seventh target ceramic; a third processing unit, configured to process a side of the seventh target ceramic that is not adhered to the third metal plate to obtain an eighth target ceramic; The third cleaning unit is used to remove the eighth target ceramic from the third metal plate and clean it using the preset solvent according to the preset cleaning procedure to obtain a target thin ceramic.

10. A thin-film ceramic processing device, characterized in that: include: one or more processors, and memory; The memory stores computer-readable instructions, and when the computer-readable instructions are executed by the one or more processors, the steps of the thin-film ceramic processing method according to any one of claims 1 to 8 are implemented.

11. A readable storage medium, characterized in that: The readable storage medium stores computer-readable instructions, and when the computer-readable instructions are executed by one or more processors, the one or more processors implement the steps of the thin-film ceramic processing method as described in any one of claims 1 to 8.