Graphene / carbon nanomaterial modified carbon fiber battery felt process

Through the modification of the carbon fiber battery felt process of graphene/carbon nanomaterials, the problems of low tensile strength of carbon fiber monofilament and poor interfacial bonding force are solved, the interface shear strength is significantly improved, and the overall performance of carbon fiber composite materials is enhanced.

CN118457012BActive Publication Date: 2024-11-26烟台奥森制动材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410912421.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-26
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The tensile strength of carbon fiber monofilament is low and the interface bonding force is poor, which affects the performance of carbon fiber composite materials.

Method used

The carbon fiber battery felt process is modified by graphene/carbon nanomaterials. The specific steps include uniformly applying phenolic resin on the carbon fiber, performing electrochemical deposition and radio frequency plasma treatment, introducing ferrocene and benzoxazole groups, and enhancing carbon fiber and phenolic acids and enhancement of carbon fiber and phenolic acid Chemical and physical interactions of resins.

Benefits of technology

It significantly improves the interface shear strength, enhances the bonding force between carbon fiber and matrix material, and improves the overall performance of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a graphene / carbon nano material modified carbon fiber battery felt process, and belongs to the technical field of carbon fiber composite materials. The invention uniformly applies phenolic resin on graphene / carbon nano material modified carbon fiber, repeats the steps to obtain 5-7 layers of fiber cloth, stacks the 5-7 layers of fiber cloth up and down, and hot presses and cures them at 200-240°C for 60-100 minutes to obtain graphene / carbon nano material modified carbon fiber battery felt; the strong chemical bonds and physical adsorption formed between the modified carbon fiber surface and the phenolic resin of the invention enable the composite material to transfer stress more effectively when subjected to external force, thereby significantly improving the interface shear strength, which is much higher than that of the unmodified carbon fiber composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber composite materials, in particular to a process for modifying carbon fiber battery felt with graphene / carbon nano materials. Background Art

[0002] Carbon fiber has excellent properties such as high strength, high modulus and light weight, and is widely used to reinforce matrix materials. The interface between carbon fiber and matrix acts as a link to connect carbon fiber and matrix material, and the interface bonding strength directly determines the performance of carbon fiber composite materials. When external forces are applied to carbon fiber composite materials, the stress inside the matrix material can be dispersed and transferred to the carbon fiber, thereby reducing the probability of stress concentration inside the composite material.

[0003] The patent application with publication number CN116770584A discloses graphene oxide modified carbon fiber and its preparation and application, composite material with interface photothermal self-repairing function and its preparation method. Graphene oxide and Diels-Alder structure are simultaneously introduced to the surface of carbon fiber by chemical grafting method, the photothermal effect of graphene oxide is repeatedly utilized, the surface of modified carbon fiber is heated up under near-infrared light irradiation, and the thermal reversible reaction of Diels-Alder structure is induced, thereby realizing multiple repairs of the interface of carbon fiber composite material.

[0004] The patent with the authorization announcement number CN114032672B discloses a carbon fiber modified with controllable reduction of graphene oxide and its use. By reducing graphene oxide in an alkaline solution by heat treatment to reduce its non-carboxyl oxygen content, the obtained graphene oxide can be combined with carbon fiber to form a special microstructure of "dragon fruit skin". This microstructure is conducive to the increase of carbon fiber surface roughness and the transfer of interface load, and can improve the wettability of carbon fiber and resin matrix, thereby enhancing the bonding performance of carbon fiber and resin matrix.

[0005] The patent application with publication number CN103569997A discloses a method for preparing graphene-modified flexible and braided carbon nanofibers. First, graphene oxide is put into a container containing DMF to obtain a saturated solution of upper brown-yellow graphene oxide, and then polyacrylonitrile polymer is dissolved in DMF to obtain a transparent polymer solution. The saturated solution of graphene oxide and the polymer solution are mixed to obtain a precursor solution, and graphene oxide-modified polyacrylonitrile fibers are obtained by electrospinning technology or melt spinning technology. The fibers are dried and stabilized, and finally the dried polyacrylonitrile fibers are carbonized in an inert gas atmosphere or under vacuum conditions to form carbon nanofibers.

[0006] However, the carbon fiber monofilaments prepared by the above patents and prior art have low tensile strength and poor interfacial bonding strength of the carbon fiber. Summary of the invention

[0007] The purpose of the present invention is to provide a graphene / carbon nanomaterial modified carbon fiber battery felt process to solve the current problems of low tensile strength of carbon fiber monofilaments and poor interface bonding strength of carbon fibers.

[0008] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0009] The process of graphene / carbon nanomaterial modified carbon fiber battery felt has the following operating steps:

[0010] The phenolic resin is evenly applied on the graphene / carbon nanomaterial modified carbon fiber, and the steps are repeated to obtain 5-7 layers of fiber cloth, and the 5-7 layers of fiber cloth are stacked up and down, and hot-pressed and cured at 200-240°C for 60-100 minutes to obtain graphene / carbon nanomaterial modified carbon fiber battery felt.

[0011] Furthermore, the preparation method of the graphene / carbon nanomaterial modified carbon fiber is:

[0012] S1: adding 10-15 parts of carbon nanotubes and 10-15 parts of thiolated graphene to 280-400 parts of ethanol aqueous solution, stirring for 30-60 minutes, to obtain a CNTs / GR dispersion;

[0013] S2: Add the CNTs / GR dispersion into an electrodeposition reaction tank, with the anode being carbon fiber and the cathode being platinum, and perform electrochemical deposition, then add 0.07-0.5 parts of vinyl ferrocene, 0.01-0.05 parts of benzothiazole-2-thiol, and 0.01-0.05 parts of potassium ethoxide, mix and immerse for 100-200 minutes to obtain oxazole-modified carbon fiber;

[0014] S3: Place the oxazole-modified carbon fiber in a radio frequency plasma generator, at a power of 100-200 W, introduce argon and ammonia in a volume ratio of 1: (0.3-0.7); the gas flow rate is 10-20 mL / min, and use a radio frequency of 13.56 MHz glow plasma for 10-30 minutes to obtain graphene / carbon nanomaterial modified carbon fiber.

[0015] Furthermore, the mass concentration of the ethanol aqueous solution is 60-70%.

[0016] Furthermore, the stirring speed is 500-800r / min.

[0017] Furthermore, the voltage of the electrochemical deposition is 5-10V.

[0018] Furthermore, the deposition time is 10-20 minutes.

[0019] The beneficial effects of the present invention are:

[0020] 1. Enhanced interfacial interaction: By grafting ferrocene and benzoxazole groups on the surface of carbon fiber, the chemical and physical interaction points between carbon fiber and phenolic resin are increased; the introduction of ferrocene groups, with their unique electronic properties and spatial structure, provides additional π-π interactions, while benzoxazole groups enhance the interaction through hydrogen bonds and van der Waals forces, thereby significantly improving the bonding strength of the interface.

[0021] 2. Improved interface shear strength: The strong chemical bonds and physical adsorption formed between the modified carbon fiber surface and the phenolic resin enable the composite material to transfer stress more effectively when subjected to external force, thereby significantly improving the interface shear strength to 88.1MPa, which is much higher than that of the unmodified carbon fiber composite material. DETAILED DESCRIPTION

[0022] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0023] Example test method:

[0024] 1. Single filament tensile strength: Tested in accordance with GB / T31290-2014;

[0025] 2. Interface shear strength: tested by micro-droplet debonding method.

[0026] Example 1: The preparation method of graphene / carbon nanomaterial modified carbon fiber is:

[0027] S1: Add 10 g of carbon nanotubes and 10 g of thiolated graphene into 280 g of ethanol aqueous solution and stir for 30 min to obtain a CNTs / GR dispersion;

[0028] S2: Add the CNTs / GR dispersion into an electrodeposition reaction tank, with the anode being carbon fiber and the cathode being platinum, and perform electrochemical deposition. Then, add 0.07 g of vinyl ferrocene, 0.01 g of benzothiazole-2-thiol, and 0.01 g of potassium ethoxide, mix and immerse for 100 min to obtain oxazole-modified carbon fiber.

[0029] S3: Place the oxazole-modified carbon fiber in a radio frequency plasma generator, at a power of 100 W, introduce argon and ammonia in a volume ratio of 1:0.3; the gas flow rate is 10 mL / min, and use a radio frequency of 13.56 MHz glow plasma for 10 minutes to obtain graphene / carbon nanomaterial modified carbon fiber.

[0030] The mass concentration of the ethanol aqueous solution is 60%.

[0031] The stirring speed is 500r / min.

[0032] The voltage of the electrochemical deposition is 5V.

[0033] The deposition time is 10 min.

[0034] The phenolic resin is evenly applied on the graphene / carbon nanomaterial modified carbon fiber, and the steps are repeated to obtain 5 layers of fiber cloth. The 5 layers of fiber cloth are stacked up and down, and hot-pressed and cured at 200°C for 60 minutes to obtain graphene / carbon nanomaterial modified carbon fiber battery felt.

[0035] Example 2: The preparation method of graphene / carbon nanomaterial modified carbon fiber is:

[0036] S1: Add 12 g of carbon nanotubes and 12 g of thiolated graphene into 320 g of ethanol aqueous solution and stir for 40 min to obtain a CNTs / GR dispersion;

[0037] S2: Add the CNTs / GR dispersion into an electrodeposition reaction tank, with the anode being carbon fiber and the cathode being platinum, and perform electrochemical deposition. Then, add 0.2 g of vinyl ferrocene, 0.02 g of benzothiazole-2-thiol, and 0.02 g of potassium ethoxide, mix and immerse for 130 min to obtain oxazole-modified carbon fiber.

[0038] S3: The oxazole-modified carbon fiber is placed in a radio frequency plasma generator, and at a power of 140 W, argon and ammonia are introduced in a volume ratio of 1:0.4; the gas flow rate is 13 mL / min, and the radio frequency is 13.56 MHz glow plasma for 15 minutes to obtain graphene / carbon nanomaterial modified carbon fiber.

[0039] The mass concentration of the ethanol aqueous solution is 65%.

[0040] The stirring speed is 600r / min.

[0041] The voltage of the electrochemical deposition is 6V.

[0042] The deposition time is 15 minutes.

[0043] The phenolic resin is evenly applied on the graphene / carbon nanomaterial modified carbon fiber, and the steps are repeated to obtain 6 layers of fiber cloth. The 6 layers of fiber cloth are stacked up and down, and hot-pressed and cured at 210°C for 70 minutes to obtain graphene / carbon nanomaterial modified carbon fiber battery felt.

[0044] Example 3: The preparation method of graphene / carbon nanomaterial modified carbon fiber is:

[0045] S1: Add 14 g of carbon nanotubes and 14 g of thiolated graphene into 380 g of ethanol aqueous solution and stir for 50 min to obtain a CNTs / GR dispersion;

[0046] S2: Add the CNTs / GR dispersion into an electrodeposition reaction tank, with the anode being carbon fiber and the cathode being platinum, and perform electrochemical deposition. Then, add 0.4 g of vinyl ferrocene, 0.04 g of benzothiazole-2-thiol, and 0.04 g of potassium ethoxide, and mix and immerse for 180 min to obtain oxazole-modified carbon fiber.

[0047] S3: The oxazole-modified carbon fiber is placed in a radio frequency plasma generator, at a power of 180 W, argon and ammonia are introduced in a volume ratio of 1:0.6; the gas flow rate is 18 mL / min, and the radio frequency is 13.56 MHz glow plasma treatment for 25 minutes to obtain graphene / carbon nanomaterial modified carbon fiber.

[0048] The mass concentration of the ethanol aqueous solution is 65%.

[0049] The stirring speed is 700r / min.

[0050] The voltage of the electrochemical deposition is 8V.

[0051] The deposition time is 15 minutes.

[0052] The phenolic resin is evenly applied on the graphene / carbon nanomaterial modified carbon fiber, and the steps are repeated to obtain 6 layers of fiber cloth. The 6 layers of fiber cloth are stacked up and down, and hot-pressed and cured at 230°C for 80 minutes to obtain graphene / carbon nanomaterial modified carbon fiber battery felt.

[0053] Example 4: The preparation method of graphene / carbon nanomaterial modified carbon fiber is:

[0054] S1: Add 15 g of carbon nanotubes and 15 g of thiolated graphene into 400 g of ethanol aqueous solution and stir for 60 min to obtain a CNTs / GR dispersion;

[0055] S2: Add the CNTs / GR dispersion into an electrodeposition reaction tank, with the anode being carbon fiber and the cathode being platinum, and perform electrochemical deposition. Then, add 0.5 g of vinyl ferrocene, 0.05 g of benzothiazole-2-thiol, and 0.05 g of potassium ethoxide, mix and immerse for 200 min to obtain oxazole-modified carbon fiber.

[0056] S3: The oxazole-modified carbon fiber is placed in a radio frequency plasma generator, and argon and ammonia are introduced at a volume ratio of 1:0.7 at a power of 200 W; the gas flow rate is 20 mL / min, and the radio frequency is 13.56 MHz glow plasma for 30 minutes to obtain graphene / carbon nanomaterial modified carbon fiber.

[0057] The mass concentration of the ethanol aqueous solution is 70%.

[0058] The stirring speed is 800r / min.

[0059] The voltage of the electrochemical deposition is 10V.

[0060] The deposition time is 20 minutes.

[0061] The phenolic resin is evenly applied on the graphene / carbon nanomaterial modified carbon fiber, and the steps are repeated to obtain 7 layers of fiber cloth. The 7 layers of fiber cloth are stacked up and down, and hot-pressed and cured at 240°C for 100 minutes to obtain graphene / carbon nanomaterial modified carbon fiber battery felt.

[0062] Comparative Example 1: Based on Example 1, but without the treatment method of S3, the rest is the same as Example 1.

[0063] Comparative Example 2: Based on Example 1, but without adding benzothiol-2-thiol, the other steps are the same as Example 1.

[0064] Comparative Example 3: Based on Example 1, but without adding vinylferrocene, the other steps are the same as Example 1.

[0065] Table 1: Test results of various embodiments and comparative examples

[0066]

[0067] Through the data analysis of the above embodiments and comparative examples, the present invention significantly improves the interface shear strength, which is much higher than that of unmodified carbon fiber composite materials.

[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Graphene / carbon nanomaterial modified carbon fiber battery felt process, characterized by: The operation steps are: The phenolic resin is evenly applied on the graphene / carbon nanomaterial modified carbon fiber, and the steps are repeated to obtain 5-7 layers of fiber cloth, and the 5-7 layers of fiber cloth are stacked up and down, and hot-pressed and cured at 200-240° C. for 60-100 minutes to obtain a graphene / carbon nanomaterial modified carbon fiber battery felt. The preparation method of the graphene / carbon nanomaterial modified carbon fiber is as follows: S1: adding 10-15 parts of carbon nanotubes and 10-15 parts of thiolated graphene to 280-400 parts of ethanol aqueous solution, stirring for 30-60 minutes to obtain a CNTs / GR dispersion; S2: Add the CNTs / GR dispersion into an electrodeposition reaction tank, with the anode being carbon fiber and the cathode being platinum, and perform electrochemical deposition, then add 0.07-0.5 parts of vinyl ferrocene, 0.01-0.05 parts of benzothiazole-2-thiol, and 0.01-0.05 parts of potassium ethoxide, mix and immerse for 100-200 minutes to obtain oxazole-modified carbon fiber; S3: Place the oxazole-modified carbon fiber in a radio frequency plasma generator, at a power of 100-200 W, introduce argon and ammonia in a volume ratio of 1: (0.3-0.7); the gas flow rate is 10-20 mL / min, and use a radio frequency of 13.56 MHz glow plasma for 10-30 minutes to obtain graphene / carbon nanomaterial modified carbon fiber.

2. The process for preparing graphene / carbon nanomaterial-modified carbon fiber battery felt according to claim 1, characterized in that: The mass concentration of the ethanol aqueous solution is 60-70%.

3. The process for modifying carbon fiber battery felt with graphene / carbon nanomaterials according to claim 2, characterized in that: The stirring speed is 500-800r / min.

4. The process for preparing graphene / carbon nanomaterial-modified carbon fiber battery felt according to claim 2, characterized in that: The voltage of the electrochemical deposition is 5-10V.

5. The process for modifying carbon fiber battery felt with graphene / carbon nanomaterials according to claim 2, characterized in that: The electrochemical deposition time is 10-20 minutes.