Single-walled carbon nanotube functional film and preparation method thereof
Through floating chemical vapor deposition and transfer printing technology, combined with nanoparticles and conductive silver paste electrodes, the problem of structural destruction and functional combination of single-walled carbon nanotube films during the preparation process was solved, and a high-performance flexible conductive film with electrothermal properties was achieved. Defogging, infrared insulation and UV protection.
Patent Information
- Application Number
- CN202410323829.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-21
AI Technical Summary
In the existing technology, single-walled carbon nanotube films are susceptible to structural damage in the dispersion process and dispersant residues during the preparation process, resulting in poor electrical conductivity and difficulty in effectively combining with other functional components to achieve multifunctionality.
The floating chemical vapor deposition method is used to dissolve and disperse nanoparticles with infrared absorption blocking properties, organic metal catalysts and co-catalysts to prepare a film growth precursor solution. Carbon nanotubes are grown in a tube furnace and transferred to a flexible and transparent substrate, combined with conductive The silver paste electrode and encapsulation layer form an overall functional film.
Significantly improves the conductivity, flexibility and light transmittance properties of the carbon nanotube film, achieving the versatility of flexibility, electric heating, UV blocking and infrared blocking, and is suitable for smart energy-saving windows.
Smart Images

Figure CN118458751B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material film preparation, and specifically provides a single-wall carbon nanotube functional film and a preparation method thereof. Background Art
[0002] Smart energy-saving windows achieve heat insulation by blocking infrared rays. As people's requirements for quality of life increase, they have more functional requirements, such as defogging, self-cleaning, and UV protection. Currently, there are many defogging methods, such as electric defogging, super hydrophilic defogging, and super hydrophobic defogging. Among them, electric defogging is an active defogging method that is not affected by the external environment and can achieve long-term stable defogging. Compared with the passive defogging method of super hydrophilic or super hydrophobic coatings, which are easily affected by dust and dirt in the air, electric active defogging has better reliability.
[0003] The exploration of combining electric heating defogger with infrared heat insulation function mainly involves directly combining electric heating materials with infrared blocking coatings. Commonly used electric heating layers can be made of ITO conductive glass, patterned metal electrode electrodes, transparent films of nano silver wires, etc. However, due to their brittleness, easy oxidation, and single function, flexible multifunctional functional films all have more or less deficiencies.
[0004] Single-walled carbon nanotubes have the most superior comprehensive properties. They are the most excellent technical solution for flexible conductive films, combining conductivity, flexibility, huge aspect ratio and ultra-low conductivity threshold. However, most of the existing technologies use single-walled carbon nanotubes as conductive fillers, which are dispersed and then coated to make transparent conductive films. The destruction of their structure during the dispersion process and the residual dispersant after film formation seriously affect their conductive properties.
[0005] The floating chemical vapor deposition single-walled carbon nanotube dry film forming technology forms a film directly after the carbon nanotubes grow, without the need for dispersion and dispersants. The film shows excellent comprehensive properties and is an ideal flexible transparent conductive film. However, the practical difficulties of continuous collection, transfer, adhesion improvement, and surface functionalization of in-situ grown carbon nanotube films have made it a challenging research task to give full play to the excellent performance of the single-walled carbon nanotube film and combine it with other functional components. Summary of the invention
[0006] In view of the above problems, the present invention provides the following technical solutions:
[0007] A method for preparing a single-walled carbon nanotube functional film, wherein nanoparticles having infrared absorption and blocking properties, an organic metal catalyst, and a co-catalyst are dissolved and dispersed in an organic solvent to prepare a film growth precursor solution;
[0008] Subsequently, the thin film growth precursor is injected into a tube furnace to grow single-walled carbon nanotubes using a floating chemical vapor deposition method. The product is uniformly deposited on the surface of the porous filter membrane at the outlet of the tube furnace and then transferred to the surface of the flexible transparent substrate.
[0009] The electrodes are printed on the surface of the flexible transparent substrate after transfer, and finally bonded to the encapsulation layer to form a whole.
[0010] Furthermore, the implementation process of the method includes the following steps:
[0011] S1) dissolving an organic metal catalyst and a co-catalyst in an organic solvent, then adding nanoparticles having infrared absorption and blocking properties thereto, and ultrasonically dispersing the nanoparticles to obtain a stable precursor solution for thin film growth;
[0012] S2) heating the tube furnace to raise the temperature, introducing the carrier gas, and then injecting the precursor solution into the tube furnace through the injection pump, and spraying it into the high temperature zone through ultrasonic atomization to react;
[0013] S3) At the outlet of the tube furnace, the grown carbon nanotube products are uniformly deposited on the porous filter membrane under the action of negative pressure suction to form a carbon nanotube composite film;
[0014] S4) transferring the carbon nanotube composite film on the filter membrane to the surface of the flexible transparent substrate by pressure transfer;
[0015] S5) printing conductive silver paste electrodes on both ends of the carbon nanotube film by screen printing and covering them with copper foil current collectors;
[0016] S6) A carbon nanotube composite film flexible transparent substrate printed with a conductive silver paste electrode and covered with a copper foil current collector is bonded together using hot melt adhesive to obtain a single-walled carbon nanotube functional film.
[0017] Furthermore, the organic metal catalyst is ferrocene, nickelocene, cobaltocene or a mixture thereof, and the concentration in the thin film growth precursor solution is 0.5-10%;
[0018] The promoter is sulfur powder, selenium powder, thiophene or carbon disulfide, and the concentration in the film growth precursor solution is 0.025-2%;
[0019] The nanoparticles with infrared absorption and blocking properties are antimony tin oxide (ATO), indium tin oxide (ITO), tungsten oxide (WO3), cesium tungstate, tungsten bronze or a mixture thereof, with a particle size of 1-100 nanometers and a concentration of 5-25% in the film growth precursor solution.
[0020] The organic solvent is methanol, ethanol, isopropanol, acetone, benzene, toluene, xylene or heptane.
[0021] Furthermore, the heating temperature in S2) is 800-1500° C.;
[0022] The carrier gas is a mixture of nitrogen, argon and hydrogen (volume ratio is 1-3:1), and the flow rate is 20-2000sccm;
[0023] The injection flow rate of the injection pump is 0.01-20 ml / min.
[0024] Furthermore, the porous filter membrane in S3) is a microporous filter membrane with a pore size of 0.1-2.0 microns;
[0025] The material of the microporous filter membrane is glass fiber-GF, ultrafiltration cellulose-CELL, mixed cellulose-MCE, polypropylene-BHP, polyethersulfone-PES, polyvinylidene fluoride-PVDF, polytetrafluoroethylene-PTFE, nylon-Nylon or regenerated cellulose-RCE.
[0026] Furthermore, the pressure of the pressure transfer in S4) is 1-20 MPa;
[0027] The flexible transparent substrate is a transparent polymer sheet made of polyethylene terephthalate, polystyrene, polymethyl methacrylate, polycarbonate, polyimide or polyvinyl chloride, and has a thickness of 10 microns to 500 microns.
[0028] Furthermore, after the transfer in S4) is completed, a solvent treatment method is used to strengthen the adhesion between the carbon nanotube composite film and the flexible transparent substrate;
[0029] The solvent treatment method is: soaking the carbon nanotube composite film and the flexible transparent substrate after the transfer in a volatile solvent;
[0030] The volatile solvent is methanol, ethanol, acetone or a mixture thereof.
[0031] Furthermore, the hot melt adhesive in S6) is TPU, EVA, PA, PES, or reactive hot melt adhesive.
[0032] Another aspect of the present invention provides a single-walled carbon nanotube functional film, which is prepared based on the method of any one of the above claims.
[0033] Furthermore, the surface resistance of the single-walled carbon nanotube functional film is 50-400 ohms / square, the electric heating temperature control range is 30-90°C, the ultraviolet blocking rate is 60-90%, the infrared blocking rate is 80-95%, and the visible light transmittance is 70-88%.
[0034] Compared with the prior art, the single-walled carbon nanotube functional film and the preparation method thereof of the present invention have the following outstanding beneficial effects:
[0035] (1) The combination of single-walled carbon nanotube flexible conductive film and infrared blocking nanomaterials can give full play to the characteristics of single-walled carbon nanotubes, such as flexibility, conductivity, visible light transmission, and ultraviolet light absorption, and the characteristics of infrared blocking materials, such as visible light transmission and infrared light absorption, to obtain the performance of flexibility, electric heating, ultraviolet light absorption, visible light transmission, and infrared light absorption, and realize electric heating defogging, infrared heat insulation, and ultraviolet radiation protection. It is an excellent intelligent energy-saving window film.
[0036] (2) The carbon nanotube film prepared by floating chemical vapor deposition does not require wet dispersion and destruction of the carbon nanotube structure, which greatly retains the structural integrity of the carbon nanotubes and does not require the use of any dispersant, significantly improving the film's comprehensive properties such as conductivity, flexibility, and light transmittance.
[0037] (3) A composite film of carbon nanotubes and infrared functional nanoparticles is synthesized in one step. The nanoparticles are uniformly embedded in the carbon nanotube network, avoiding the problem of insufficient film uniformity caused by secondary recombination. The process is simple and fast, and the functional properties of the film can be effectively controlled by simply adjusting the synthesis and collecting process parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a scanning electron microscope image of a carbon nanotube film prepared by the present invention;
[0039] Figure 2 is the Raman spectrum;
[0040] Figure 3 It is the temperature rise curve of carbon nanotube film under different voltages. DETAILED DESCRIPTION
[0041] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Example 1
[0042] Ferrocene (5%) and thiophene (0.5%) were dissolved in ethanol, and then cesium tungstate (15%) nanopowder (diameter 20 nm) was added thereto and ultrasonically dispersed to obtain a stable precursor solution for thin film growth;
[0043] The growth tube furnace was heated to 1150 °C, and a mixture of argon gas (100 sccm) and hydrogen gas (50 sccm) was introduced as a carrier gas. The precursor solution was then injected into the tube furnace via a syringe pump (0.05 mL / min) and sprayed into the high temperature zone via ultrasonic atomization for reaction.
[0044] At the outlet of the tube furnace, the grown carbon nanotube products are uniformly deposited on the mixed cellulose porous filter membrane (pore size 0.45 microns) under the action of negative pressure suction to form a carbon nanotube composite film;
[0045] The carbon nanotube composite film on the filter membrane was transferred to the surface of the PET flexible transparent substrate by pressure transfer (5 MPa), and then immersed in ethanol and treated with solvent to strengthen the adhesion to the substrate;
[0046] Conductive silver paste electrodes are printed on both ends of the carbon nanotube film by screen printing, covering the copper foil current collector; TPU hot melt adhesive is used to bond the PET flexible transparent substrate into a whole to obtain a functional film product.
[0047] like Figure 1 The following is a scanning electron microscope photo of the prepared carbon nanotube film. Figure 2 This is the Raman spectrum. The Raman spectrum is located at 1250 cm -1 and 1550 cm -1 The peaks near the graphite layer correspond to the D peak and the G peak, respectively. The G peak represents the degree of graphitization crystallization, and the D peak represents the non-graphitized structure. Therefore, the ratio of the two peak intensities is I G / I D The ratio can be used to qualitatively determine the degree of graphitization and crystallization of single-walled carbon nanotubes; before film encapsulation, a four-probe test is used to test its surface resistance, with a surface resistance of 200 ohms / square; a continuous temperature measurement and acquisition instrument is used to test the electrical heating characteristics, such as Figure 3 The figure shows the temperature rise curve of the film under different voltages. The electric heating temperature control range is 30-90°C. The optical performance is tested with a solar film tester, with an ultraviolet blocking rate of 87%, an infrared blocking rate of 90%, and a visible light transmittance of 85%. Example 2
[0048] Nickelocene (0.5%) and carbon disulfide (0.025%) were dissolved in acetone, and then nanopowder (diameter 10nm) of antimony tin oxide (5%) was added thereto, and a stable precursor solution for thin film growth was obtained by ultrasonic dispersion. The growth tube furnace was raised to 1000℃, and a mixture of argon 1000sccm and hydrogen 500sccm was introduced as carrier gas. Then the precursor solution was injected into the tube furnace through an injection pump (2.5mL / min), and then ultrasonically sprayed into the high temperature zone for reaction. At the outlet of the tube furnace, the grown carbon nanotube product was uniformly deposited on a glass cellulose filter membrane (pore size 0.1 micron) under the action of negative pressure suction to form a carbon nanotube composite film. Pressure transfer (5 MPa) to transfer the carbon nanotube composite film on the filter membrane to the surface of the PS flexible transparent substrate, then soak it in ethanol and strengthen the adhesion to the substrate through solvent treatment; screen printing is used to print conductive silver paste electrodes on both ends of the carbon nanotube film, covering the copper foil current collector; EVA hot melt adhesive is used to bond the PS flexible transparent substrate to obtain a functional film product. Before film packaging, a four-probe test is used to test its surface resistance, and the surface resistance is 800 ohms / square; a continuous temperature measurement and acquisition instrument is used to test the electric heating characteristics, and the electric heating temperature control range is 30-90℃; a solar film tester is used to test the optical performance, with a UV blocking rate of 76%, an infrared blocking rate of 80%, and a visible light transmittance of 89%. Example 3
[0049] Cobaltocene (10%) and sulfur powder (2%) were dissolved in toluene, and then ITO (25%) nanopowder (diameter ~20nm) was added thereto, and a stable film growth precursor solution was obtained by ultrasonic dispersion. The growth tube furnace was raised to 1500 ℃, and a mixture of argon 1500sccm and hydrogen 500sccm was introduced as a carrier gas. Then, the precursor solution was injected into the tube furnace through a syringe pump (20 mL / min), and ultrasonically sprayed into the high-temperature zone for reaction. At the outlet of the tube furnace, the grown carbon nanotube product was uniformly deposited on a nylon porous filter membrane (pore size 2.0 microns) under the action of negative pressure suction to form a carbon nanotube composite film. Pressure transfer (5 MPa) to transfer the carbon nanotube composite film on the filter membrane to the surface of the PC flexible transparent substrate, then soak it in ethanol and strengthen the adhesion to the substrate through solvent treatment; screen printing is used to print conductive silver paste electrodes on both ends of the carbon nanotube film, covering the copper foil current collector; PA hot melt adhesive is used to bond it to the PC flexible transparent substrate to obtain a functional film product. Before film packaging, a four-probe test is used to test its surface resistance, and the surface resistance is 95 ohms / square; a continuous temperature measurement and acquisition instrument is used to test the electrical heating characteristics, such as Figure 3 The figure shows the temperature rise curve of the film under different voltages. The electric heating temperature control range is 30-90°C. The optical performance is tested using a solar film tester, with a UV blocking rate of 95%, an infrared blocking rate of 94%, and a visible light transmittance of 65%. Example 4
[0050] Ferrocene (2.5%), cobaltocene (2.5%) and thiophene (1%) were dissolved in isopropanol, and then cesium tungstate (10%) nanopowder (diameter 50nm) was added thereto, and a stable film growth precursor solution was obtained by ultrasonic dispersion. The growth tube furnace was raised to 1150℃, and a mixture of argon 500sccm and hydrogen 500sccm was introduced as carrier gas. Then the precursor solution was injected into the tube furnace through a syringe pump (10 mL / min), and then ultrasonically sprayed into the high temperature zone for reaction. At the outlet of the tube furnace, the grown carbon nanotube product was uniformly deposited on a polyvinylidene fluoride porous filter membrane (pore size 0.6 microns) under the action of negative pressure suction to form a carbon nanotube composite film. Pressure transfer (5 MPa) to transfer the carbon nanotube composite film on the filter membrane to the surface of the PET flexible transparent substrate, then soak it in ethanol and strengthen the adhesion to the substrate through solvent treatment; screen printing is used to print conductive silver paste electrodes on both ends of the carbon nanotube film, covering the copper foil current collector; PES hot melt adhesive is used to bond the PET flexible transparent substrate to obtain a functional film product. Before film packaging, a four-probe test is used to test its surface resistance, with a surface resistance of 150 ohms / square; a continuous temperature measurement and acquisition instrument is used to test the electric heating characteristics, and the electric heating temperature control range is 30-90℃; a solar film tester is used to test the optical performance, with a UV blocking rate of 94%, an infrared blocking rate of 92%, and a visible light transmittance of 80%.
[0051] Comparative Example 1:
[0052] Comparative Example 1: A single-walled carbon nanotube film is first obtained in the same manner as in Example 1, and then a cesium tungstate dispersion is sprayed on the surface of the single-walled carbon nanotube film. Other processes are the same as in Example 1. Before film encapsulation, a four-probe test is used to test the surface resistance, and the surface resistance is 600 ohms / square; a continuous temperature measurement and acquisition instrument is used to test the electric heating characteristics, and the electric heating temperature control range is 30-90°C; a solar film tester is used to test the optical properties, and the ultraviolet blocking rate is 84%, the infrared blocking rate is 85%, and the visible light transmittance is 81%. The comparative data are summarized in Table 1.
[0053] Table 1
[0054] Example Surface resistance (ohms / square) UV blocking rate Infrared blocking rate Visible light transmittance Example 1 200 87% 90% 85% Example 2 800 76% 80% 89% Example 3 95 95% 94% 65% Example 4 150 94% 92% 80% Comparative Example 1 600 84% 85% 81%
[0055] From the above comparative data, it can be seen that Example 1 of the present invention and the comparative example have higher conductivity and better light transmittance under similar processes, and the difference is obvious; it can be seen from other examples that the performance of the film prepared by the present invention is more balanced.
[0056] The embodiments described above are only preferred specific implementations of the present invention. Common changes and substitutions made by those skilled in the art within the scope of the technical solution of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a single-walled carbon nanotube functional film, characterized in that: The method prepares a thin film growth precursor solution by dissolving and dispersing nanoparticles with infrared absorption and blocking properties, an organic metal catalyst, and a co-catalyst in an organic solvent; Subsequently, the thin film growth precursor is injected into a tube furnace to grow single-walled carbon nanotubes using a floating chemical vapor deposition method. The product is uniformly deposited on the surface of the porous filter membrane at the outlet of the tube furnace and then transferred to the surface of the flexible transparent substrate. The electrodes are printed on the surface of the transferred flexible transparent substrate, and finally bonded to the encapsulation layer to form a whole; The organic metal catalyst is ferrocene, nickelocene, cobaltocene or a mixture thereof, and the concentration in the thin film growth precursor solution is 0.5-10%; The promoter is sulfur powder, selenium powder, thiophene or carbon disulfide, and the concentration in the film growth precursor solution is 0.025-2%; The nanoparticles with infrared absorption and blocking properties are antimony tin oxide, indium tin oxide, tungsten oxide, cesium tungstate, tungsten bronze or a mixture thereof, with a particle size of 1-100 nanometers and a concentration of 5-25% in the film growth precursor solution; The organic solvent is methanol, ethanol, isopropanol, acetone, benzene, toluene, xylene or heptane.
2. The method for preparing a single-walled carbon nanotube functional film according to claim 1, characterized in that: The implementation process of the method includes the following steps: S1) dissolving an organic metal catalyst and a co-catalyst in an organic solvent, then adding nanoparticles having infrared absorption and blocking properties thereto, and ultrasonically dispersing the nanoparticles to obtain a stable precursor solution for thin film growth; S2) heating the tube furnace to raise the temperature, introducing the carrier gas, and then injecting the precursor solution into the tube furnace through the injection pump, and spraying it into the high temperature zone through ultrasonic atomization to react; S3) At the outlet of the tube furnace, the grown carbon nanotube products are uniformly deposited on the porous filter membrane under the action of negative pressure suction to form a carbon nanotube composite film; S4) transferring the carbon nanotube composite film on the filter membrane to the surface of the flexible transparent substrate by pressure transfer; S5) printing conductive silver paste electrodes on both ends of the carbon nanotube film by screen printing and covering them with copper foil current collectors; S6) A carbon nanotube composite film flexible transparent substrate printed with a conductive silver paste electrode and covered with a copper foil current collector is bonded together using hot melt adhesive to obtain a single-walled carbon nanotube functional film.
3. The method for preparing a single-walled carbon nanotube functional film according to claim 2, characterized in that: The heating temperature in S2) is 800-1500° C.; The carrier gas is a mixture of nitrogen, argon and hydrogen, respectively, with a volume ratio of 1-3 to 1 and a flow rate of 20-2000 sccm; The injection flow rate of the injection pump is 0.01-20 ml / min.
4. The method for preparing a single-walled carbon nanotube functional film according to claim 2, characterized in that: The porous filter membrane in S3) is a microporous filter membrane with a pore size of 0.1-2.0 microns; The material of the microporous filter membrane is glass fiber-GF, ultrafiltration cellulose-CELL, mixed cellulose-MCE, polypropylene-BHP, polyethersulfone-PES, polyvinylidene fluoride-PVDF, polytetrafluoroethylene-PTFE, nylon-Nylon or regenerated cellulose-RCE.
5. The method for preparing a single-walled carbon nanotube functional film according to claim 2, characterized in that: The pressure of the pressure transfer in S4) is 1-20 MPa; The flexible transparent substrate is a transparent polymer sheet made of polyethylene terephthalate, polystyrene, polymethyl methacrylate, polycarbonate, polyimide or polyvinyl chloride, and has a thickness of 10 microns to 500 microns.
6. The method for preparing a single-walled carbon nanotube functional film according to claim 2, characterized in that: After the transfer in S4) is completed, a solvent treatment method is used to strengthen the adhesion between the carbon nanotube composite film and the flexible transparent substrate; The solvent treatment method is: soaking the carbon nanotube composite film and the flexible transparent substrate after the transfer in a volatile solvent; The volatile solvent is methanol, ethanol, acetone or a mixture thereof.
7. The method for preparing a single-walled carbon nanotube functional film according to claim 2, characterized in that: The hot melt adhesive in S6) is TPU, EVA, PA, PES, or reactive hot melt adhesive.
8. A single-walled carbon nanotube functional film, characterized in that: The single-walled carbon nanotube functional film is prepared based on the method of any one of the above claims.
9. The single-walled carbon nanotube functional film according to claim 8, characterized in that: The surface resistance of the single-walled carbon nanotube functional film is 50-400 ohms / square, the electric heating temperature control range is 30-90°C, the ultraviolet blocking rate is 60-90%, the infrared blocking rate is 80-95%, and the visible light transmittance is 70-88%.