Active Si raw material and preparation method thereof, negative electrode material precursor and preparation method thereof, negative electrode material and preparation method thereof, and negative electrode sheet

By optimizing the preparation process of silicon sludge, high-quality active Si raw materials were prepared, and negative electrode materials with excellent electrochemical properties were prepared through disproportionation reaction with SiO2 and carbon-encapsulated treatment, which solved the volume expansion and production cost of silicon negative electrode materials. High problems have achieved improved material performance and reduced cost.

CN118458788BActive Publication Date: 2024-11-29ZHEJIANG LICHEN NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410939663.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-29
Estimated Expiration
2044-07-15

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of silicon negative electrode materials, and in particular to an active Si raw material and a preparation method thereof, a negative electrode material precursor and a preparation method thereof, a negative electrode material and a preparation method thereof, and a negative electrode plate. The preparation method of the above-mentioned active Si raw material comprises: drying and dehydrating a silicon mud material to obtain air-dried silicon mud; granulating and sieving the air-dried silicon mud in sequence to obtain granular silicon mud and powdered silicon mud; blending the granular silicon mud and powdered silicon mud to obtain blended silicon mud; drying the blended silicon mud at high temperature to obtain dried silicon mud; depolymerizing the dried silicon mud to obtain an active Si raw material. The preparation method has the advantages of low cost, high safety, and good product performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon anode materials, and particularly to an active Si raw material and its preparation method, a precursor of an anode material and its preparation method, an anode material and its preparation method, and an anode electrode sheet. Background Art

[0002] Silicon anode materials are considered an ideal choice for the next-generation lithium-ion battery anodes because pure silicon (Si), as the active material of the anode material, has a theoretical capacity as high as 4200 mAh / g. However, pure silicon will undergo significant volume expansion (up to more than 300%) during the charge and discharge process, which leads to the rupture of the electrode material and the rapid decay of battery performance, thus making the direct application of pure silicon in lithium-ion battery anodes face major challenges.

[0003] To overcome this problem, researchers have developed silicon oxide (SiO x , where 0 < x ≤ 2) materials. These materials can form inert substances such as inactive Li2O and Li4SiO4 during the first lithium intercalation process, and these inert substances, as buffer layers, can significantly reduce the volume expansion during the lithium intercalation process. In addition, by carbon coating the surface of silicon monoxide, not only can the overall conductivity of the material be improved, but the carbon layer also has a certain restrictive effect on the expansion of silicon monoxide, thereby enhancing the overall cycle performance of the material.

[0004] In industrial production, the large-scale preparation of silicon monoxide usually uses micron-sized silicon powder and quartz powder as raw materials. After充分 mixing, they are then fired in a high-temperature vacuum furnace. Although this method is simple and feasible, it has a strong dependence on raw materials, especially the demand for high-purity silicon powder. The price of high-purity silicon powder is expensive, which directly leads to an increase in the production cost of silicon monoxide materials, thus limiting the possibility of their large-scale commercial application.

[0005] Therefore, developing a cost-effective synthesis method for silicon powder and silicon monoxide is crucial for promoting the application of silicon-based anode materials in commercial lithium-ion batteries. Summary of the Invention

[0006] To solve or partially solve the problems existing in the related art, the present invention provides an active Si raw material and its preparation method, a precursor of an anode material and its preparation method, an anode material and its preparation method, and an anode electrode sheet.

[0007] The present invention provides a preparation method for an active Si raw material, which includes:

[0008] Air-drying and dehydrating the silicon mud material to obtain air-dried silicon mud;

[0009] Granulating and sieving the air-dried silicon mud in sequence to obtain granular silicon mud and powdered silicon mud;

[0010] The granular silicon mud and the powdered silicon mud are blended to obtain blended silicon mud;

[0011] Drying the mixed silicon mud at high temperature to obtain dried silicon mud;

[0012] The dried silicon mud is depolymerized to obtain active Si raw material.

[0013] Furthermore, the water content of the silicon mud material is 45wt%~55wt%, and the water removal rate in the drying and dehydration process is 3wt%~10wt%; and / or, the particle size of the granular silicon mud is 0.5~5cm, and the particle size of the powdered silicon mud is less than 0.5cm.

[0014] Furthermore, the content of powdered silicon mud in the blended silicon mud is 0.5wt%~10wt%; and / or, the temperature of the high-temperature drying is 450~850°C, and the time is 3~5 hours.

[0015] The present invention also provides an active Si raw material, which is prepared according to any of the methods described above; the oxygen content of the active Si raw material is less than 5wt%, the carbon content is less than 0.5wt%, and the particle size D50 is 0.5~1.0um.

[0016] The present invention also provides a method for preparing a negative electrode material precursor, which comprises:

[0017] The above-mentioned active Si raw material and SiO2 are used as raw materials for disproportionation reaction, and the product is crushed and classified to obtain a negative electrode material precursor;

[0018] The mixing ratio of the active Si raw material to SiO2 is 1:(1.5-2.5); the temperature of the disproportionation reaction is 1250-1450°C, and the pressure is 0.01-100 Pa.

[0019] The present invention also provides a negative electrode material precursor, which is prepared according to the above method.

[0020] Furthermore, the particle size D50 of the negative electrode material precursor is 5.5±1 um.

[0021] The present invention also provides a method for preparing a negative electrode material, which comprises:

[0022] The negative electrode material precursor is subjected to carbon coating treatment and then sieved to obtain the negative electrode material; the carbon coating treatment is solid phase carbon coating or gas phase carbon coating.

[0023] The present invention also provides a negative electrode material, which is prepared according to the above method; the particle size D50 of the negative electrode material is 7±1 um.

[0024] The present invention also provides a negative electrode plate, which comprises a negative electrode current collector and a negative electrode active material layer deposited on the negative electrode current collector; the negative electrode active material layer contains the above-mentioned negative electrode material.

[0025] The present invention also embodies a negative electrode sheet, which includes a negative electrode current collector and a negative electrode active material layer deposited on the negative electrode current collector; the negative electrode active material layer contains the negative electrode material.

[0026] The preparation method of the active Si raw material provided by the present invention can have the following beneficial effects:

[0027] 1. This method removes water and organic matter from the silicon mud by drying, dehydrating, granulating, screening, and mixing and drying. After drying, granulation is performed to obtain silicon mud in the form of particles with relatively uniform volume, ensuring the uniformity of drying and minimizing the occurrence of oxidation. In the drying process, a mixed drying method of powdered silicon mud and granular silicon mud is introduced. The flammable nature of powdered silicon mud is utilized to generate instantaneous high temperature during the drying process to help fully volatilize organic matter such as cutting fluid and coolant remaining in the silicon mud. Therefore, this method not only effectively reduces the risk of spontaneous combustion of silicon mud during the drying process and ensures production safety, but also obtains high-quality active Si raw materials with uniform raw material particle size and low oxygen and carbon content.

[0028] 2. This method uses silicon mud as raw material, improves the utilization rate of silicon mud by optimizing the purification process, reduces the production cost of active Si raw materials, and the obtained active Si raw materials have low oxygen and carbon content, which helps to improve the performance of its downstream products, such as silicon oxide, negative electrode materials, etc., provides competitive raw materials for related industries, and improves economic benefits.

[0029] In summary, the preparation method of the active Si raw material provided by the present invention has the advantages of low cost, high safety and good product performance.

[0030] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms "a", "the" and "the" used in the present invention and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0033] It should be understood that although the terms "first", "second", "third", etc. may be used to describe various information in the present invention, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0034] Crystalline silicon is the core material of the global photovoltaic industry, and silicon wafers are an important component of photovoltaic cells. The production process of silicon wafers is the silicon debris produced by the cutting of polycrystalline silicon by diamond wire. Because the thickness of silicon wafers (150 microns) is similar to that of diamond wire (50 microns), cutting 1 ton of polycrystalline silicon will produce about 300 kilograms of silicon mud. Because cutting fluid and coolant are required during cutting, silicon mud in a broad sense is a mixture of a solution containing silicon powder by pressure filtration. In terms of weight, Si and water account for a large proportion. Silicon mud is packaged and sold as solid waste every year. According to statistics, about 400,000 tons of silicon mud are produced every year, most of which are re-smelted and enter the industrial silicon recycling industry. At present, the recycling of silicon mud mainly involves high-purity silicon, ceramics, silicon carbide and lithium batteries. Considering that silicon mud contains a large amount of Si, the inventors of this application consider using silicon mud as a reducing agent to synthesize silicon oxide to reduce the raw material cost of silicon oxide and increase the added value of silicon mud.

[0035] However, the inventors of the present application have found that the following properties of silicon mud affect its effect as a reducing agent in silicon oxide synthesis:

[0036] Silica mud itself is a mixture with complex components and high water content, which makes it easy for the silica mud to agglomerate during the drying process. Agglomeration will lead to uneven drying, making it difficult for the moisture inside the silica mud to evaporate, thus affecting the dryness of the silica mud and subsequent chemical reactions. In addition, it also contains organic matter, which is easy to decompose at high temperatures to produce carbon residues, which not only reduces the purity of the silicon oxide product, but may also affect its electrochemical properties.

[0037] Therefore, the inventors of the present application continued to improve the purification process, increasing the uniformity of water removal during the drying process, increasing the removal rate of organic matter, and reducing the amount of oxidation during the purification process.

[0038] Based on the above inventive concept, an embodiment of the present invention provides a method for preparing an active Si raw material, which comprises:

[0039] Drying and dehydrating the silicon mud material to obtain dried silicon mud;

[0040] The dried silicon mud is granulated and sieved in sequence to obtain granular silicon mud and powdered silicon mud;

[0041] The granular silicon mud and the powdered silicon mud are blended to obtain blended silicon mud;

[0042] Drying the mixed silicon mud at high temperature to obtain dried silicon mud;

[0043] The dried silicon mud is depolymerized to obtain active Si raw material.

[0044] Since silicon mud contains a large amount of highly active nano-silicon and has a high water content, direct drying of silicon mud is prone to spontaneous combustion in the drying equipment; and it is easy to agglomerate and clump during drying, resulting in a long drying time and uneven drying of moisture. In this embodiment, it is considered to first granulate the silicon mud to make it into a granular state with a relatively uniform size, so as to make the volume of the particles entering the drying equipment consistent, ensure the uniformity of drying and minimize the occurrence of oxidation. However, the water content in the silicon mud is too large, which leads to adhesion between particles, reduces fluidity, and is not easy to form particles during granulation. Therefore, in this embodiment, the silicon mud material is first dried and dehydrated to remove part of the water, so that it is more suitable for the subsequent granulation process, and it can be specifically dried on the ground. It can be understood by those skilled in the art that the silicon mud described in this application refers to the silicon mud produced in the production and cutting of silicon wafers. Preferably, the water content of the above-mentioned silicon mud material is 45wt%~55wt%, and the water removal rate of the drying and dehydration process is 3wt%~10wt%. In some embodiments, the water content of the silicon mud material is 45wt%, 47wt%, 50wt%, 52wt%, 55wt%, etc.; the water removal rate of the drying and dehydration process is 3wt%, 5wt%, 7wt%, 10wt%, etc., and of course it can also be other values ​​within the above range, which is not limited here. The water content of the dried silicon mud obtained is most preferably 37~ 50wt%. The water content of the dried silicon mud can be 37wt%, 40wt%, 42wt%, 45wt%, 49wt%, 50wt%, etc., and of course it can also be other values ​​within the above range.

[0045] After the dried silicon mud is obtained, the granulation process can be carried out. The purpose of this step is to obtain granular silicon mud (i.e., the aforementioned granular silicon mud) to improve the uniformity of silicon mud drying in the subsequent drying process. During the granulation process, the particle size of the silicon mud can be controlled. If the particles are too small, because the surface area of ​​the particles is relatively large, it is easy to react with oxygen in the outside air, so it is easy to cause more oxidation. On the contrary, if the particles are too large, drying will be difficult, resulting in more residual moisture. The particle size of the granular silicon mud is preferably 0.5~5cm. In some embodiments, the particle size of the granular silicon mud is 0.5cm, 1cm, 1.5cm, 2cm, 2.5cm, 3cm, 3.5cm, 4cm, 4.5cm, 5cm, etc., of course, it can also be other values ​​within the above range. More preferably 1~2cm, specifically 1cm, 1.5cm, 2cm, etc.

[0046] At the same time, this process also screens after granulation, and collects the powdered silicon mud under the screen. The powdered silicon mud is extremely active, and it will spontaneously combust and produce instantaneous high temperature during the subsequent drying process, which is usually considered to be a feature that is not suitable for drying. However, the inventors of this application consider mixing it with granular silicon mud in a certain proportion and then drying it. The instantaneous high temperature generated by the powdered silicon mud during the drying process helps to fully volatilize the organic matter (such as cutting fluid and coolant, etc.) remaining in the granular silicon mud. By controlling the blending ratio of the powdered silicon mud, it can be ensured that the organic matter is rapidly volatilized and removed without causing the overall spontaneous combustion of the silicon mud material. The particle size of the powdered silicon mud is preferably less than 0.5 cm. The particle size of the powdered silicon mud can be 0.5 cm, 0.4 cm, 0.3 cm, 0.2 cm, 0.1 cm, 0.05 cm, 0.01 cm, etc., and of course it can also be other values ​​within the above range.

[0047] After obtaining the granular silicon mud and the powdered silicon mud according to the above steps, the step of blending can be performed. The role of blending is to use the instantaneous high temperature generated by the powdered silicon mud to help fully volatilize the organic matter remaining in the granular silicon mud. In this step, the content of the powdered silicon mud in the blended silicon mud is preferably 0.5wt%~10wt%. In some embodiments, the content of the powdered silicon mud in the blended silicon mud is 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, etc., and of course it can also be other values ​​within the above range. More preferably, it is 1~ 5wt%, specifically 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, etc., and of course it can also be other values ​​within the above range.

[0048] After obtaining the mixed silicon mud, the step of high temperature drying can be carried out, which is used to remove moisture and organic matter in the silicon mud. As a preferred embodiment of this embodiment, the temperature of high temperature drying is 450-850°C. In some embodiments, the temperature of high temperature drying is 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc., and of course it can also be other values ​​within the above range. More preferably, it is 550-800°C, specifically 550°C, 580°C, 600°C, 620°C, 650°C, 680°C, 700°C, 730°C, 750°C, 780°C, 800°C, etc., and of course it can also be other values ​​within the above range. The drying temperature is too low, moisture or other impurities are not completely removed, and the active silicon and SiO2 mixture are finally obtained. In the process of producing silicon dioxide, one is that moisture will corrode the vacuum furnace, and the other is that the impurities that are not completely removed affect the sintering process of active silicon and silicon dioxide, which will result in extremely low yields. If the drying temperature is too high, although most of the moisture and impurities are removed, oxidation occurs inside the granular silicon mud, and the amount of active silicon is greatly reduced, and it cannot be reused. The high-temperature drying time is preferably 3 to 5 hours. After drying, it is also preferred to perform a vibration screening step to screen out the burnt powder.

[0049] After high-temperature drying to obtain dried silicon mud, it is necessary to depolymerize the dried silicon mud. The depolymerization process helps to destroy the particle structure and release active silicon, which can be solved by air flow crushing. After depolymerization, active Si raw material can be obtained. The particle size D50 of the obtained active Si raw material is 0.5~1.0um. In some embodiments, the particle size D50 of the active Si raw material is 0.5um, 0.55um, 0.59um, 0.6um, 0.65um, 0.69um, 0.7um, 0.75um, 0.78um, 0.8um, 0.83um, 0.85um, 0.87um, 0.9um, 0.91um, 0.93um, 0.95um, 0.98um, 1.0um, etc., of course, it can also be other values ​​within the above range. The oxygen and carbon content of the obtained active Si raw material is low, the oxygen content is less than 5wt%, and the carbon content is less than 0.5wt%. The obtained active Si raw material can be mixed with SiO2 and used as a raw material for preparing silicon monoxide.

[0050] From the above content, it can be seen that the preparation method of active Si raw material provided by the embodiment of the present invention has the following advantages:

[0051] 1. This method removes water and organic matter from the silicon mud by drying, dehydrating, granulating, screening, and mixing and drying. After drying, granulation is performed to obtain silicon mud in the form of particles with relatively uniform volume, ensuring the uniformity of drying and minimizing the occurrence of oxidation. In the drying process, a mixed drying method of powdered silicon mud and granular silicon mud is introduced. The flammable nature of powdered silicon mud is utilized to generate instantaneous high temperature during the drying process to help fully volatilize organic matter such as cutting fluid and coolant remaining in the silicon mud. Therefore, this method not only effectively reduces the risk of spontaneous combustion of silicon mud during the drying process and ensures production safety, but also obtains high-quality active Si raw materials with uniform raw material particle size and low oxygen and carbon content.

[0052] 2. This method uses silicon mud as raw material, improves the utilization rate of silicon mud by optimizing the purification process, reduces the production cost of active Si raw materials, and the obtained active Si raw materials have low oxygen and carbon content, which helps to improve the performance of its downstream products, such as silicon monoxide and negative electrode materials prepared therefrom, etc., provides competitive raw materials for related industries and improves economic benefits.

[0053] In summary, the method for preparing the active Si raw material provided by the embodiment of the present invention has the advantages of low cost, high safety and good product performance.

[0054] Another embodiment of the present invention also provides an active Si raw material, which is prepared according to the method of the above embodiment, and the specific implementation method is the same as the above embodiment, and this embodiment is not repeated here. The active Si raw material has uniform particle size, low oxygen and carbon content, and can be used as a raw material for silicon oxide production, which helps to improve the performance of silicon oxide while reducing production costs. Preferably, the oxygen content of the active Si raw material is less than 5wt%, and the carbon content is less than 0.5wt%. In some embodiments, the particle size D50 of the active Si raw material is 0.5um, 0.55um, 0.59um, 0.6um, 0.65um, 0.69um, 0.7um, 0.75um, 0.78um, 0.8um, 0.83um, 0.85um, 0.87um, 0.9um, 0.91um, 0.93um, 0.95um, 0.98um, 1.0um, etc., of course, it can also be other values ​​within the above range.

[0055] Another embodiment of the present invention further provides a method for preparing a negative electrode material precursor, which comprises: using the active Si raw material of the above embodiment and SiO2 as raw materials for a disproportionation reaction, and crushing and classifying the product to obtain a negative electrode material precursor.

[0056] This method uses SiO2 and the active Si raw material of the above embodiment as reaction raw materials. The purity of the SiO2 used is preferably >99.9%, and the particle size D50 is preferably 2~20 µm. The performance of silicon-oxygen negative electrode materials, such as capacity, cycle stability, etc., is related to the mixing ratio of silicon and silicon dioxide. In this embodiment, the mixing ratio of the active Si raw material and SiO2 is preferably controlled to be 1: (1.5~2.5), which helps to obtain a silicon-oxygen negative electrode material with excellent electrochemical properties. In some embodiments, the mixing ratio of the active Si raw material and SiO2 is 1:1.5, 1:1.6, 1:1.8, 1:2, 1:2.1, 1:2.3, 1:2.5, and of course it can also be other values ​​within the above range.

[0057] The active Si raw material and SiO2 can be mixed by a VC mixer, a three-eccentric mixer or a V-type mixer. The disproportionation reaction can be completed with the aid of a vacuum sintering furnace. The temperature of the disproportionation reaction is preferably 1250 ~ 1450 ° C, and the pressure is preferably 0.01 ~ 100 Pa. The temperature of the disproportionation reaction can be 1250 ° C, 1300 ° C, 1350 ° C, 1400 ° C, 1450 ° C, etc., and of course it can also be other values ​​within the above range. The pressure of the disproportionation reaction can be 10 Pa, 20 Pa, 30 Pa, 40 Pa, 50 Pa, 60 Pa, 70 Pa, 80 Pa, 90 Pa, 100 Pa, etc., more preferably 20~30 Pa, specifically 20 Pa, 22 Pa, 25 Pa, 28 Pa, 30 Pa, etc., and of course it can also be other values ​​within the above range. After the disproportionation reaction, bulk silicon oxide is obtained. After the obtained bulk silicon oxide is crushed and classified, silicon oxide bare powder, that is, the precursor of the negative electrode material, can be obtained. Specifically, the crushing can be performed by first using a double-roll jaw crusher for coarse crushing, and then using a ball mill or air flow crushing equipment for crushing. After crushing, classification can obtain silicon oxide bare powder with a D50 of 5.5±1um. In some embodiments, the particle size D50 of the silicon oxide bare powder is 4.5um, 4.9um, 5.0um, 5.3um, 5.5um, 5.8um, 6.0um, 6.3um, 6.5um, etc., and of course it can also be other values ​​within the above range. More preferably, the particle size distribution of the silicon oxide bare powder is as follows: D10 is 3±1um, D50 is 5.5±1um, and D90 is 9±1um.

[0058] Another embodiment of the present invention provides a negative electrode material precursor, which is prepared according to the method of the above embodiment. The specific implementation is the same as the above embodiment, and this embodiment is not repeated here. The particle size D50 of the negative electrode material precursor is preferably 5.5±1um. In some embodiments, the particle size D50 of bare silicon oxide powder is 4.5um, 4.9um, 5.0um, 5.3um, 5.5um, 5.8um, 6.0um, 6.3um, 6.5um, etc., and of course it can also be other values ​​within the above range. More preferably, the particle size distribution of the negative electrode material precursor is as follows: D10 is 3±1um, D50 is 5.5±1um, and D90 is 9±1um. The silicon-oxygen negative electrode material prepared with the negative electrode material precursor has excellent electrochemical properties.

[0059] Another embodiment of the present invention also provides a method for preparing a negative electrode material, which comprises: carbon coating the negative electrode material precursor of the above embodiment and then sieving to obtain the negative electrode material. The carbon coating treatment can be solid phase carbon coating or gas phase carbon coating. Solid phase carbon coating is to mix asphalt with bare powder, and carbon coating is performed under nitrogen protection and high temperature conditions. The mixing ratio of asphalt and silicon oxide bare powder (i.e., negative electrode material precursor) is preferably 1: (9~32). The temperature range of high temperature is preferably 850~1000℃. Carbon coating can be performed in a tube furnace or a box furnace. The gas phase carbon coating method is CVD carbon coating, which can be specifically: the negative electrode material precursor is put into a CVD furnace, the nitrogen atmosphere is heated to 900~1050℃, and a carbon source gas is introduced for carbon deposition. The carbon source gas can be acetylene, methane or propane, and the deposited carbon content is preferably 2wt%~7wt%.

[0060] Correspondingly, another embodiment of the present invention further provides a negative electrode material, which is prepared according to the method of the above embodiment. The specific implementation method is the same as the above embodiment, and this embodiment is not repeated here. The preferred particle size of the negative electrode material is as follows: D50 is 7±1um. In some embodiments, the particle size D50 of the negative electrode material is 6.0um, 6.3um, 6.5um, 6.8um, 7.0um, 7.1um, 7.4um, 7.9um, 8.0um, and of course it can also be other values ​​within the above range. More preferably, its particle size distribution is: D10 is 4±1um, D50 is 7±1um, and D90 is 11±1um. The specific surface area of ​​the negative electrode material is preferably 1.0 ~ 2.0 m 2 In some embodiments, the specific surface area of ​​the negative electrode material is 1.0 m 2 / g, 1.08m 2 / g, 1.09m 2 / g, 1.10m 2 / g, 1.11m 2 / g, 1.16m 2 / g, 1.2m 2 / g, / 1.25m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 1.9m 2 / g, 2.0m 2 / g, etc., and of course, other values ​​within the above range may also be used. The negative electrode material has excellent electrochemical properties.

[0061] Another embodiment of the present invention further provides a negative electrode sheet, which includes a negative electrode current collector and a negative electrode active material layer deposited on the negative electrode current collector; the negative electrode active material layer contains the above-mentioned negative electrode material. The lithium-ion battery assembled with the negative electrode sheet has excellent cycle stability, high reversible specific capacity and first coulombic efficiency.

[0062] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0063] The silicon mud raw materials in the following examples are all from the silicon mud mixture produced by diamond wire cutting when slicing polycrystalline silicon, and the water content thereof is about 52wt%. The SiO2 in the following examples is purchased from Guangzhou Xinxi Metallurgical Chemical Co., Ltd.

[0064] Example 1

[0065] (1) Spreading the silicon mud raw material on the ground to dry and remove moisture, removing 10wt% of moisture to obtain dried silicon mud; granulating the dried silicon mud with a granulator, and then passing it through a vibrating screen after granulation to screen out granular silicon mud with a size of 1.5cm and powdered silicon mud with a size of 0.2cm.

[0066] (2) The granular silicon mud obtained in (1) was mixed with the powdered silicon mud, with the powdered silicon mud accounting for 5wt% and the granular silicon mud accounting for 95wt%. The mixture was then placed in a drying furnace for high-temperature drying at a temperature of 600°C for 3.5 hours to obtain dried silicon mud.

[0067] (3) The obtained dried silicon mud is passed through a vibrating screen to remove the overburned powder; the dried silicon mud is depolymerized using air flow milling to obtain an active Si raw material with a D50 of 0.7 um.

[0068] (4) The active Si raw material is mixed with SiO2 with a D50 of 10 μm, and the mixing ratio of Si:SiO2 mass ratio is 1:2.

[0069] (5) The mixed material in (4) is put into a vacuum sintering furnace, and silicon oxide is reacted and deposited under the conditions of 1300°C and 25 Pa to obtain bulk silicon oxide. After crushing and classification, silicon oxide bare powder with a D50 of 5.50 μm is obtained.

[0070] (6) The bare silicon oxide powder in step (5) was subjected to gas phase carbon coating. The bare powder was placed in a CVD furnace, the temperature was raised to 1000°C in a nitrogen atmosphere, acetylene was used as a carbon source, and the deposition was performed for 2 hours. The deposited carbon content was controlled to be 5wt%.

[0071] (7) The carbon-coated material in step (6) is sieved to obtain a finished silicon oxide negative electrode material.

[0072] Example 2

[0073] The method is basically the same as Example 1, except that the amount of water removed in step (1) is reduced to 15 wt%.

[0074] Example 3

[0075] The method is basically the same as Example 1, except that the amount of water removed in step (1) is 2 wt%.

[0076] Example 4

[0077] The process is basically the same as Example 1, except that the proportion of powdered silicon mud in step (2) is adjusted to 1 wt %, the proportion of granular silicon mud is adjusted to 99 wt %, the drying temperature is 800° C., and the drying time is 5 h.

[0078] Example 5

[0079] The method is basically the same as Example 1, except that the proportion of powdered silicon mud in step (2) is adjusted to 10wt%, the proportion of granular silicon mud is adjusted to 90wt%, the drying temperature is 450°C, and the drying time is 3h.

[0080] Example 6

[0081] The method is basically the same as Example 1, except that the mass ratio of active Si raw material to SiO2 in step (4) is adjusted to 1:1.5.

[0082] Example 7

[0083] The method is basically the same as Example 1, except that the mass ratio of active Si raw material to SiO2 in step (4) is adjusted to 1:2.5.

[0084] Comparative Example 1

[0085] The method is basically the same as Example 1, except that steps (1) to (3) are replaced by the following steps:

[0086] The silicon mud raw material is dried at high temperature in an inert atmosphere at a drying temperature of 700° C. for a drying time of 4 hours to obtain dried silicon mud; the dried silicon mud is broken up to obtain an active Si raw material with a D50 of 0.9 um.

[0087] Comparative Example 2

[0088] The method is basically the same as Example 1, except that the proportion of silicon powder in step (2) is adjusted to 10wt%, and the proportion of silicon particles is adjusted to 90wt%. The silicon mud is then placed in a drying furnace for high-temperature drying at a temperature of 850°C for 10 hours to obtain dried silicon mud.

[0089] Comparative Example 3

[0090] The method is basically the same as Example 1, except that the proportion of silicon powder in step (2) is adjusted to 1wt%, and the proportion of silicon particles is adjusted to 99wt%. The silicon mud is then placed in a drying furnace for high-temperature drying at 300°C for 3h to obtain dried silicon mud.

[0091] Comparative Example 4

[0092] The method is basically the same as Example 1, except that the drying temperature in step (2) is adjusted to 1000°C.

[0093] Comparative Example 5

[0094] The process is basically the same as Example 1, except that the drying temperature in step (2) is adjusted to 300°C.

[0095] Comparative Example 6

[0096] The method is basically the same as Example 1, except that the proportion of powdered silicon mud in step (2) is adjusted to 0wt% and the proportion of granular silicon mud is adjusted to 100wt%.

[0097] The composition and structure of the active Si raw materials obtained in the above examples and comparative examples were characterized, wherein the oxygen content was tested by a German Elter Elementrac ONH-p oxygen and nitrogen analyzer, and the carbon content was tested by a German Elter ELEMentraccs-i high-frequency infrared carbon and sulfur analyzer. The sintering yield of the above active Si raw materials was also tested. The specific test results are shown in Table 1.

[0098] The particle sizes of the active silicon raw materials, bare silicon oxide powder and silicon oxide negative electrode materials obtained in the above embodiments and comparative examples were tested. The particle sizes (D50) were tested by using Mastersizer 3000 laser diffraction technology. The test results are shown in Table 2.

[0099]

[0100]

[0101] From Table 1 and Table 2, we can see that:

[0102] The method of the present invention can be used to dry silicon mud evenly, with low oxygen content, less organic residue, uniform particle size distribution, and high sintering yield after being mixed with silicon dioxide.

[0103] From the comparison of the data of Example 1 and Comparative Example 1, it can be seen that if the raw silicon mud is directly dried, the drying process is very uneven, the oxygen content of the silicon mud after drying is too high (10.4wt%), the organic matter residue is large (1.55wt%), and the sintering yield after mixing with silicon dioxide is low (76.3%), which is much lower than the yield of the silicon mud prepared by the present invention when sintered (93.2%).

[0104] Application Examples

[0105] The negative electrode materials prepared in each embodiment and comparative example are assembled into a battery, and the specific operation is as follows:

[0106] The preparation of the battery is divided into several steps: slurry stirring, pole piece preparation and battery assembly. The slurry is mainly composed of active material, conductive agent (SP), thickener (CMC) and binder (AB), with a mass ratio of 70:15:5:10. Take a clean and dry 300mL stirring tank, add conductive glue, negative electrode active material, CMC and AB, first put it into a mixer, stir at 800 r / min for 30s, and then stir at 2000 r / min for 20 minutes; the stirred slurry is coated on the copper foil to form a uniform line, and the coated copper foil is transferred to a vacuum drying oven, vacuum dried at 80℃ for 30 min, and then dried at 110℃ for 10h. After taking it out, weigh it, use a punching machine to punch the dried plate into a circular pole piece with a diameter of 14 mm, and use a tablet press to press it. And press the pole piece into a glove box. The battery assembly is carried out in a glove box filled with high-purity argon, and the water and oxygen content are kept <0.5 ppm. Lithium metal is used as the counter electrode, the electrolyte medium is 1M LiFP6, and the solvent is a mixture of EC, DEC and FEC in a volume ratio of 1:1:0.1. The battery is assembled in the order of positive electrode shell, pole piece, diaphragm, lithium sheet, nickel foam, and negative electrode shell. After being packaged in a hydraulic press, it can be taken out for electrochemical performance testing.

[0107] When assembling the battery, five batteries are prepared for each test, and a total of five sets of data are tested. The final performance is the average value of the five sets of data.

[0108] The battery cycle performance is tested on the Xinwei equipment, specifically:

[0109] At 25°C, first discharge at 0.1C to 0.005V, then discharge at 0.08C to 0.001V, discharge at 0.05C to 0.001V, discharge at 0.02C to 0.001V, and let stand for 10 minutes; then charge to 1.5V at 0.1C, let stand for 10 minutes, record the charge and discharge capacity after the first cycle, and calculate the first coulomb efficiency; cycle 300 times in the above manner, record the charge and discharge capacity after 300 times, and calculate the capacity retention rate after 300 cycles; the resistivity is tested by a semiconductor powder resistivity tester (30MPa four-probe V1.4); the specific surface area is the specific surface area of ​​the negative electrode material, measured using the American Mac TriStar3020 specific surface area and pore size analyzer. The specific test results are shown in Table 3 below.

[0110]

[0111] It can be seen from Table 3 that the lithium-ion battery assembled from the negative electrode material prepared by the present invention has excellent electrochemical properties, with a finished product capacity ≥1630 mAh / g, a first efficiency ≥75.5%, a resistivity ≤0.8Ω•cm at 10Mpa, and high cycle stability.

[0112] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing an active Si raw material, characterized in that: include: Drying and dehydrating the silicon mud material to obtain dried silicon mud; The water content of the silicon mud material is 45wt%~55wt%, and the water removal rate in the drying and dehydration process is 3wt%~10wt%; The dried silicon mud is granulated and sieved in sequence to obtain granular silicon mud and powdered silicon mud; the particle size of the granular silicon mud is 0.5-5 cm, and the particle size of the powdered silicon mud is less than or equal to 0.2 cm; The granular silicon mud and the powdered silicon mud are mixed to obtain mixed silicon mud; the content of the powdered silicon mud in the mixed silicon mud is 0.5wt% to 10wt%; The mixed silicon mud is subjected to high temperature drying to obtain dried silicon mud; the high temperature drying temperature is 450 to 850° C., and the time is 3 to 5 hours; The dried silicon mud is depolymerized to obtain active Si raw material.

2. An active Si raw material, characterized in that: It is prepared according to the method described in the claim; the oxygen content of the active Si raw material is less than 5wt%, the carbon content is less than 0.5wt%, and the particle size D50 is 0.5~1.0μm.

3. A method for preparing a negative electrode material precursor, characterized in that: include: The active Si raw material according to claim 2 is used as raw materials for a disproportionation reaction with SiO2, and the product is crushed and classified to obtain a negative electrode material precursor; The mixing ratio of the active Si raw material to SiO2 is 1:(1.5-2.5); the temperature of the disproportionation reaction is 1250-1450°C, and the pressure is 0.01-100 Pa.

4. A negative electrode material precursor, characterized in that: It is prepared according to the method described in claim 3.

5. The negative electrode material precursor according to claim 4, characterized in that: The particle size D50 of the negative electrode material precursor is 5.5±1 μm.

6. A method for preparing a negative electrode material, characterized in that: include: The negative electrode material precursor according to claim 4 is subjected to carbon coating treatment and then sieved to obtain the negative electrode material; the carbon coating treatment is solid phase carbon coating or gas phase carbon coating.

7. A negative electrode material, characterized in that: It is prepared according to the method described in claim 6; the particle size D50 of the negative electrode material is 7±1 μm.

8. A negative electrode plate, characterized in that: The invention comprises a negative electrode current collector and a negative electrode active material layer deposited on the negative electrode current collector; the negative electrode active material layer comprises the negative electrode material according to claim 7.

Citation Information

Patent Citations

  • Method for improving yield of metal silicon prepared by smelting diamond wire cutting silicon sludge

    CN114772602A

  • Active carbon layer-coated siloxy negative electrode material, preparation method and application of active carbon layer-coated siloxy negative electrode material

    CN116053437A