Antibacterial coating and preparation method thereof
By adjusting the composition and sintering technology of the ceramic coating, the problem of poor stability of the ceramic coating slurry is solved, an antibacterial coating with high strength, durability and ease of cleaning is achieved, and the overall performance and service life of the ceramic coating are improved. .
Patent Information
- Application Number
- CN202410916801.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
When the existing ceramic coating is combined with the metal embryo, the slurry has poor stability and is prone to delamination or precipitation, causing surface defects and voids in the coating, affecting the strength and cleanliness of the ceramic coating.
By adjusting the composition of the antibacterial coating, reducing the silica content, increasing the boron oxide content, combining nano-cuprous oxide and nano-magnesium oxide, and using step-temperature sintering technology, a uniform and dense coating structure is formed, which improves adhesion and resistance. Abrasion resistance, and improved thermal conductivity and ease of cleaning through boron nitride and carboxymethyl cellulose.
It achieves the high strength, durability and ease of cleaning of the ceramic coating, reduces defects and voids after sintering, improves the antibacterial performance and service life of the coating, and at the same time reduces the sintering temperature and energy consumption.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of coating processing, and in particular to an antibacterial coating and a preparation method thereof. Background Art
[0002] In the prior art, a Chinese invention patent with publication number CN100390098C proposes a ceramic product with antibacterial, mineralizing and water activating functions, as well as a preparation method and application thereof, wherein the functional ceramic product is composed of the following ingredients: montmorillonite, diatomaceous earth, aluminum oxide, silicon oxide, calcium carbonate, multifunctional healthy enamel material, and a binder; the multifunctional healthy enamel material is composed of silicon dioxide, aluminum oxide, iron oxide, sodium oxide, potassium oxide, calcium oxide, zinc oxide, boron oxide, and magnesium oxide, and the remainder is rare earth oxides and their inevitable impurities.
[0003] However, the formed slurry has poor stability and is prone to stratification or precipitation when combined with a metal body, resulting in defects and voids on the coating surface, which affects the strength of the ceramic coating or makes it difficult to clean. Summary of the invention
[0004] In order to reduce the impact on the strength of the ceramic coating and facilitate cleaning, the present application provides an antibacterial coating and a preparation method thereof.
[0005] In the first aspect, the present application provides an antibacterial coating, which adopts the following technical solution:
[0006] An antibacterial coating comprises, by weight percentage, 25.0-35.0% silicon dioxide, 8.0-9.0% aluminum oxide, 4.0-9.0% sodium oxide, 0-1.0% potassium oxide, 6.0-8.0% calcium oxide, 5.0-6.0% zinc oxide, 8.0-17.0% boron oxide, 4.0-6.0% magnesium oxide, 0-3.0% nano cuprous oxide, 0-3.0% nano magnesium oxide, 1.6-2.0% nano titanium dioxide, 13.0-16.5% titanium dioxide, 1.0-1.5% sodium salt, 1.0-3.0% boron nitride, and the remainder is rare earth oxide and its inevitable impurities.
[0007] By adopting the above technical scheme, by reducing the content of silicon dioxide in the antibacterial coating, reducing or removing the content of sodium oxide and potassium oxide, and increasing the content of boron oxide, it is beneficial to reduce the thermal expansion coefficient, change the fluidity and stability of the slurry, improve the adhesion and uniformity between the particles during the sintering process, reduce the slurry from stratification or precipitation, and at the same time improve the wear resistance of the coating and the hardness of the coating, which is helpful to form a uniform and dense coating structure during the sintering process, and improve the bonding strength and durability of the coating; improve the thermal conductivity and melt viscosity of the slurry during the sintering process, thereby reducing the sintering of the enamel material. The defects and gaps formed after the surface are removed make it easier to clean and have anti-adhesion, thereby improving the cleanability of the enamel material. The sodium salt enhances the adhesion between the embryo and the antibacterial coating. At the same time, silicon dioxide combines with boron oxide to wrap the oxides and sodium salts that are easily soluble in water, reducing their solubility in water. Titanium dioxide and cuprous oxide have a bactericidal effect. Sodium salt exists in the enamel coating as a network modifier, which can adjust the density, fluidity and uniformity of the glass network formed by boron oxide and silicon oxide, making the formed film structure more stable and dense, reducing the entry of water and making the surface smoother.
[0008] In a second aspect, the present application provides a method for preparing an antibacterial coating, which adopts the following technical solution:
[0009] A method for preparing an antibacterial coating, the preparation process steps are as follows:
[0010] a. Select the following raw materials by mass: 25.0-35.0 silicon dioxide, 8.0-9.0 aluminum oxide, 4.0-9.0 sodium oxide, 0-1.0 potassium oxide, 6.0-8.0 calcium oxide, 5.0-6.0 zinc oxide, 8.0-17.0 boron oxide, 4.0-6.0 magnesium oxide, 13.0-16.5 titanium dioxide; according to the above chemical composition, convert the various components into quartz, feldspar, borax, titanium dioxide, schachtite, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, kuye stone, magnesite, bauxite mineral raw materials according to common knowledge, weigh and mix, and add them to the ball mill in turn;
[0011] b. Screening the ball-milled material to form a mixed raw material;
[0012] c. sintering the mixed raw materials at 1100-1200°C in an oxygen environment to form a frit;
[0013] d. Select the raw material mass fraction: 4.0-5.0 of the nano antibacterial composite material, pre-mix it with triethanolamine, and mix the triethanolamine and the nano antibacterial material in a molar ratio of 1.0:0.8-0.9 to form an antibacterial agent; select the raw material mass fraction: 2.0-3.0 of boron nitride as an auxiliary agent;
[0014] e. The melt is cooled and crushed, mixed with an antibacterial agent and an additive to form a base glaze, and then carboxymethyl cellulose and water are added and added to a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 75-80%: 18-25%: 0-1.0%;
[0015] f. The ball-milled material is screened to form a slurry, the slurry is glazed on the body, and sintered at 700-900°C in an oxygen environment in a sintering furnace to form an enamel coating on the surface of the body, in which the carboxymethyl cellulose and water are removed during sintering.
[0016] By adopting the above technical scheme, according to the determined content ratio, according to the origin and component proportion of the raw materials, a certain weight of quartz, feldspar, borax, titanium dioxide, olivine and other mineral raw materials are sequentially added to the ball mill for ball milling, so that the above materials are broken and evenly dispersed, and then sieved to form a uniform mixed raw material, the mixed raw material is sintered under oxygen conditions to form a frit, during the sintering process, boron oxide and silicon oxide are mixed to form borosilicate glass, other metal oxides are coated, and then the frit is quickly cooled and crushed, and then added to the ball mill with a suspending agent, a nano-antibacterial composite material, boron nitride, carboxymethyl cellulose and water in a certain proportion, and ball milled again, and after the ball milling is completed, it is sieved, and then glazed on the surface of the embryo, and then sintered to form an antibacterial coating. The preparation of the antibacterial coating is completed through the above process, and the sintering temperature and sintering time are reduced by reducing the content of silicon, sodium and potassium, and increasing the content of boron oxide and calcium oxide. The thermal expansion coefficient of the material is reduced, the thermal stability is improved, and the addition of boron nitride makes the various components fully dispersed, making the internal structure more uniform, while reducing the defects and gaps formed after the enamel coating is sintered, making it easier to clean and anti-adhesive; and after sintering, silicon oxide and boron oxide combine to form borosilicate, which coats the oxide and sodium salt, reduces the reaction of water-soluble sodium salt and oxide with water, prolongs the service life of the coating, and reduces the harm to the human body; at the same time, the addition of boron nitride is convenient to improve the insulation of the enamel coating, improves the thermal conductivity, and facilitates the rapid heating of the cooker when cooking, and can reduce the sintering temperature, improve the surface smoothness, and facilitate cleaning; and the antibacterial material is mixed with triethanolamine, so that its molecular structure is uniformly mixed, and when mixed with the frit and sintered, the molecular structure formed together is adsorbed into the glass phase formed by silicon oxide and boron oxide, so that the antibacterial agent has the best antibacterial performance, and the triethanolamine is volatilized and separated from the antibacterial material during sintering, reducing the influence of the substance on the coating.
[0017] Optionally, in step a, the antibacterial nano composite material is nano titanium dioxide and one or two of nano magnesium oxide and nano cuprous oxide, and the nano titanium dioxide is anatase type.
[0018] By adopting the above technical scheme, nano-rutile titanium dioxide and one or more of nano-magnesium oxide, nano-boron oxide, nano-zinc oxide, and nano-cuprous oxide can all play a certain antibacterial role. Nano-rutile titanium dioxide has excellent photocatalytic and antibacterial properties, can effectively degrade organic matter and fight against bacteria, fungi and other microorganisms, and is helpful to improve the self-cleaning and antibacterial properties of the enamel coating; nano-magnesium oxide has good antibacterial properties, can inhibit the growth of bacteria and fungi, and is helpful to keep the enamel coating sanitary and clean; nano-boron oxide: has excellent high temperature resistance and chemical stability, and can enhance the wear resistance and corrosion resistance of the enamel coating; nano-zinc oxide and nano-cuprous oxide have antibacterial and anti-corrosion properties, can effectively inhibit the growth of bacteria, fungi and other microorganisms, and are helpful to improve the sanitary properties and service life of the enamel coating, so that it is easy to clean, anti-corrosive and can extend the service life while ensuring its antibacterial properties.
[0019] Optionally, in step b, the ball-milled material is added with anhydrous sodium hydroxide for further ball-milling, and then sieved.
[0020] By adopting the above technical scheme, in the preparation process of the enamel coating, the pH value of the environment is adjusted by adding sodium hydroxide. The appropriate pH value can promote the dispersion of various materials, which is beneficial to the uniform distribution between various materials, and facilitates the subsequent formation of a uniform and dense coating, thereby improving the stability of the coating. In addition, sodium hydroxide can react with a small amount of boron oxide, silicon oxide and aluminum oxide to form sodium salt, which plays a catalytic role in the curing process of the enamel coating, helps to improve the hardness and corrosion resistance of the coating, and improves the adhesion between the coating and the embryo. At the same time, during the sintering process, the sodium salt is coated with silicon oxide and boron oxide to form borosilicate, thereby reducing the dissolution of oxides and sodium salts in the water environment; and a trace amount of sodium hydroxide reacts with calcium oxide or magnesium oxide to form calcium hydroxide or magnesium hydroxide. A trace amount of calcium hydroxide and magnesium hydroxide are added to the enamel coating as fillers, and can increase the hardness and wear resistance of the coating, making it more durable and scratch-resistant, and can fill the tiny pores in the coating, thereby improving the sealing and waterproof properties of the coating.
[0021] Optionally, the content of sodium hydroxide is 6.0-7.0% of the content of silicon oxide.
[0022] By adopting the above technical scheme, the content of sodium hydroxide is limited, the excessive sodium hydroxide is reduced, and the excessive reaction with metal oxides such as silicon oxide and boron oxide that affects the proper properties of the enamel is reduced. The participation of sodium hydroxide can adjust the pH value, which is beneficial to the uniform distribution of various materials, and the produced sodium salt can increase the adhesion to the metal blank.
[0023] Optionally, in step f, the sintering temperature is 750-800°C.
[0024] By adopting the above technical scheme, the sintering temperature is reduced by adding boron oxide, and when anatase titanium dioxide is added, the anatase titanium dioxide is easily transformed from anatase titanium dioxide to rutile titanium dioxide after the temperature exceeds 800 degrees. The antibacterial effect is significantly improved by mixing anatase titanium dioxide and rutile titanium dioxide. The addition of boron oxide facilitates the reduction of the sintering temperature, and the antibacterial effect is maintained at the maximum without affecting the sintering effect, and can reduce the energy waste caused by sintering.
[0025] Optionally, the ratio of nano-anatase titanium dioxide to nano-magnesium oxide, nano-zinc oxide and nano-cuprous oxide is 2:3.
[0026] By adopting the above technical scheme, by adjusting the ratio of titanium dioxide to other metal oxides, it is convenient to improve the photocatalytic performance of each other, improve the antibacterial effect, and can interact with each other to form a heterojunction, improve the separation efficiency of carriers, thereby enhancing the photocatalytic activity. The formation of a heterojunction can reduce the recombination of electron-hole pairs, increase the lifetime of photogenerated carriers, adjust the band gap of the composite material, improve the response to visible light, and further improve the bactericidal effect.
[0027] Optionally, in step b, the particle size of the material is controlled to be 400-520 mesh and all pass.
[0028] By adopting the above technical solution and controlling the particle size during the first sintering, it is convenient to fully combine the components during sintering, and can achieve uniform dispersion of multiple substances, making the material structure more stable.
[0029] Optionally, in step f, the particle size of the material is controlled to be 900-1100 mesh and all passes.
[0030] By adopting the above technical solution and controlling the particle size of the material, the fineness of the slurry can be maintained, which helps to make up for the defects of the ceramic coating and reduce the generation of voids. At the same time, it can make the coating bond to the embryo and make the formed coating surface smoother, thereby maintaining and enhancing the cleanability of the coating.
[0031] Optionally, in step c, a step-by-step heating method is used during sintering to raise the temperature to 1100-1200°C.
[0032] By adopting the above technical solution, through the setting of step-by-step heating, the step-by-step heating can ensure that the entire melt can reach the required temperature and time at different stages, which is conducive to the uniform sintering of the material, reducing internal defects and improving the quality of the final product; and the different temperature platforms in the gradual heating process can promote the gradual reaction of different components in the material, optimize the microstructure and phase change behavior, and thus improve the physical and mechanical properties of the material; by reasonably designing the heating program, it is possible to stay at certain stages for a longer time to allow the material to fully react, which may reduce energy consumption overall because unnecessary overheating can be avoided; staying at certain temperature stages can control the growth rate of the grains; it is helpful to slowly eliminate the pores and defects inside the material, reduce the residual stress after sintering, improve the density and strength of the material, and make the structure formed in the melt more uniform and stable.
[0033] In summary, the present application includes at least one of the following beneficial technical effects:
[0034] 1. By reducing the content of silicon dioxide in the antibacterial coating, reducing or removing the content of sodium oxide and potassium oxide, and increasing the content of boron oxide, it is beneficial to reduce the thermal expansion coefficient, change the fluidity and stability of the slurry, improve the bonding force and uniformity between particles during sintering, reduce the stratification or precipitation of the slurry, and at the same time improve the wear resistance and hardness of the coating, which helps to form a uniform and dense coating structure during the sintering process, improve the bonding strength and durability of the coating; improve the thermal conductivity and melt viscosity of the slurry during the sintering process, thereby reducing the formation of enamel materials after sintering. Defects and voids are removed, making it easier to clean and anti-adhesive, thereby improving the cleanability of the enamel material, and the adhesion between the embryo and the antibacterial coating is enhanced through sodium salt. At the same time, silicon dioxide is combined with boron oxide to wrap the oxides and sodium salts that are easily soluble in water, reducing their solubility in water; titanium dioxide and cuprous oxide have a bactericidal effect; and sodium salt exists in the enamel coating, as a network modifier, it can adjust the density, fluidity and uniformity of the glass network formed by boron oxide and silicon oxide, making the formed film structure more stable and dense, reducing the entry of water, and making the surface smoother.
[0035] 2. By adjusting the ratio of titanium dioxide to other metal oxides, it is convenient to improve the photocatalytic performance of each other, improve the antibacterial effect, and interact with each other to form a heterojunction, improve the separation efficiency of carriers, and thus enhance the photocatalytic activity. The formation of a heterojunction can reduce the recombination of electron-hole pairs, increase the life span of photogenerated carriers, adjust the band gap of the composite material, improve the response to visible light, and further improve the bactericidal effect.
[0036] 3. Through the setting of step heating, the step heating can ensure that the entire melt can reach the required temperature and time at different stages, which is conducive to the uniform sintering of the material, reducing internal defects and improving the quality of the final product; and the different temperature platforms in the gradual heating process can promote the gradual reaction of different components in the material, optimize the microstructure and phase change behavior, and thus improve the physical and mechanical properties of the material; through the reasonable design of the heating program, it is possible to stay at certain stages for a longer time to allow the material to fully react, which may reduce energy consumption overall because unnecessary overheating can be avoided; staying at certain temperature stages can control the growth rate of the grains; it is helpful to slowly eliminate the pores and defects inside the material, reduce the residual stress after sintering, improve the density and strength of the material, and make the structure formed in the melt more uniform and stable. DETAILED DESCRIPTION
[0037] The embodiment of the present application discloses an antibacterial coating.
[0038] The composition includes by weight percentage: 25.0-35.0% silicon dioxide, 8.0-9.0% aluminum oxide, 4.0-9.0% sodium oxide, 0-1.0% potassium oxide, 6.0-8.0% calcium oxide, 5.0-6.0% zinc oxide, 8.0-17.0% boron oxide, 4.0-6.0% magnesium oxide, 0-3.0% nano cuprous oxide, 0-3.0% nano magnesium oxide, 1.6-2.0% nano titanium dioxide, 13.0-16.5% titanium dioxide, 1.0-1.5% sodium salt, 1.0-3.0% boron nitride, and the balance is rare earth oxides and inevitable impurities thereof.
[0039] The preparation method of the antibacterial coating comprises the following steps:
[0040] a. Select the following raw materials by mass: 25.0-35.0 silicon dioxide, 8.0-9.0 aluminum oxide, 4.0-9.0 sodium oxide, 0-1.0 potassium oxide, 6.0-8.0 calcium oxide, 5.0-6.0 zinc oxide, 8.0-17.0 boron oxide, 4.0-6.0 magnesium oxide, 13.0-16.5 titanium dioxide; according to the above chemical composition, convert the various components into quartz, feldspar, borax, titanium dioxide, schachtite, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, kuye stone, magnesite, bauxite mineral raw materials according to common knowledge, weigh and mix, and add them to the ball mill in turn;
[0041] b. After the ball milling, the material is added with anhydrous sodium hydroxide having a silicon oxide content of 6.0 to 7.0% for further ball milling, and then the material is sieved, and the particle size of the material is controlled to pass through 400 to 520 meshes to form a mixed raw material;
[0042] After anhydrous sodium hydroxide is mixed with the above-mentioned components at room temperature, part of the anhydrous sodium hydroxide reacts with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, part of the sodium hydroxide reacts with calcium oxide and magnesium oxide to form calcium hydroxide and magnesium hydroxide, and part of the sodium hydroxide remains unreacted and exists in the mixed raw materials in its original form. Under high-temperature sintering, part of the sodium hydroxide continues to react with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, and most of the calcium hydroxide and magnesium hydroxide form calcium oxide and magnesium oxide again at high temperature, resulting in the presence of trace amounts of calcium hydroxide and magnesium hydroxide, and sodium hydroxide forms sodium oxide at high temperature, wherein the total proportion of sodium silicate salt and sodium borate salt is between 1.0 and 1.5%, and the remaining components are sodium oxide, and the sum of the proportions of calcium hydroxide and magnesium hydroxide is 0.2%.
[0043] c. Sintering the mixed raw materials at 1100-1200°C in an oxygen environment, using a step-by-step heating method to raise the temperature to 1100-1200°C to form a melt;
[0044] d. Select the raw material mass fraction: 4.0-5.0 of the nano antibacterial composite material, pre-mix it with triethanolamine, and mix the triethanolamine and the nano antibacterial material in a molar ratio of 1.0:0.8-0.9 to form an antibacterial agent; select the raw material mass fraction: 2.0-3.0 of boron nitride as an auxiliary agent;
[0045] The nano antibacterial composite material is nano anatase titanium dioxide and one or two of nano magnesium oxide and nano cuprous oxide; the ratio of nano anatase titanium dioxide to nano magnesium oxide and nano cuprous oxide is 2:3;
[0046] e. The melt is cooled and crushed, mixed with an antibacterial agent and an additive, and then carboxymethyl cellulose and water are added, and the melt is added into a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 75-80%: 18-25%: 0-1.0%;
[0047] f. Screen the ball-milled material, control the particle size of the material to be 900-1100 meshes and allow it to pass through completely to form a slurry, glaze the slurry on the body, and sinter at 700-900°C in an oxygen environment in a sintering furnace. During sintering, a step-by-step temperature increase is adopted to form an enamel coating on the surface of the body, in which the carboxymethyl cellulose and water are removed during sintering.
[0048] Furthermore, the present invention also provides some specific embodiments and comparative examples in combination with the raw materials in the prior art, and tests the effects of the antibacterial coatings prepared in the embodiments and comparative examples, as shown below:
[0049] The raw materials and reagents used in the following examples are all commercially available or homemade.
[0050] Example 1: This example discloses an antibacterial coating, which comprises, by weight percentage, 35.0% silicon dioxide, 9.0% aluminum oxide, 4.0% sodium oxide, 1.0% potassium oxide, 8.0% calcium oxide, 6.0% zinc oxide, 8.0% boron oxide, 4.0% magnesium oxide, 0% nano cuprous oxide, 2.4% nano magnesium oxide, 1.6% nano titanium dioxide, 16.0% titanium dioxide, 1.0% sodium salt, 3.0% boron nitride, and the remainder being rare earth oxides and their inevitable impurities.
[0051] The preparation method is as follows:
[0052] a. Select the mass fraction of raw materials: 35.0 silica, 9.0 alumina, 3.0 sodium oxide, 1.0 potassium oxide, 8.0 calcium oxide, 6.0 zinc oxide, 8.0 boron oxide, 4.0 magnesium oxide, 16.0 titanium dioxide; according to the above chemical composition, the various components are converted into quartz, feldspar, borax, titanium dioxide, schaechette, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, Kuye stone, magnesite, bauxite mineral raw materials, weigh and mix, and add them to the ball mill in turn;
[0053] Among the above-mentioned minerals, 6 grams of dolomite, 17 grams of borax, 6 grams of calcined heavy zinc oxide, 14 grams of dolomite, 16 grams of titanium dioxide, 3 grams of potassium feldspar (forming 1 aluminum oxide), 34 grams of quartz, and 8 grams of bauxite are used as raw materials and mixed.
[0054] b. Add anhydrous sodium hydroxide with a silicon oxide content of 6.0% to the ball-milled material for further ball-milling, and then screen the material, and control the particle size of the material to pass through 450 meshes to form a mixed raw material; c. Sinter the mixed raw material at 1150°C in an aerobic environment, and the temperature difference during sintering shall not exceed ±50°C. The sintering shall be carried out in a step-by-step manner. When heating, each 100°C is used as a gradient, and each gradient is sintered for 10 minutes. After the temperature is raised to 1150°C, sinter for 30 minutes to form a frit;
[0055] Specifically, after anhydrous sodium hydroxide is mixed with the above ingredients at room temperature, part of the anhydrous sodium hydroxide reacts with silicon oxide and boron oxide to form sodium silicate and sodium borate, part of the sodium hydroxide reacts with calcium oxide and magnesium oxide to form calcium hydroxide and magnesium hydroxide, and part of the sodium hydroxide remains unreacted in the mixed raw material in its original form. The mixture is sintered at 100° C. for 10 minutes at each gradient, and the temperature is raised to 1150° C. for sintering, so that part of the sodium hydroxide continues to react with silicon oxide and boron oxide to form sodium silicate and sodium borate, and most of the calcium hydroxide and magnesium hydroxide are reacted at high temperature. Calcium oxide and magnesium oxide are formed again, resulting in the presence of trace amounts of calcium hydroxide and magnesium hydroxide. Sodium hydroxide forms sodium oxide at high temperature, wherein the mass proportions of sodium silicate, sodium borate, sodium oxide, calcium hydroxide and magnesium hydroxide are 0.7%: 0.3%: 0.9%: 0.12%: 0.08%, wherein calcium hydroxide and magnesium hydroxide exist in trace amounts; and the reaction of sodium hydroxide is related to the proportions of boron oxide, silicon dioxide, calcium oxide and magnesium oxide as well as the temperature, and the content is relatively small, forming a small amount of sodium salt and hydroxide, mainly sodium salt and sodium oxide, which play the role of a dense glass crystal phase.
[0056] d. Select the raw material by mass fraction: 4.0 nano antibacterial composite material, pre-mix with triethanolamine, and mix the triethanolamine and nano antibacterial material in a molar ratio of 1.0:0.8 to form an antibacterial agent; select the raw material by mass fraction: 3.0 boron nitride as an auxiliary agent;
[0057] Among them, the nano antibacterial composite material uses nano anatase titanium dioxide and nano magnesium oxide, and the ratio of nano anatase titanium dioxide to nano magnesium oxide is 2:3;
[0058] e. The melt is cooled and crushed, mixed with the antibacterial agent and the additive, and then carboxymethyl cellulose and water are added, and the melt is added into a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 80%:19%:1.0%;
[0059] f. The material after ball milling is sieved, and the particle size of the material is controlled to be 1000 mesh and all pass through to form a slurry. The slurry is glazed on the body and sintered at 800°C in an oxygen environment in a sintering furnace. The temperature difference during sintering does not exceed ±30°C, and the temperature is increased to 800°C by a step-by-step heating method, with each 150 degrees as a gradient, and each gradient is sintered for 10 minutes. After the temperature is increased to 800°C, it is sintered for 30 minutes to form an enamel coating on the surface of the body, and the carboxymethyl cellulose and water therein are removed during sintering.
[0060] Example 2: This example discloses an antibacterial coating, which comprises, by weight percentage, 25.0% silicon dioxide, 8.0% aluminum oxide, 9.0% sodium oxide, 0% potassium oxide, 6.0% calcium oxide, 5.0% zinc oxide, 17.0% boron oxide, 5.0% magnesium oxide, 3.0% nano cuprous oxide, 0% nano magnesium oxide, 2.0% nano titanium dioxide, 13.6% titanium dioxide, 1.0% sodium salt, 3.0% boron nitride, and the remainder being rare earth oxides and their inevitable impurities.
[0061] The preparation method is as follows:
[0062] a. Select the mass fractions of raw materials: 25.0 silica, 8.0 alumina, 8.2 sodium oxide, 0 potassium oxide, 6.0 calcium oxide, 5.0 zinc oxide, 17.0 boron oxide, 5.0 magnesium oxide, 13.6 titanium dioxide. According to the above chemical composition, the various components are converted into quartz, feldspar, borax, titanium dioxide, schaechette, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, Kuye stone, magnesite, bauxite mineral raw materials, weigh and mix, and add them to the ball mill in turn;
[0063] Among the above-mentioned minerals, 8 grams of magnesite, 35.7 grams of borax, 5 grams of calcined heavy zinc oxide, 10 grams of dolomite, 13.6 grams of titanium dioxide, 25 grams of quartz, and 8 grams of bauxite are used as raw materials for mixing.
[0064] b. The milled material was added with anhydrous sodium hydroxide having a silicon oxide content of 8.0% for further ball milling, and then the material was sieved, and the particle size of the material was controlled to pass through 450 mesh to form a mixed raw material;
[0065] c. Sinter the mixed raw materials at 1150℃ in an oxygen environment. The temperature difference during sintering does not exceed ±50℃. The temperature is increased in steps. When heating, each 100℃ is used as a gradient. Each gradient is sintered for 10min. After the temperature is increased to 1150℃, it is sintered for 30min, and a molten block is formed after rapid cooling.
[0066] Specifically, after anhydrous sodium hydroxide is mixed with the above-mentioned ingredients at room temperature, part of the anhydrous sodium hydroxide reacts with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, part of the sodium hydroxide reacts with calcium oxide and magnesium oxide to form calcium hydroxide and magnesium hydroxide, and part of the sodium hydroxide remains unreacted and exists in the mixed raw materials in its original form. Under high-temperature sintering, part of the sodium hydroxide continues to react with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, and most of the calcium hydroxide and magnesium hydroxide form calcium oxide and magnesium oxide again at high temperature, so that trace amounts of calcium hydroxide and magnesium hydroxide exist, and the sodium hydroxide forms sodium oxide at high temperature, wherein the mass proportions of sodium silicate salt, sodium borate salt, sodium oxide, calcium hydroxide, and magnesium hydroxide are 0.7%: 0.3%: 0.8%: 0.12%: 0.08%, wherein calcium hydroxide and magnesium hydroxide exist in trace amounts.
[0067] d. Select the raw material by mass fraction: 5.0 nano antibacterial composite material, pre-mix with triethanolamine, and mix the triethanolamine and nano antibacterial material in a molar ratio of 1.0:0.9 to form an antibacterial agent; select the raw material by mass fraction: 3.0 boron nitride as an auxiliary agent;
[0068] Among them, the nano antibacterial composite material uses nano anatase titanium dioxide and nano magnesium oxide, and the ratio of nano anatase titanium dioxide to nano cuprous oxide is 2:3;
[0069] e. The melt is cooled and crushed, mixed with the antibacterial agent and the additive, and then carboxymethyl cellulose and water are added, and the melt is added into a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 78%: 21.5%: 0.5%;
[0070] f. The material after ball milling is sieved, and the particle size of the material is controlled to be 1000 mesh and all pass through to form a slurry. The slurry is glazed on the body and sintered at 800°C in an oxygen environment in a sintering furnace. The temperature difference during sintering does not exceed ±30°C, and the temperature is increased to 800°C by a step-by-step heating method, with each 150 degrees as a gradient, and each gradient is sintered for 10 minutes. After the temperature is increased to 800°C, it is sintered for 30 minutes to form an enamel coating on the surface of the body, and the carboxymethyl cellulose and water therein are removed during sintering.
[0071] Example 3: This example discloses an antibacterial coating, which comprises, by weight percentage, 30.0% silicon dioxide, 8.0% aluminum oxide, 7.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 6.0% zinc oxide, 13.0% boron oxide, 5.5% magnesium oxide, 3.0% nano cuprous oxide, 0% nano magnesium oxide, 2.0% nano titanium dioxide, 12.6% titanium dioxide, 1.5% sodium salt, 3.0% boron nitride, and the remainder being rare earth oxides and their inevitable impurities.
[0072] The preparation method is as follows:
[0073] a. Select the mass fractions of raw materials: 30.0 silica, 8.0 alumina, 6.1 sodium oxide, 0 potassium oxide, 7.0 calcium oxide, 6.0 zinc oxide, 13.0 boron oxide, 5.5 magnesium oxide, 12.6 titanium dioxide. According to the above chemical composition, the various components are converted into quartz, feldspar, borax, titanium dioxide, zinc olivine, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, Kuye stone, magnesite, bauxite mineral raw materials, weigh and mix, and add them to the ball mill in turn;
[0074] Among the above-mentioned minerals, 9 grams of magnesite, 27 grams of borax, 6 grams of calcined heavy zinc oxide, 12.5 grams of dolomite, 12.6 grams of titanium dioxide, 30 grams of quartz, and 8 grams of bauxite are used as raw materials for mixing.
[0075] b. The milled material was added with anhydrous sodium hydroxide having a silicon oxide content of 8.0% for further ball milling, and then the material was sieved, and the particle size of the material was controlled to pass through 500 mesh to form a mixed raw material;
[0076] c. Sinter the mixed raw materials at 1150℃ in an oxygen environment. The temperature difference during sintering does not exceed ±50℃. The temperature is increased in steps. When heating, each 100℃ is used as a gradient. Each gradient is sintered for 10min. After the temperature is raised to 1150℃, it is sintered for 30min. After rapid cooling, a molten block is formed.
[0077] Specifically, after anhydrous sodium hydroxide is mixed with the above-mentioned ingredients at room temperature, part of the anhydrous sodium hydroxide reacts with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, part of the sodium hydroxide reacts with calcium oxide and magnesium oxide to form calcium hydroxide and magnesium hydroxide, and part of the sodium hydroxide remains unreacted and exists in the mixed raw materials in its original form. Under high-temperature sintering, part of the sodium hydroxide continues to react with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, and most of the calcium hydroxide and magnesium hydroxide form calcium oxide and magnesium oxide again at high temperature, so that trace amounts of calcium hydroxide and magnesium hydroxide exist, and the sodium hydroxide forms sodium oxide at high temperature, wherein the mass proportions of sodium silicate salt, sodium borate salt, sodium oxide, calcium hydroxide, and magnesium hydroxide are 1.0%: 0.5%: 0.9%: 0.10%: 0.10%, wherein calcium hydroxide and magnesium hydroxide exist in trace amounts.
[0078] d. Select the raw material by mass: 5.0 nano antibacterial composite material, pre-mix with triethanolamine, and mix the triethanolamine and nano antibacterial material in a molar ratio of 1.0:0.8 to form an antibacterial agent; select the raw material by mass: 3.0 boron nitride as an auxiliary agent;
[0079] Among them, the nano antibacterial composite material uses nano anatase titanium dioxide and nano magnesium oxide, and the ratio of nano anatase titanium dioxide to nano cuprous oxide is 2:3;
[0080] e. The melt is cooled and crushed, mixed with the antibacterial agent and the additive, and then carboxymethyl cellulose and water are added, and the melt is added into a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 75%: 24%: 1.0%;
[0081] f. The material after ball milling is sieved, and the particle size of the material is controlled to be 1000 mesh and all pass through to form a slurry. The slurry is glazed on the body and sintered at 800°C in an oxygen environment in a sintering furnace. The temperature difference during sintering does not exceed ±30°C, and the temperature is increased to 800°C by a step-by-step heating method, with each 150 degrees as a gradient, and each gradient is sintered for 10 minutes. After the temperature is increased to 800°C, it is sintered for 30 minutes to form an enamel coating on the surface of the body, and the carboxymethyl cellulose and water therein are removed during sintering.
[0082] Example 4: This example discloses an antibacterial coating, which comprises, by weight percentage, 30.0% silicon dioxide, 8.0% aluminum oxide, 7.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.0% zinc oxide, 12.0% boron oxide, 6.0% magnesium oxide, 3.0% nano cuprous oxide, 0% nano magnesium oxide, 2.0% nano titanium dioxide, 14.0% titanium dioxide, 1.5% sodium salt, 3.0% boron nitride, and the remainder being rare earth oxides and their inevitable impurities.
[0083] The preparation method is as follows:
[0084] a. Select the mass fractions of raw materials: 30.0 silica, 8.0 alumina, 6.1 sodium oxide, 0 potassium oxide, 7.0 calcium oxide, 5.0 zinc oxide, 12.0 boron oxide, 6.0 magnesium oxide, 14.0 titanium dioxide. According to the above chemical composition, the various components are converted into quartz, feldspar, borax, titanium dioxide, schaechette, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, Kuye stone, magnesite, bauxite mineral raw materials, weigh and mix, and add them to the ball mill in turn;
[0085] Among the above-mentioned minerals, 10 grams of magnesite, 25 grams of borax, 5 grams of calcined heavy zinc oxide, 12.5 grams of dolomite, 14 grams of titanium dioxide, 30 grams of quartz, and 8 grams of bauxite are used as raw materials for mixing.
[0086] b. The milled material was added with anhydrous sodium hydroxide having a silicon oxide content of 8.0% for further ball milling, and then the material was sieved, and the particle size of the material was controlled to pass through 500 mesh to form a mixed raw material;
[0087] c. Sinter the mixed raw materials at 1150°C in an oxygen environment. The temperature difference during sintering does not exceed ±50°C. The temperature is increased in steps. When the temperature is increased, each 100°C is used as a gradient. Each gradient is sintered for 10 minutes. After the temperature is increased to 1150°C, it is sintered for 30 minutes to form a molten block.
[0088] Specifically, after anhydrous sodium hydroxide is mixed with the above-mentioned ingredients at room temperature, part of the anhydrous sodium hydroxide reacts with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, part of the sodium hydroxide reacts with calcium oxide and magnesium oxide to form calcium hydroxide and magnesium hydroxide, and part of the sodium hydroxide remains unreacted and exists in the mixed raw materials in its original form. Under high-temperature sintering, part of the sodium hydroxide continues to react with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, and most of the calcium hydroxide and magnesium hydroxide form calcium oxide and magnesium oxide again at high temperature, so that trace amounts of calcium hydroxide and magnesium hydroxide exist, and the sodium hydroxide forms sodium oxide at high temperature, wherein the mass proportions of sodium silicate salt, sodium borate salt, sodium oxide, calcium hydroxide, and magnesium hydroxide are 1.0%: 0.5%: 0.9%: 0.10%: 0.10%, wherein calcium hydroxide and magnesium hydroxide exist in trace amounts.
[0089] d. Select the raw material by mass: 5.0 nano antibacterial composite material, pre-mix with triethanolamine, and mix the triethanolamine and nano antibacterial material in a molar ratio of 1.0:0.8 to form an antibacterial agent; select the raw material by mass: 3.0 boron nitride as an auxiliary agent;
[0090] Among them, the nano antibacterial composite material uses nano anatase titanium dioxide and nano magnesium oxide, and the ratio of nano anatase titanium dioxide to nano cuprous oxide is 2:3;
[0091] e. The melt is cooled and crushed, mixed with the antibacterial agent and the additive, and then carboxymethyl cellulose and water are added, and the melt is added into a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 80%:19%:1.0%;
[0092] f. The material after ball milling is sieved, and the particle size of the material is controlled to be 1000 mesh and all pass through to form a slurry. The slurry is glazed on the body and sintered at 800°C in an oxygen environment in a sintering furnace. The temperature difference during sintering does not exceed ±30°C, and the temperature is increased to 800°C by a step-by-step heating method, with each 150 degrees as a gradient, and each gradient is sintered for 10 minutes. After the temperature is increased to 800°C, it is sintered for 30 minutes to form an enamel coating on the surface of the body, and the carboxymethyl cellulose and water therein are removed during sintering.
[0093] Example 5: This example discloses an antibacterial coating, the composition of which includes by weight percentage: 30.0% silicon dioxide, 8.0% aluminum oxide, 7.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 14.0% boron oxide, 6.0% magnesium oxide, 3.0% nano cuprous oxide, 3.0% nano magnesium oxide, 2.0% nano titanium dioxide, 14.0% titanium dioxide, 1.0% sodium salt, 1.0% boron nitride, and the remainder is rare earth oxides and their inevitable impurities.
[0094] The preparation method is as follows:
[0095] a. Select the mass fractions of raw materials: 30.0 silica, 8.0 alumina, 7.4 sodium oxide, 0 potassium oxide, 7.0 calcium oxide, 5.5 zinc oxide, 14.0 boron oxide, 5.0 magnesium oxide, 14.0 titanium dioxide. According to the above chemical composition, the various components are converted into quartz, feldspar, borax, titanium dioxide, zinc olivine, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, Kuye stone, magnesite, bauxite mineral raw materials, weigh and mix, and add them to the ball mill in turn;
[0096] Among the above-mentioned minerals, 8 grams of magnesite, 29 grams of borax, 5 grams of calcined heavy zinc oxide, 12.5 grams of dolomite, 14 grams of titanium dioxide, 30 grams of quartz, and 8 grams of bauxite are used as raw materials for mixing. ;
[0097] b. The milled material was added with anhydrous sodium hydroxide having a silicon oxide content of 6.0% for further ball milling, and then the material was sieved, and the particle size of the material was controlled to pass through 500 mesh to form a mixed raw material;
[0098] c. Sinter the mixed raw materials at 1150°C in an oxygen environment. The temperature difference during sintering does not exceed ±50°C. The temperature is increased in steps. When the temperature is increased, each 100°C is used as a gradient. Each gradient is sintered for 10 minutes. After the temperature is increased to 1150°C, it is sintered for 30 minutes to form a molten block.
[0099] Specifically, after anhydrous sodium hydroxide is mixed with the above-mentioned ingredients at room temperature, part of the anhydrous sodium hydroxide reacts with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, part of the sodium hydroxide reacts with calcium oxide and magnesium oxide to form calcium hydroxide and magnesium hydroxide, and part of the sodium hydroxide remains unreacted and exists in the mixed raw materials in its original form. Under high-temperature sintering, part of the sodium hydroxide continues to react with silicon oxide and boron oxide to form sodium silicate salt and sodium borate salt, and most of the calcium hydroxide and magnesium hydroxide form calcium oxide and magnesium oxide again at high temperature, so that trace amounts of calcium hydroxide and magnesium hydroxide exist, and the sodium hydroxide forms sodium oxide at high temperature, wherein the mass proportions of sodium silicate salt, sodium borate salt, sodium oxide, calcium hydroxide, and magnesium hydroxide are 0.7%: 0.3%: 0.6%: 0.10%: 0.10%, wherein calcium hydroxide and magnesium hydroxide exist in trace amounts.
[0100] d. Select the raw material by mass fraction: 5.0 nano antibacterial composite material, pre-mix with triethanolamine, and mix the triethanolamine and nano antibacterial material in a molar ratio of 1.0:0.8 to form an antibacterial agent; select the raw material by mass fraction: 1.0 boron nitride as an auxiliary agent;
[0101] Among them, the nano antibacterial composite material uses nano anatase titanium dioxide and nano magnesium oxide, and the ratio of nano anatase titanium dioxide to nano cuprous oxide is 2:3;
[0102] e. The melt is cooled and crushed, mixed with the antibacterial agent and the additive, and then carboxymethyl cellulose and water are added, and the melt is added into a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 80%:19%:1.0%;
[0103] f. The material after ball milling is sieved, and the particle size of the material is controlled to be 1000 mesh and all pass through to form a slurry. The slurry is glazed on the body and sintered at 800°C in an oxygen environment in a sintering furnace. The temperature difference during sintering does not exceed ±30°C, and the temperature is increased to 800°C by a step-by-step heating method, with each 150 degrees as a gradient, and each gradient is sintered for 10 minutes. After the temperature is increased to 800°C, it is sintered for 30 minutes to form an enamel coating on the surface of the body, and the carboxymethyl cellulose and water therein are removed during sintering.
[0104] The test mainly tests the hardness, glossiness, surface flatness, dispersion and photocatalytic rate of the enamel coating. The wear resistance can be reflected by the hardness, glossiness and surface flatness, or the scratch test can be carried out on the surface of the enamel coating by metal tools, and the depth of the scratch can be observed under a microscope. When testing the dispersion, the finished product is cut and then observed under a microscope. When testing the adhesion, it is observed by immersing in chemical reagents. When testing the photocatalytic rate, 10×10 -5mol / L methyl orange aqueous solution was used as the experimental reference agent. It was illuminated under natural light for 3 hours, and the methyl orange concentration after illumination was detected to determine the photocatalytic rate.
[0105] The enamel products prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 were tested and experimented.
[0106]
[0107] By comparing Example 1, Example 2, Example 3, Example 4, and Example 5, it can be seen that when the content of silicon dioxide and aluminum oxide is greater, the hardness and glossiness are higher, and when the content of silicon dioxide and aluminum oxide decreases, the hardness and glossiness will become lower. Moreover, when the content of cuprous oxide or magnesium oxide and nano-titanium dioxide increases, the photocatalytic effect is stronger, and when the content of cuprous oxide and nano-titanium dioxide decreases, the photocatalytic effect decreases, but the decrease is not obvious and is within an acceptable range. Compared with cuprous oxide and nano-titanium dioxide, magnesium oxide and nano-titanium dioxide have higher photocatalytic properties, but when the content of magnesium oxide increases, the hardness increases.
[0108] Example 6: This example discloses an antibacterial coating, the composition of which includes by weight percentage: 35.0% silicon dioxide, 8.0% aluminum oxide, 5.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 11.0% boron oxide, 6.0% magnesium oxide, 3.0% nano cuprous oxide, 0% nano magnesium oxide, 2.0% nano titanium dioxide, 14.0% titanium dioxide, 1.0% sodium salt, 1.0% boron nitride, and the remainder is rare earth oxides and their inevitable impurities.
[0109] The preparation method and the ratio of the enamel coating are different from those in Example 2, and the rest are exactly the same as those in Example 2.
[0110] Example 7: This example discloses an antibacterial coating, the composition of which includes by weight percentage: 30.0% silicon dioxide, 8.0% aluminum oxide, 4.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 17.0% boron oxide, 6.0% magnesium oxide, 3.0% nano cuprous oxide, 0% nano magnesium oxide, 2.0% nano titanium dioxide, 14.0% titanium dioxide, 1.0% sodium salt, 1.0% boron nitride, and the remainder is rare earth oxides and their inevitable impurities.
[0111] The preparation method and the ratio of the enamel coating are different from those in Example 2, and the rest are exactly the same as those in Example 2.
[0112] Example 8: This example discloses an antibacterial coating, the weight percentage of which includes: 35.0% silicon dioxide, 8.0% aluminum oxide, 8.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 8.0% boron oxide, 6.0% magnesium oxide, 3.0% nano cuprous oxide, 0% nano magnesium oxide, 2.0% nano titanium dioxide, 14.0% titanium dioxide, 1.0% sodium salt, 1.0% boron nitride, and the remainder is rare earth oxides and their inevitable impurities.
[0113] The preparation method and the ratio of the enamel coating are different from those in Example 2, and the rest are exactly the same as those in Example 2.
[0114] Example 9: This example discloses an antibacterial coating, the weight percentage of which includes: 30.0% silicon dioxide, 8.0% aluminum oxide, 7.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 14.0% boron oxide, 6.0% magnesium oxide, 3.0% nano-cuprous oxide, 0% nano-magnesium oxide, 2.0% nano-titanium dioxide, 14.0% titanium dioxide, 1.0% sodium salt, 1.0% boron nitride, and the remainder is rare earth oxides and their inevitable impurities.
[0115] The preparation method and the ratio of the enamel coating are different from those in Example 2, and the rest are exactly the same as those in Example 2.
[0116] Comparative Example 1: This comparative example discloses an antibacterial coating, which comprises, by weight percentage, 32.0% silicon dioxide, 8.0% aluminum oxide, 7.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 14.0% boron oxide, 6.0% magnesium oxide, 3.0% nano-cuprous oxide, 0% nano-magnesium oxide, 2.0% nano-titanium dioxide, 14.0% titanium dioxide, and the remainder being rare earth oxides and inevitable impurities thereof.
[0117] The preparation method and the ratio of the antibacterial coating are different from those in Example 2, and sodium hydroxide is not added in step b, while boron nitride is added in step d.
[0118] The antibacterial coatings prepared in Example 6, Example 7, Example 8, Example 9 and Comparative Example 1 were tested and tested.
[0119]
[0120] In the comparative example 1, powder aggregation occurred during step f. Since sodium hydroxide and boron nitride were not added, the dispersion effect was poor and aggregation occurred, which made the chemical composition unstable. As a result, boron oxide failed to fully react with silicon dioxide to vitrify. As a result, when making wet enamel, part of the boron oxide reacted with water, resulting in a small amount of separation between the coating and the embryo.
[0121] By comparing Example 2 with Comparative Example 1, it can be seen that after increasing the content of silicon dioxide, the hardness increases significantly; after reducing the content of boron nitride, its dispersion is affected. By comparing Comparative Example 7 with Comparative Example 1, it can be seen that after removing boron nitride and sodium hydroxide, the chemical structure becomes unstable, boron oxide dissolves in water, and its photocatalytic effect is affected.
[0122] Example 10: This example discloses an antibacterial coating, whose composition is exactly the same as that of comparative example 1, except that in step c, when heating, each 200°C is used as a gradient, and each gradient is sintered for 10 minutes. After the temperature is raised to 1150°C, it is sintered for 30 minutes to form a molten block.
[0123] Comparative Example 2: This comparative example discloses an antibacterial coating, which comprises, by weight percentage, 30.0% silicon dioxide, 8.0% aluminum oxide, 7.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 15.0% boron oxide, 6.0% magnesium oxide, 3.0% cuprous oxide, 16.0% titanium dioxide, 1.0% sodium salt, and the remainder being rare earth oxides and inevitable impurities thereof.
[0124] By reducing step d, the addition of boron nitride.
[0125] Comparative Example 3: This comparative example discloses an antibacterial coating, which comprises, by weight percentage, 35.0% silicon dioxide, 8.0% aluminum oxide, 6.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 11.0% boron oxide, 6.0% magnesium oxide, 3.0% cuprous oxide, 16.0% titanium dioxide, 1.0% boron nitride, and the remainder being rare earth oxides and their inevitable impurities.
[0126] By reducing the addition of sodium hydroxide in step b.
[0127] Comparative Example 4: This comparative example discloses an antibacterial coating, which comprises, by weight percentage, 40.0% silicon dioxide, 8.0% aluminum oxide, 6.0% sodium oxide, 0% potassium oxide, 7.0% calcium oxide, 5.5% zinc oxide, 11.0% boron oxide, 6.0% magnesium oxide, 14.0% titanium dioxide, 1.0% boron nitride, and the remainder being rare earth oxides and inevitable impurities thereof.
[0128] By reducing the addition of the antibacterial agent in step d, the addition of nano cuprous oxide or nano magnesium oxide and nano titanium dioxide can be reduced.
[0129] The antibacterial coatings prepared in Example 10, Comparative Example 2, Comparative Example 3, and Comparative Example 4 were tested and tested.
[0130]
[0131] By comparing Comparative Example 6 with Example 10, it can be seen that when sintering, if the temperature rises too quickly, the density of the frit will be reduced, which will lead to a decrease in the bonding force in the subsequent steps, and at the same time, it has a certain impact on the degree of dispersion. By comparing Example 5 with Comparative Example 2, it can be seen that after removing the addition of boron nitride, the degree of dispersion decreases, which has a slight impact on the glossiness; by comparing Example 6 with Comparative Example 3, it can be seen that when anhydrous sodium hydroxide is not added, the bonding force decreases, resulting in separation; by comparing Example 5 with Comparative Example 4, it can be seen that after increasing the content of silicon dioxide, its hardness increases significantly, and the corresponding fluidity deteriorates, resulting in protrusions on the coating surface, and the corresponding bonding force is maintained, and with the removal of the nano-antibacterial composite material, its photocatalytic effect deteriorates, and the sterilization effect depends only on the titanium dioxide and magnesium oxide in the coating, and the antibacterial effect is attenuated.
[0132] The implementation principle of an antibacterial coating and a preparation method thereof in an embodiment of the present application is as follows: by reducing the content of silicon dioxide and aluminum oxide, the antibacterial enamel material has better thermal stability, and by adding sodium hydroxide, a small amount of sodium salt is produced, and by combining silicon dioxide and boron oxide, the sodium salt is coated to reduce its solubility in water, and the adhesion between the prepared coating and the embryo body is increased, and the attachment is more uniform; and by adding the frit and the antibacterial agent in batches, the titanium dioxide in the antibacterial agent and the titanium dioxide in the frit are maintained as two types, thereby improving the antibacterial effect, reducing the requirements for the external environment, and improving the applicability; by step-by-step heating, the damage to the chemical stability of the coating caused by rapid sintering is reduced, the stability of the glass phase is higher, and the coating effect of silicon dioxide and boron oxide on other substances is maintained.
[0133] Through the combined action of nano titanium dioxide, titanium dioxide and nano cuprous oxide, and magnesium oxide, the optical catalytic property is improved while the light stability is improved, thereby further improving the bactericidal effect; and the antibacterial material is pre-mixed and adsorbed by triethanolamine, so that the antibacterial material is evenly distributed and enters the molecular structure of the frit in the form of a combined substance, and then after the triethanolamine evaporates, it remains in the coating at the original position, thereby facilitating the improvement of its photocatalytic property, and triethanolamine and boron nitride cooperate with each other to increase the dispersibility of the frit and the antibacterial agent and improve the degree of dispersion; and the step-by-step heating is adopted to facilitate the slow volatilization of triethanolamine and reduce the generation of pores.
[0134] By adding anhydrous sodium hydroxide and boron nitride, it is easy to improve the insulation of the enamel coating, improve the thermal conductivity, facilitate the rapid heating of the cooker when cooking, and can reduce the sintering temperature, while improving its adhesion; and the sodium salt formed by the sodium salt acts as a network modifier. Through the dispersion of boron nitride, the density, fluidity and uniformity of the glass network formed by boron oxide and silicon oxide can be adjusted, so that the formed film structure is more stable and dense, and the entry of water is reduced. At the same time, the surface is smoother and the components are more dispersed, so as to form a uniform glass phase, fill the glass phase, improve the surface smoothness, and facilitate cleaning.
[0135] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing an antibacterial coating, characterized in that: The preparation process steps are as follows: a. Select the following raw materials by mass: silicon dioxide 25.0-35.0, aluminum oxide 8.0-9.0, sodium oxide 4.0-9.0, potassium oxide 0-1.0, calcium oxide 6.0-8.0, zinc oxide 5.0-6.0, boron oxide 8.0-17.0, magnesium oxide 4.0-6.0, titanium dioxide 13.0-16.5; according to the above chemical composition, convert the various components into quartz, feldspar, borax, titanium dioxide, schachtite, calcined heavy zinc oxide, dolomite, calcite, chalcedony, alum, mullite, magnesite, bauxite mineral raw materials according to common knowledge, weigh and mix, and add them to the ball mill in turn; b. Screening the ball-milled material to form a mixed raw material; c. sintering the mixed raw materials at 1100-1200°C in an oxygen environment to form a frit; d. Select the raw material mass fraction: 4.0-5.0 of the nano antibacterial composite material, pre-mix it with triethanolamine, and mix the triethanolamine and the nano antibacterial material in a molar ratio of 1.0:0.8-0.9 to form an antibacterial agent; select the raw material mass fraction: 2.0-3.0 of boron nitride as an auxiliary agent; The nano antibacterial composite material is nano titanium dioxide and one or two of nano magnesium oxide and nano cuprous oxide, and the nano titanium dioxide is anatase type; e. The melt is cooled and crushed, mixed with an antibacterial agent and an additive to form a base glaze, and then carboxymethyl cellulose and water are added and added to a ball mill for ball milling, wherein the mass proportion of the base glaze, water and hydroxymethyl cellulose is 75-80%: 18-25%: 0-1.0%; f. The ball-milled material is screened to form a slurry, the slurry is glazed on the body, and the body is sintered at 700 to 900° C. in an oxygen environment in a sintering furnace to form an enamel coating on the body surface, wherein the carboxymethyl cellulose and water are removed during sintering; In step b, the ball-milled material is added with anhydrous sodium hydroxide for further ball-milling, and then sieved; The content of sodium hydroxide is 6.0-7.0% of the content of silicon dioxide.
2. The method for preparing the antibacterial coating according to claim 1, characterized in that: In step f, the sintering temperature is 750-800°C.
3. The method for preparing the antibacterial coating according to claim 1, characterized in that: The ratio of nano-anatase titanium dioxide to nano-magnesium oxide and nano-cuprous oxide is 2:
3.
4. The method for preparing the antibacterial coating according to claim 1, characterized in that: In step b, the particle size of the material is controlled to be 400-520 mesh and all pass.
5. The method for preparing the antibacterial coating according to claim 1, characterized in that: In step f, the particle size of the material is controlled to be 900-1100 mesh and all passes.
6. The method for preparing the antibacterial coating according to claim 1, characterized in that: In step c, a step-by-step heating method is used during sintering to raise the temperature to 1100-1200°C.