A carbon-fixing ecostone from multi-source solid waste carbon mineralization and its preparation method
Through multi-source solid waste carbon mineralization technology, the use of solid waste and fiber and other materials, the high carbon emission and performance problems of traditional cement-based artificial stones are solved. The mineralized carbon solid ecological stones produced have higher density and compressive strength , and the hydrophobicity and glossiness are better than traditional products.
Patent Information
- Application Number
- CN202410941467.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Traditional cement-based artificial stones have problems such as high carbon emissions, low density, poor hardness, high water absorption and poor gloss.
The mineralized carbon solid waste mineralization technology is adopted to replace cement as cementitious material, waste crude slag as aggregate, and carbon dioxide as reaction medium. The mineralized carbon solid ecostone produced is optimized and introduced through optimization of formula and introduction. Calcium oxide, fiber and long-chain fatty acid modifiers to improve product density, compressive strength and hydrophobicity.
It achieves better performance and decorative effects than traditional artificial stones, reduces carbon emissions, improves product density and compressive strength, while reducing water absorption and improving gloss.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparing carbon-fixing ecological stone by utilizing multi-source solid waste, and specifically to a carbon-fixing ecological stone mineralized by multi-source solid waste and a preparation method thereof. Background Art
[0002] Artificial stone is a traditional building material made of marble chips, quartz, granite chips or other natural or artificial material aggregates mixed with cement or resin adhesives. Artificial stone has a series of decorative properties such as durability, beauty, customizability, and anti-penetration. It is generally used for floor decoration in shopping malls, hospitals, and home decoration.
[0003] Traditional artificial stone is mainly formed by pressing cement and quartz aggregate, marble aggregate, etc., and hardening naturally. For example, the Chinese patent document (authorization announcement number is CN 109553340 B) discloses recycled aggregate terrazzo and its preparation method and application. Using recycled aggregate terrazzo to replace the existing stone aggregate can reduce the production cost by 250 to 600 yuan / m 3 At the same time, based on the light weight and porous nature of the recycled aggregate, the porous structure has the effect of sound absorption and sound absorption; the Chinese patent document (authorization announcement number is CN115215604B) discloses a natural terrazzo and its preparation process, which uses a mixture of multiple stone powders to evenly disperse dolomite powder and quartz powder on the surface of the terrazzo, forming a layer of glass film on the surface of the terrazzo, reducing the corrosion loss of the stone powder inside the stone, and at the same time will not cover the natural texture of the stone surface, taking into account both aesthetics and corrosion resistance.
[0004] However, cement is used as the gel material, and cement belongs to the high carbon emission industry. The production of cement has a large amount of carbon emissions, and cement-based terrazzo has a low density (2.3t / m 3 ), poor gloss, high water absorption (≥4%), low hardness and other problems. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a carbon-fixing ecological stone with multi-source solid waste carbon mineralization, which uses bulk solid waste to replace cement as a cementitious material, uses waste slag as aggregate, and uses carbon dioxide as a reaction medium. The final mineralized carbon-fixing ecological stone can achieve performance and decorative effects comparable to or even better than traditional artificial stones with the concept of pure solid waste.
[0006] On the one hand, the present invention provides a carbon-fixing ecological stone obtained by carbon mineralization of multi-source solid waste. The raw materials for its preparation include at least 40-80 parts of calcium solid waste, 20-55 parts of aggregate, 10-30 parts of ultrafine solid waste, 1-5 parts of fiber, 1-10 parts of modifier, and 5-40 parts of water by weight; the modifier is a long-chain fatty acid containing two carboxyl groups and the two carboxyl groups are connected to the same carbon atom.
[0007] Further preferably, the carbon-fixing ecological stone obtained by carbon mineralization of multi-source solid waste comprises, by weight, at least 40-80 parts of calcareous solid waste, 25-55 parts of aggregate, 10-30 parts of ultrafine solid waste, 1-5 parts of fiber, 2-8 parts of modifier, and 10-35 parts of water as raw materials for its preparation.
[0008] As a preferred technical solution, the carbon chain length of the long-chain fatty acid is C 12 -C 20 .
[0009] Preferably, the long-chain fatty acid is selected from hexadecylmalonic acid (CAS No. 4371-64-6).
[0010] As a preferred technical solution, the ratio of water to the total mass of calcareous solid waste and ultrafine solid waste is 0.05-0.4, preferably 0.1-0.35.
[0011] As a preferred technical solution, the calcareous solid waste is at least one of steel slag, magnesium slag, calcium silicon slag and carbide slag.
[0012] Preferably, the calcareous solid waste contains at least steel slag.
[0013] Preferably, the calcareous solid waste is steel slag or a combination of steel slag and at least one of magnesium slag, calcium-silicon slag and carbide slag.
[0014] As a preferred technical solution, the aggregate is at least one of quartz waste, broken glass, shells, and metal recycling tailings.
[0015] Preferably, the aggregate contains at least quartz waste.
[0016] Preferably, the aggregate is quartz waste or a combination of quartz waste and at least one of broken glass, shells, and metal recycling tailings.
[0017] As a preferred technical solution, the fineness of the ultrafine solid waste is 200-800 mesh, preferably 300-500 mesh, and more preferably 300-400 mesh.
[0018] As a preferred technical solution, the ultrafine solid waste contains calcium oxide.
[0019] Preferably, the ultrafine solid waste is selected from at least one of slag powder, steel slag powder and quartz tailings powder.
[0020] Preferably, the ultrafine solid waste is selected from at least one of slag powder and steel slag powder.
[0021] As a preferred technical solution, the fiber is one or a mixture of inorganic fiber, plant fiber and synthetic fiber.
[0022] Preferably, the inorganic fiber is selected from at least one of waste glass fibers and waste carbon fibers; the plant fiber is selected from at least one of sawdust, straw, and bamboo fibers; and the synthetic fiber is selected from at least one of polyamide fibers, polypropylene fibers, and polyacrylonitrile fibers.
[0023] Preferably, the fiber is plant fiber; preferably, the plant fiber is at least one of sawdust, straw, and bamboo fiber.
[0024] As a preferred technical solution, the raw materials for preparing the carbon-fixing ecological stone obtained by multi-source solid waste carbon mineralization also include a defoaming agent, and the amount of the defoaming agent used is 0.1-0.5wt% of the modifier, preferably 0.2-0.3wt%.
[0025] As a preferred technical solution, the defoaming agent is at least one of a polyether defoaming agent, a silicone defoaming agent, and a polyether-modified polysiloxane defoaming agent, preferably a polyether-modified polysiloxane defoaming agent. By adding the defoaming agent, bubbles generated by the modifier during the material stirring process are eliminated, thereby improving the tap density of the product.
[0026] In response to the problems of high carbon emissions from raw materials, low product density, poor hardness, high water absorption and poor glossiness of traditional cement-based artificial stones, the present invention has developed a mineralized carbon-fixing ecological stone system, which uses industrial solid waste as raw material to react with industrial flue gas, and the mineralized products improve the density and compressive strength of the product.
[0027] Specifically, the present invention ensures the performance and appearance of mineralized ecological stone by optimizing the solid waste aggregate system in the formula system and coordinating the mineralized solid waste raw material system. On the other hand, by introducing ultrafine solid waste containing calcium oxide, while not affecting the progress of the mineralization reaction and the appearance of the product after polishing, it also helps the modifier in the system to undergo sufficient decarboxylation reaction and generate sufficient fatty acid calcium, fill the pores and interface transition zone of the mineralized product, improve the strength and hydrophobicity, and reduce the water absorption rate of the product; in addition, the present invention introduces at least one fiber from straw, sawdust, and waste glass fibers, which can react with the carboxyl group in the modifier without affecting the mineralization reaction and the final polishing effect, further improve the strength, enhance the toughness of the early green body, and solve the problem of the fragility of the early green body of the mineralization system (unlike cement that will harden naturally).
[0028] Furthermore, the present invention can ensure the occurrence of decarboxylation reaction in the reaction environment by adding 2-8 parts by weight of a modifier in the system, especially controlling the modifier to be a long-chain fatty acid containing two carboxyl groups and the two carboxyl groups are linked to the same carbon atom and the carbon chain length is C12-C20, so as to generate carbon dioxide, so that the inside of the blank can undergo a sufficient mineralization reaction, improve the strength of the product, and play a good hydrophobic role, reducing the water absorption rate of the product. The inventor analyzed that the reason may be: during the mineralization reaction, as the temperature in the reactor increases with the exothermic heat of mineralization, and the calcium oxide contained in the steel slag acts as a catalyst, the modifier undergoes a decarboxylation reaction, removes a carboxyl group and releases CO2, which can cause a sufficient mineralization reaction inside the blank and improve the strength of the product. Moreover, the carboxyl group on the modifier or the product after the decarboxylation reaction (still containing a carboxyl group) can react with the calcium oxide in the system to generate fatty acid calcium, which can not only fill the gaps inside the product and further improve the strength, but also play a good hydrophobic role and reduce the water absorption rate of the product. Monocarboxyl fatty acids (such as stearic acid) do not contain electron-withdrawing groups, and it is difficult for decarboxylation to occur in the environment of this system. They only play a hydrophobic role and cannot produce CO2 to achieve internal mineralization. Short-chain fatty dicarboxylic acids (such as propylmalonic acid) have too short carbon chains. Although they can produce CO2 to achieve internal mineralization, the short-chain fatty acid calcium produced has poor hydrophobic effect.
[0029] Another aspect of the present invention provides a method for preparing carbon-fixing ecological stone by multi-source solid waste carbon mineralization, which comprises at least the following steps:
[0030] The calcareous solid waste, aggregate, ultrafine solid waste, fiber and modifier are uniformly mixed to obtain a mixed dry material;
[0031] adding water to the mixed dry materials to obtain a mixed slurry;
[0032] The mixed slurry is put into a mold and pressed by a press, the molding pressure is 10-60MPa, the pressure holding time is 1-5 minutes, and after molding, the green body is pushed out by the press to obtain a green body;
[0033] Move the green body to the curing kiln for moisturizing curing, with the humidity in the kiln at 70-95% and the temperature at 40-80℃;
[0034] After the moisturizing and curing, the green body is moved to a mineralization reactor for mineralization reaction, the pressure is controlled at 0.2-0.8MPa, the reaction time is 2-10h, and the plate is obtained;
[0035] The slabs are subjected to thickness-setting, polishing and grinding treatments to obtain ecological stone slabs with high surface gloss, and then surface protection treatments are performed to obtain finished products.
[0036] Preferably, the molding pressure of the compression molding in the mold is 30-50 MPa, and the holding time is 2-4 minutes.
[0037] Preferably, the vacuum system is turned on while pressing in the mold to extract excess moisture and gas from the green body from the pressing system, and the moisture content after molding is controlled at 6-12%.
[0038] Preferably, the moisture content after molding is controlled at 6-8%.
[0039] Preferably, the humidity in the kiln for moisturizing curing is 85-95%, and the temperature is 50-70°C.
[0040] Preferably, the pressure of the mineralization reaction is controlled at 0.4-0.8 MPa, and the reaction time is 6-8 h.
[0041] Preferably, the reaction temperature in the mineralization reactor is controlled at above 100° C., or the volume of the green body undergoing the mineralization reaction in the mineralization reactor is above 15% of the inner volume of the reactor, preferably above 18%.
[0042] The inventors found that in actual production, after the green body is placed in the reactor, the volume of the green body accounts for more than 15% of the internal volume of the reactor, and the temperature in the reactor can reach more than 100°C through the mineralization heat release of the mineralizable substances in the green body. Therefore, for the control of the temperature in the reactor, the temperature in the reactor can be controlled to be above 100°C by additional heating, or the temperature in the reactor can be controlled to be more than 100°C by controlling the volume of the green body to be more than 15% of the internal volume of the reactor.
[0043] Beneficial Effects
[0044] 1. The present invention provides a carbon-fixing ecological stone that is mineralized from multi-source solid waste carbon. It uses bulk solid waste to replace cement as a cementitious material, uses waste slag as aggregate, and uses carbon dioxide as a reaction medium. The final mineralized carbon-fixing ecological stone can achieve performance and decorative effects comparable to or even better than traditional artificial stones with the concept of pure solid waste.
[0045] 2. In view of the problems of high carbon emissions from raw materials, low product density, poor hardness, high water absorption and poor glossiness in traditional cement-based artificial stones, the present invention has developed a mineralized carbon-fixing ecological stone system, which uses industrial solid waste as raw material to react with industrial flue gas, and the mineralized products improve the density and compressive strength of the product.
[0046] 3. On the one hand, the present invention ensures the performance and appearance of the mineralized carbon-fixing ecological stone by optimizing the solid waste aggregate system in the formula system and coordinating the mineralized solid waste raw material system. On the other hand, by introducing ultrafine solid waste containing calcium oxide, while not affecting the progress of the mineralization reaction and the appearance of the product after polishing, it also helps the modifier in the system to fully decarboxylate and generate sufficient fatty acid calcium, fill the pores and interface transition areas of the mineralized product, improve the strength and hydrophobicity, and reduce the water absorption rate of the product.
[0047] 4. The present invention introduces at least one fiber selected from straw, wood chips, and waste glass fibers, which can react with the carboxyl group in the modifier without affecting the mineralization reaction and the final polishing effect, thereby further improving the strength and enhancing the early toughness of the green body, thereby solving the problem of the early green body fragility of the mineralization system (unlike cement that hardens naturally).
[0048] 5. The present invention adds a modifier to the system, especially controls the modifier to be a long-chain fatty acid containing two carboxyl groups linked to the same carbon atom and having a carbon chain length of C12-C20, so that a sufficient mineralization reaction can be carried out inside the blank, thereby improving the strength of the product and playing a good hydrophobic role, thereby reducing the water absorption rate of the product. DETAILED DESCRIPTION
[0049] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0050] Example
[0051] The carbon-fixing ecological stone of multi-source solid waste carbon mineralization of the present invention comprises, by weight, at least 40-80 parts of calcareous solid waste, 20-55 parts of aggregate, 10-30 parts of ultrafine solid waste, 1-5 parts of fiber, 1-10 parts of modifier, and 5-40 parts of water; the modifier is a long-chain fatty acid containing two carboxyl groups and the two carboxyl groups are connected to the same carbon atom.
[0052] A method for preparing carbon-fixing ecological stone by multi-source solid waste carbon mineralization, comprising at least the following steps:
[0053] The calcareous solid waste, aggregate, ultrafine solid waste, fiber and modifier are uniformly mixed to obtain a mixed dry material;
[0054] adding water to the mixed dry materials to obtain a mixed slurry;
[0055] The mixed slurry is put into a mold and pressed by a press, the molding pressure is 10-60MPa, the pressure holding time is 1-5 minutes, and after molding, the green body is pushed out by the press to obtain a green body;
[0056] Move the green body to the curing kiln for moisturizing curing, with the humidity in the kiln at 70-95% and the temperature at 40-80℃;
[0057] After the moisturizing and curing, the green body is moved to a mineralization reactor for mineralization reaction, the pressure is controlled at 0.2-0.8MPa, the reaction time is 2-10h, and the plate is obtained;
[0058] The slabs are subjected to thickness-setting, polishing and grinding treatments to obtain ecological stone slabs with high surface gloss, and then surface protection treatments are performed to obtain finished products.
[0059] In some embodiments, the carbon-fixing ecological stone obtained by multi-source solid waste carbon mineralization comprises, by weight, at least 40-80 parts of calcium solid waste, 25-55 parts of aggregate, 10-30 parts of ultrafine solid waste, 1-5 parts of fiber, 2-8 parts of modifier, and 10-35 parts of water.
[0060] In some embodiments, the long chain fatty acids have a carbon chain length of C12-C20.
[0061] In some embodiments, the long chain fatty acid is selected from hexadecylmalonic acid (CAS No. 4371-64-6).
[0062] In some embodiments, the ratio of water to the total mass of calcareous solid waste and ultrafine solid waste is 0.05-0.4.
[0063] In some embodiments, the ratio of water to the total mass of calcareous solid waste and ultrafine solid waste is 0.1-0.35.
[0064] In some embodiments, the calcareous solid waste is at least one of steel slag, magnesium slag, calcium-silicon slag, and carbide slag.
[0065] In some embodiments, the calcareous solid waste is steel slag or a combination of steel slag and at least one of magnesium slag, calcium-silicon slag, and carbide slag.
[0066] In some embodiments, the aggregate is at least one of quartz waste, cullet, shells, and metal recycling tailings.
[0067] In some embodiments, the aggregate is quartz waste or a combination of quartz waste and at least one of cullet, shellfish, and metal recycling tailings.
[0068] In some embodiments, the fineness of the ultrafine solid waste is 200-800 mesh.
[0069] In some embodiments, the fineness of the ultrafine solid waste is 300-500 mesh.
[0070] In some embodiments, the fineness of the ultrafine solid waste is 300-400 mesh.
[0071] In some embodiments, the ultrafine solid waste contains calcium oxide.
[0072] In some embodiments, the ultrafine solid waste is selected from at least one of slag powder, steel slag powder, and quartz tailings powder.
[0073] In some embodiments, the ultrafine solid waste is selected from at least one of slag powder and steel slag powder.
[0074] In some embodiments, the fiber is inorganic fiber, plant fiber, synthetic fiber, or a mixture of the two or more thereof.
[0075] In some embodiments, the inorganic fiber is selected from at least one of waste glass fibers and waste carbon fibers; the plant fiber is selected from at least one of sawdust, straw, and bamboo fibers; and the synthetic fiber is selected from at least one of polyamide fibers, polypropylene fibers, and polyacrylonitrile fibers.
[0076] In some embodiments, the fibers are plant fibers.
[0077] In some embodiments, the plant fiber is at least one of sawdust, straw, and bamboo fiber.
[0078] In some embodiments, the raw materials for preparing the carbon-fixing ecological stone obtained by multi-source solid waste carbon mineralization also include a defoaming agent, and the amount of the defoaming agent used is 0.1-0.5wt% of the modifier.
[0079] In some embodiments, the defoaming agent is used in an amount of 0.2-0.3 wt % of the modifier.
[0080] In some embodiments, the defoaming agent is at least one of a polyether defoaming agent, a silicone defoaming agent, and a polyether-modified polysiloxane defoaming agent.
[0081] In some embodiments, the defoaming agent is a polyether-modified polysiloxane defoaming agent, and the defoaming agent is added to eliminate bubbles generated by the modifier during the material stirring process, thereby increasing the tap density of the product.
[0082] In response to the problems of high carbon emissions from raw materials, low product density, poor hardness, high water absorption and poor glossiness of traditional cement-based artificial stones, the present invention has developed a mineralized carbon-fixing ecological stone system, which uses industrial solid waste as raw material to react with industrial flue gas, and the mineralized products improve the density and compressive strength of the product.
[0083] Specifically, the present invention ensures the performance and appearance of mineralized ecological stone by optimizing the solid waste aggregate system in the formula system and coordinating the mineralized solid waste raw material system. On the other hand, by introducing ultrafine solid waste containing calcium oxide, while not affecting the progress of the mineralization reaction and the appearance of the product after polishing, it also helps the modifier in the system to undergo sufficient decarboxylation reaction and generate sufficient fatty acid calcium, fill the pores and interface transition zone of the mineralized product, improve the strength and hydrophobicity, and reduce the water absorption rate of the product; in addition, the present invention introduces at least one fiber from straw, sawdust, and waste glass fibers, which can react with the carboxyl group in the modifier without affecting the mineralization reaction and the final polishing effect, further improve the strength, enhance the toughness of the early green body, and solve the problem of the fragility of the early green body of the mineralization system (unlike cement that will harden naturally).
[0084] Furthermore, the present invention can ensure the occurrence of decarboxylation reaction in the reaction environment by adding 2-8 parts by weight of a modifier in the system, especially controlling the modifier to be a long-chain fatty acid containing two carboxyl groups and the two carboxyl groups are linked to the same carbon atom and the carbon chain length is C12-C20, so as to generate carbon dioxide, so that the inside of the blank can undergo a sufficient mineralization reaction, improve the strength of the product, and play a good hydrophobic role, reducing the water absorption rate of the product. The inventor analyzed that the reason may be: during the mineralization reaction, as the temperature in the reactor increases with the exothermic heat of mineralization, and the calcium oxide contained in the steel slag acts as a catalyst, the modifier undergoes a decarboxylation reaction, removes a carboxyl group and releases CO2, which can cause a sufficient mineralization reaction inside the blank and improve the strength of the product. Moreover, the carboxyl group on the modifier or the product after the decarboxylation reaction (still containing a carboxyl group) can react with the calcium oxide in the system to generate fatty acid calcium, which can not only fill the gaps inside the product and further improve the strength, but also play a good hydrophobic role and reduce the water absorption rate of the product. Monocarboxyl fatty acids (such as stearic acid) do not contain electron-withdrawing groups, and it is difficult for decarboxylation to occur in the environment of this system. They only play a hydrophobic role and cannot produce CO2 to achieve internal mineralization. Short-chain fatty dicarboxylic acids (such as propylmalonic acid) have too short carbon chains. Although they can produce CO2 to achieve internal mineralization, the short-chain fatty acid calcium produced has poor hydrophobic effect.
[0085] In some embodiments, the molding pressure during compression molding in the mold is 30-50 MPa, and the holding time is 2-4 minutes.
[0086] In some embodiments, the vacuum system is turned on while pressing in the mold to extract excess moisture and gas from the blank from the pressing system, and the moisture content after molding is controlled at 6-12%.
[0087] In some embodiments, the moisture content after molding is controlled at 6-8%.
[0088] In some embodiments, the humidity in the kiln for moisturizing curing is 85-95% and the temperature is 50-70°C.
[0089] In some embodiments, the pressure of the mineralization reaction is controlled at 0.4-0.8 MPa, and the reaction time is 6-8 hours.
[0090] In some embodiments, the reaction temperature in the mineralization reactor is controlled to be above 100° C., or the volume of the green body undergoing the mineralization reaction in the mineralization reactor is above 15% of the volume of the reactor, preferably above 18%.
[0091] The carbon-fixing ecological stone prepared according to the above scheme has higher mechanical strength and lower water absorption rate.
[0092] Example 1
[0093] Example 1 of the present invention provides a carbon-fixing ecological stone obtained by carbon mineralization of multi-source solid waste. The raw materials for its preparation include, by weight, 40 parts of calcium solid waste, 25 parts of aggregate, 13 parts of ultrafine solid waste (6 parts of slag powder and 7 parts of steel slag powder), 1.7 parts of fiber (0.7 parts of corn straw and 1 part of wood chips), 3 parts of modifier, 0.0075 parts of defoaming agent, and 16 parts of water.
[0094] The calcareous solid waste is steel slag.
[0095] The aggregate is quartz stone waste.
[0096] The fineness of the ultra-fine solid waste is 300-400 meshes.
[0097] The modifier is hexadecylmalonic acid (CAS No. 4371-64-6).
[0098] The defoamer is a polyether-modified polysiloxane defoamer.
[0099] Embodiment 1 of the present invention provides a method for preparing carbon-fixing ecological stone by multi-source solid waste carbon mineralization, comprising the following steps:
[0100] The calcareous solid waste, aggregate, ultrafine solid waste, fiber and modifier are uniformly mixed to obtain a mixed dry material;
[0101] adding water to the mixed dry materials to obtain a mixed slurry;
[0102] The mixed slurry is put into the mold and pressed by a press. The molding pressure is 40MPa and the pressure holding time is 3 minutes. The vacuum system is turned on while pressing to extract the excess moisture and gas of the green body from the pressing system. The moisture content after molding is controlled at 7%. After molding, the green body is pushed out by the press to obtain the green body.
[0103] Move the green body to the curing kiln for moisturizing curing, with the humidity in the kiln at 90% and the temperature at 60°C;
[0104] After the moisturizing and curing, the green body is moved to the mineralization reactor for mineralization reaction, the pressure is controlled at 0.6MPa, and the reaction time is 7h to obtain the plate;
[0105] The slabs are subjected to thickness-setting, polishing and grinding treatments to obtain ecological stone slabs with high surface gloss, and then surface protection treatments are performed to obtain finished products.
[0106] The volume of the green body undergoing the mineralization reaction in the mineralization reactor is 30% of the inner volume of the reactor.
[0107] Example 2
[0108] Example 2 of the present invention provides a carbon-fixing ecological stone obtained by carbon mineralization of multi-source solid waste. The raw materials for its preparation include, by weight, 60 parts of calcium solid waste, 40 parts of aggregate, 18 parts of ultrafine solid waste (6 parts of slag powder and 12 parts of steel slag powder), 3 parts of fiber (1 part of corn straw and 2 parts of sawdust), 5 parts of modifier, 0.015 parts of defoaming agent, and 24 parts of water.
[0109] The calcareous solid waste is steel slag.
[0110] The aggregate is quartz stone waste.
[0111] The fineness of the ultra-fine solid waste is 300-400 meshes.
[0112] The modifier is hexadecylmalonic acid (CAS No. 4371-64-6).
[0113] The defoamer is a polyether-modified polysiloxane defoamer.
[0114] The preparation method is the same as Example 1.
[0115] Example 3
[0116] Example 3 of the present invention provides a carbon-fixing ecological stone obtained by carbon mineralization of multi-source solid waste. The raw materials for its preparation include, by weight, 80 parts of calcium solid waste, 53 parts of aggregate, 25 parts of ultrafine solid waste (15 parts of slag powder and 10 parts of steel slag powder), 4.5 parts of fiber (4.5 parts of sawdust), 7 parts of modifier, 0.014 parts of defoaming agent, and 35 parts of water.
[0117] The calcareous solid waste is steel slag.
[0118] The aggregate is quartz stone waste.
[0119] The fineness of the ultra-fine solid waste is 300-400 meshes.
[0120] The modifier is hexadecylmalonic acid (CAS No. 4371-64-6).
[0121] The defoamer is a polyether-modified polysiloxane defoamer.
[0122] The preparation method is the same as Example 1.
[0123] Example 4
[0124] Example 4 of the present invention provides a carbon-fixing ecological stone mineralized from multi-source solid waste carbon. The formula is the same as that of Example 2, and the preparation method is different from that of Example 2 in that the volume of the green body undergoing the mineralization reaction in the mineralization reactor is 40% of the volume of the reactor.
[0125] Example 5
[0126] Example 5 of the present invention provides a carbon-fixing ecological stone mineralized from multi-source solid waste carbon. The formula is the same as that of Example 2, and the preparation method is different from that of Example 2 in that the volume of the green body undergoing the mineralization reaction in the mineralization reactor is 50% of the internal volume of the reactor.
[0127] Example 6
[0128] Example 6 of the present invention provides a carbon-fixing ecological stone mineralized from multi-source solid waste carbon. The formula is the same as that of Example 2, and the preparation method is different from that of Example 2 in that the volume of the green body undergoing the mineralization reaction in the mineralization reactor is 18% of the volume of the reactor.
[0129] Example 7
[0130] Example 7 of the present invention provides a carbon-fixing ecological stone mineralized from multi-source solid waste carbon. The formula is the same as that of Example 2, and the preparation method is different from that of Example 2 in that the volume of the green body undergoing the mineralization reaction in the mineralization reactor is 15% of the internal volume of the reactor.
[0131] Example 8
[0132] Example 8 of the present invention provides a carbon-fixing ecological stone obtained by mineralizing multi-source solid waste carbon. The formula is different from that of Example 2 in that the fibers are replaced by waste glass fibers, and the preparation method is the same as that of Example 2.
[0133] Example 9
[0134] Example 9 of the present invention provides a carbon-fixing ecological stone obtained by mineralizing carbon from multi-source solid waste. The difference between the formula and that of Example 2 is that the modifier is replaced by propylmalonic acid, and the preparation method is the same as that of Example 2.
[0135] Comparative Example 1
[0136] Comparative Example 1 of the present invention provides a carbon-fixing ecological stone obtained by carbon mineralization of multi-source solid waste. The difference between the formula and that of Example 2 is that the ultrafine solid waste is replaced by quartz tailings powder, and the preparation method is the same as that of Example 2.
[0137] Comparative Example 2
[0138] Comparative Example 2 of the present invention provides a carbon-fixing ecological stone obtained by multi-source solid waste carbon mineralization. The formula is different from that of Example 2 in that, by weight, the raw materials for its preparation include 65 parts of calcium solid waste, 40 parts of aggregate, 18 parts of ultrafine solid waste (6 parts of slag powder and 12 parts of steel slag powder), 3 parts of fiber (1 part of corn straw and 2 parts of sawdust), 0.015 parts of defoaming agent, and 24 parts of water. The preparation method is the same as that of Example 2.
[0139] Comparative Example 3
[0140] Comparative Example 3 of the present invention provides a carbon-fixing ecological stone obtained by mineralizing carbon from multi-source solid waste. The difference between the formula and that of Example 2 is that the modifier is replaced by stearic acid, and the preparation method is the same as that of Example 2.
[0141] Comparative Example 4
[0142] Comparative Example 4 of the present invention provides a carbon-fixing ecological stone obtained by mineralizing carbon from multi-source solid waste. The difference between the formula and that of Example 2 is that the modifier is replaced by calcium stearate, and the preparation method is the same as that of Example 2.
[0143] Performance Testing
[0144] The flexural strength, compressive strength and water absorption rate of the carbon-fixing ecological stone obtained by mineralizing multi-source solid waste carbon provided in the embodiments and comparative examples were tested. The test methods are as follows. The test results are shown in Table 1.
[0145] With reference to JC / T2604-2021 "Stone-like concrete panels and facing bricks", the flexural strength and compressive strength of the eco-stones obtained in each embodiment and comparative example were tested. With reference to GB / T4111-2013 "Test methods for concrete blocks and bricks", the water absorption rate of the eco-stones obtained in each embodiment and comparative example was tested.
[0146] Table 1
[0147]
[0148] The data in Table 1 show that the eco-stone products prepared in Examples 1-9 of the present application have high compressive strength and flexural strength, low water absorption and excellent performance.
[0149] Compared with Example 2, Examples 4 and 5 have improved flexural strength and compressive strength. The reason may be that the volume ratio increases, the exothermic degree of the mineralization reaction combined with the space in the reactor increases the temperature in the reactor, which is conducive to the full reaction of the modifier to release more carbon dioxide, improve the internal mineralization degree, and improve the strength.
[0150] Compared with Example 2, Examples 6 and 7 have decreased flexural strength and compressive strength, and increased water absorption. The reasons may be that the volume share is reduced, the exothermic degree of the mineralization reaction combined with the space in the reactor makes the temperature in the reactor lower, affecting the decarboxylation reaction and the reaction of generating insoluble substances similar to calcium stearate that can improve the impermeability, resulting in a decrease in strength and an increase in water absorption.
[0151] Compared with Example 2, Example 8 has decreased flexural strength and compressive strength. This may be mainly attributed to the fact that straw and wood chips contain a large amount of hydroxyl groups, which can bond with the carboxyl groups in the modifier, thus helping to improve the strength of the system. The glass fibers have a small amount of hydroxyl groups and contribute less to the strength.
[0152] Compared with Example 2, Example 9 has an increased strength, but also an increased water absorption rate. This may be because the carbon chain of propylmalonic acid is shorter. Although it can generate more carbon dioxide to enhance internal mineralization and increase strength, the hydrophobic effect of the short chain is not as good as that of the long chain, so the hydrophobic effect is reduced.
[0153] Comparative Example 1 is relative to Example 2: the flexural strength and compressive strength decrease, and the water absorption rate increases. This may be because calcium oxide is a catalyst for the decarboxylation reaction and the main component for generating fatty acid calcium (water repellent). The calcium oxide content in steel slag itself is relatively small, and both slag powder and steel slag powder contain calcium oxide, which can be supplemented. Quartz tailings powder basically does not contain free calcium oxide, which is not conducive to the decarboxylation reaction and the generation of water repellent, and affects both the strength and water absorption rate.
[0154] Compared with Example 2, the flexural strength and compressive strength of Comparative Example 2 are significantly reduced, and the water absorption rate is significantly increased. This is because without adding a modifier, carbon dioxide cannot be generated by reaction inside the blank, the interior is difficult to mineralize, the strength is significantly reduced, and a hydrophobic agent similar to calcium stearate cannot be generated, and the water absorption rate is significantly increased.
[0155] The strength of Comparative Example 3 is significantly reduced relative to Example 2. This may be because stearic acid has no electron-withdrawing groups in its structure. Under the conditions of mineralization self-heating, it is difficult to undergo a decarboxylation reaction to generate carbon dioxide internally. However, calcium stearate can be generated to fill the gaps, increase strength, and have a hydrophobic effect. Therefore, the strength is significantly reduced, but it is still better than Comparative Example 2. In addition, stearic acid can bond with the fiber hydroxyl groups, so the strength is better than Comparative Example 4.
[0156] The strength of Comparative Example 4 is significantly reduced relative to Example 2, which may be due to the inability to generate carbon dioxide internally. However, calcium stearate can fill the gaps, increase the strength, and play a hydrophobic role. Therefore, the strength is significantly reduced, but it is still better than Comparative Example 2 and worse than Comparative Example 3.
Claims
1. A carbon-fixing ecological stone for multi-source solid waste carbon mineralization, It is characterized in that The raw materials for its preparation include at least 40-80 parts of calcareous solid waste, 20-55 parts of aggregate, 10-30 parts of ultrafine solid waste, 1-5 parts of fiber, 1-10 parts of modifier, and 5-40 parts of water by weight; the modifier is a long-chain fatty acid containing two carboxyl groups and the two carboxyl groups are connected to the same carbon atom; the ultrafine solid waste is selected from at least one of slag micropowder and steel slag micropowder; the fineness of the ultrafine solid waste is 200-800 mesh.
2. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 1, It is characterized in that The amount of the modifier used is 2-8 parts by weight.
3. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 1, It is characterized in that The carbon chain length of the long-chain fatty acid is C 12 -C 20 .
4. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 3, It is characterized in that The long-chain fatty acid is selected from hexadecylmalonic acid.
5. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 1, It is characterized in that The calcareous solid waste is selected from at least one of steel slag, magnesium slag, calcium silicate slag and carbide slag; the aggregate is at least one of quartz waste, broken glass, shells and metal recycling tailings.
6. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 1, It is characterized in that The fiber is one or a mixture of inorganic fiber, plant fiber, and synthetic fiber; the inorganic fiber is selected from at least one of waste glass fiber and waste carbon fiber; the plant fiber is selected from at least one of sawdust, straw, and bamboo fiber; the synthetic fiber is selected from at least one of polyamide fiber, polypropylene fiber, and polyacrylonitrile fiber.
7. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 1, It is characterized in that The fiber is plant fiber; the plant fiber is at least one of sawdust, straw and bamboo fiber.
8. The carbon-fixing ecological stone for multi-source solid waste carbon mineralization according to claim 1, It is characterized in that The calcareous solid waste at least includes steel slag; the ultrafine solid waste contains calcium oxide; and the aggregate at least includes quartz stone waste.
9. A method for preparing carbon-fixing ecological stone by multi-source solid waste carbon mineralization according to any one of claims 1 to 8, It is characterized in that At least the following steps are included: The calcareous solid waste, aggregate, ultrafine solid waste, fiber and modifier are uniformly mixed to obtain a mixed dry material; adding water to the mixed dry materials to obtain a mixed slurry; The mixed slurry is put into a mold and pressed by a press, the molding pressure is 10-60MPa, the pressure holding time is 1-5 minutes, and after molding, the green body is pushed out by the press to obtain a green body; Move the green body to the curing kiln for moisturizing curing, with the humidity in the kiln at 70-95% and the temperature at 40-80℃; After the moisturizing and curing, the green body is moved to a mineralization reactor for mineralization reaction, the reaction pressure is controlled at 0.2-0.8MPa, the reaction time is 2-10h, and the plate is obtained; The plate is subjected to thickness setting, polishing and grinding to obtain carbon-fixing ecological stone with high surface gloss, and then surface protection treatment is performed to obtain the finished product.
10. The method for preparing carbon-fixing ecological stone by multi-source solid waste carbon mineralization according to claim 9, It is characterized in that The reaction temperature in the mineralization reactor is controlled to be above 100° C., or the volume of the green body undergoing the mineralization reaction in the mineralization reactor is above 15% of the inner volume of the reactor.