High-strength flame-retardant TPU material and preparation method thereof

By using ionic liquids and flame retardants in TPU materials, the problems of flammability and poor compatibility of TPU materials are solved, high-strength flame retardant effect and improved mechanical properties are achieved, and the charging pile cables of new energy vehicles are met security requirements.

CN118459715BActive Publication Date: 2024-11-12SHANDONG INOV POLYURETHANE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925501.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The existing TPU materials are flammable and have poor compatibility between flame retardants and polymer matrix, resulting in poor flame retardant effect and a great impact on the mechanical properties of the materials. It is necessary to develop high-strength flame retardant TPU materials to meet the charging of new energy vehicles. Safety requirements for pile cables.

Method used

Using ionic liquid as a synergist, synergistically works with flame retardant, improves the compatibility and mechanical properties of TPU materials by exerting flame retardant in the condensed phase and gas phase, and inhibits free radicals through the pyrolysis of cations and anions. Reaction, a dense carbon layer is formed to prevent combustion.

Benefits of technology

It significantly improves the flame retardant effect, thermal stability and mechanical properties of TPU materials, reduces smoke release and toxic gas production, achieves the effect of reaching the V-0 flame retardant level with a lower addition amount, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The present invention discloses a high-strength flame-retardant TPU material and a preparation method thereof, and relates to the technical field of polyurethane elastomers. Its technical scheme is: comprising the following components by mass: 45-67 parts of diols, 29-43 parts of isocyanates, 4-12 parts of chain extenders, 0.2-0.8 parts of synergists, 0.4-0.9 parts of flame retardants, 0.1-0.4 parts of antioxidants, 0.1-0.25 parts of hydrolysis-resistant agents, 0.03-0.12 parts of catalysts, and 0.1-0.25 parts of ultraviolet absorbers; the synergist is an ionic liquid. The present invention uses an ionic liquid as a synergist, and utilizes its synergistic effect with a flame retardant to solve the problem of poor dispersion compatibility and easy precipitation between a flame retardant and a polymer matrix, thereby improving the flame retardant effect of the TPU material and improving the thermal stability and mechanical properties of the TPU material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane elastomers, and in particular to a high-strength flame-retardant TPU material and a preparation method thereof. Background Art

[0002] With the popularization of new energy vehicles, charging pile cables, as important supporting facilities for new energy vehicles, have higher requirements for the use environment and safety compared with traditional cable materials. Therefore, higher requirements are also placed on the covering materials of charging pile cables.

[0003] As a new type of elastomer material, thermoplastic polyurethane elastomer (TPU) has a wide hardness range compared to other materials, and has good comprehensive performance in terms of wear resistance, elasticity and mechanical properties. It is an excellent base material for cable sheaths. However, TPU itself is a flammable material. In order to achieve a sufficient flame retardant effect, a large amount of halogen-free flame retardant needs to be added. Although this type of flame retardant can inhibit combustion or slow down the spread of flames, a large amount of addition will have a great impact on the mechanical properties of the material, and the compatibility between fillers and polymers is generally poor, which makes liquid flame retardants easy to precipitate. In addition, the heat resistance and mechanical properties of TPU materials also need to be further improved. In summary, it is urgent to develop a new high-strength flame-retardant TPU material to solve the above problems. Summary of the invention

[0004] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art, to provide a high-strength flame-retardant TPU material and a preparation method thereof, to use ionic liquid as a synergist, to utilize its synergistic effect with the flame retardant, to solve the problem of poor dispersion compatibility and easy precipitation between the flame retardant and the polymer matrix, to enhance the flame retardant effect of the TPU material, and to improve the thermal stability and mechanical properties of the TPU material.

[0005] The technical solution of the present invention is:

[0006] In one aspect, the present invention provides a high-strength flame-retardant TPU material, comprising the following components in parts by weight:

[0007] 45-67 parts of diol

[0008] Isocyanate 29-43 parts

[0009] Chain extender 4-12 parts

[0010] Synergist 0.2-0.8 parts

[0011] Flame retardant 0.4-0.9 parts

[0012] Antioxidant 0.1-0.4 parts

[0013] Anti-hydrolysis agent 0.1-0.25 parts

[0014] Catalyst 0.03-0.12 parts

[0015] 0.1-0.25 parts of ultraviolet absorber;

[0016] The synergist is an ionic liquid, and the preparation method thereof is as follows: tetrabutylphosphine chloride and sodium 2-naphthalenesulfonate (NSS) are dissolved in deionized water at a molar ratio of (1-1.5): (1-1.5), respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 20-30° C. for 11-16 hours for reaction, and after the reaction is completed, dichloromethane is added to extract the mixed aqueous solution, and the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 100-110° C. for 10-15 hours to obtain the synergist; the reaction formula is as follows:

[0017] .

[0018] Preferably, the diol is one or both of polycaprolactone diol (PCL) and polytetramethylene ether glycol (PTMG).

[0019] Preferably, the number average molecular weight of the diol is 1000-2500.

[0020] Preferably, the isocyanate is diphenylmethane diisocyanate (MDI).

[0021] Preferably, the chain extender is 1,4-butanediol (BDO) and 2-methyl-1,3-propanediol (MPO).

[0022] Preferably, in the chain extender, the mass percentage of 1,4-butanediol (BDO) is 90-99%.

[0023] The present invention uses a mixture of isomeric BDO and a small amount of MPO as a composite chain extender, which can improve the transparency of the TPU material while ensuring the mechanical properties of the TPU material. At the same time, when the amount of MPO added is too much, on the one hand, the mechanical properties of the TPU material will be reduced, and on the other hand, its price is high, which will also increase the product preparation cost.

[0024] Preferably, the flame retardant is triphenyl phosphate (TPP), triethyl phosphate (TEP), tricresyl phosphate (TCP), resorcinol bis(diphenyl phosphate) (RDP), toluene diphenyl phosphate (CDP) or bisphenol A bis(diphenyl phosphate) (BDP).

[0025] Preferably, the antioxidant is tris(2,4-di-tert-butylphenyl) phosphite (Antioxidant 168), poly(dipropylene glycol) phenyl phosphite (PDP) or diphenyl isodecyl phosphite; the anti-hydrolysis agent is carbodiimide; and the catalyst is stannous octoate.

[0026] Preferably, the ultraviolet absorber is N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine (UV-1), N-(ethoxycarbonylphenyl)-N'-ethyl-N'-phenylformamidine (UV-2), 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2,4-dihydroxybenzophenone (UV-0), 2-hydroxy-4-methoxybenzophenone (UV-9) or 2-hydroxy-4-octyloxybenzophenone (UV-531).

[0027] On the other hand, the present invention provides a method for preparing the above-mentioned high-strength flame-retardant TPU material. The synergist, flame retardant, antioxidant, hydrolysis resistance agent and ultraviolet absorber are first added to the diol, stirred evenly, and then added into zone 1 of a twin-screw extruder together with isocyanate, chain extender and catalyst to carry out a continuous polymerization reaction. After underwater granulation, aging and drying, a high-strength flame-retardant TPU material is obtained.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The present invention synthesizes a new ionic liquid with good thermal stability, non-flammability and low volatility. The ionic liquid is used as a synergist to play a synergistic role with the flame retardant. The two are used simultaneously to have both condensed phase and gas phase flame retardant effects. In the condensed phase, cations are pyrolyzed to generate compounds containing PC and POC bonds, anions are pyrolyzed to generate sulfonic acid compounds, and flame retardants are pyrolyzed to generate phosphoric acid and its derivatives, which promote the dehydration of TPU to form a dense and stable carbon layer, which not only isolates the transfer of heat, combustible substances and oxygen, but also reduces smoke release and inhibits the generation of toxic gases such as CO. In the gas phase, cations and flame retardants form during the thermal decomposition process. and , anions generate sulfur-containing free radicals, quenching the active free radicals and , preventing chain free radical reactions, thus achieving the purpose of synergistic flame retardancy. The increase in the chain length of the alkyl substituent in the ionic liquid can promote compatibility with TPU, solve the problem of poor dispersion compatibility and easy precipitation between the flame retardant and the polymer matrix, and achieve a V-0 flame retardant effect with a small amount of addition, thereby improving the flame retardant properties of the TPU material and enhancing the thermal stability and mechanical properties of the TPU material. DETAILED DESCRIPTION

[0030] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0031] The raw materials used in the examples of the present invention, unless otherwise specified, are all commercially available conventional raw materials; the process methods used in the examples, unless otherwise specified, are all conventional methods in the art.

[0032] The PTMG-1800, PTMG-2000 and PTMG-2500 used in the examples have number average molecular weights of 1800, 2000 and 2500, respectively, and are provided by BASF AG.

[0033] The PCL-1500 and PCL-1000 used in the examples have number average molecular weights of 1500 and 1000, respectively, and are provided by Hunan Juren New Materials Co., Ltd.

[0034] Example 1

[0035] The high-strength flame-retardant TPU material of this embodiment includes the following components in parts by mass:

[0036] PTMG-2000: 45 parts

[0037] MDI: 43 parts

[0038] BDO: 10.8 parts

[0039] MPO: 1.2 parts

[0040] Ionic liquid: 0.2 parts

[0041] BDP: 0.4 parts

[0042] Antioxidant 168: 0.1 parts

[0043] Carbodiimide: 0.1 parts

[0044] Stannous octoate: 0.03 parts

[0045] UV-2: 0.1 parts.

[0046] Among them, the preparation method of the ionic liquid of this embodiment is: tetrabutylphosphine chloride and NSS are dissolved in 1L of deionized water in a molar ratio of 1:1, respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 20°C for 11h to react. After the reaction, 3L of dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 100°C for 10h to obtain an ionic liquid.

[0047] The preparation method of the high-strength flame-retardant TPU material of this embodiment is as follows:

[0048] First, add ionic liquid, BDP, antioxidant 168, carbodiimide and UV-2 to PTMG-2000, stir evenly and pour them into zone 1 of twin-screw extruder with MDI, BDO and MPO through a pouring machine for continuous polymerization. Stannous octoate is added into zone 1 of twin-screw extruder by a pouring machine (Wuyi Henghui Polyurethane Equipment Factory, model TPU-MS); after underwater cutting and granulation, aging and drying, high-strength flame-retardant TPU material is obtained.

[0049] The twin-screw extruder is divided into twelve temperature zones. The temperatures from the first zone to the twelfth zone are 160℃, 200℃, 200℃, 205℃, 205℃, 195℃, 185℃, 180℃, 160℃, 160℃, 160℃, 160℃; the die outlet temperature is 225℃; the main engine speed is 180r / min.

[0050] Example 2

[0051] The high-strength flame-retardant TPU material of this embodiment includes the following components in parts by mass:

[0052] PTMG-2500: 67 parts

[0053] MDI: 29 parts

[0054] BDO: 3.76 parts

[0055] MPO: 0.24 parts

[0056] Ionic liquid: 0.8 parts

[0057] RDP: 0.9 copies

[0058] PDP: 0.4 parts

[0059] Carbodiimide: 0.25 parts

[0060] Stannous octoate: 0.12 parts

[0061] UV-1: 0.25 parts.

[0062] Among them, the preparation method of the ionic liquid of this embodiment is: tetrabutylphosphine chloride and NSS are dissolved in 1L of deionized water in a molar ratio of 1:1.5, respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 26°C for 12h to react. After the reaction, 3L of dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 106°C for 11h to obtain an ionic liquid.

[0063] The preparation method of the high-strength flame-retardant TPU material of this embodiment is as follows:

[0064] First, add ionic liquid, RDP, PDP, carbodiimide and UV-1 to PTMG-2500, stir evenly and then pour them into zone 1 of the twin-screw extruder with MDI, BDO and MPO through a pouring machine for continuous polymerization. Stannous octoate is added to zone 1 of the twin-screw extruder by a pouring machine (Wuyi Henghui Polyurethane Equipment Factory, model TPU-MS); after underwater cutting and granulation, aging and drying, a high-strength flame-retardant TPU material is obtained.

[0065] The twin-screw extruder is divided into twelve temperature zones. The temperatures from the first zone to the twelfth zone are 120℃, 205℃, 210℃, 210℃, 210℃, 190℃, 180℃, 170℃, 165℃, 165℃, 165℃, and 165℃ respectively; the die outlet temperature is 220℃; and the main engine speed is 220r / min.

[0066] Example 3

[0067] The high-strength flame-retardant TPU material of this embodiment includes the following components in parts by mass:

[0068] PCL-1000: 55 copies

[0069] MDI: 39 parts

[0070] BDO: 5.76 parts

[0071] MPO: 0.24 parts

[0072] Ionic liquid: 0.3 parts

[0073] TPP: 0.6 parts

[0074] Isodecyl diphenyl phosphite: 0.2 parts

[0075] Carbodiimide: 0.15 parts

[0076] Stannous octoate: 0.05 parts

[0077] UV-0: 0.15 parts.

[0078] Among them, the preparation method of the ionic liquid of this embodiment is: tetrabutylphosphine chloride and NSS are dissolved in 1L of deionized water in a molar ratio of 1.5:1, respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 30°C for 13h to react. After the reaction, 3L of dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 110°C for 12h to obtain an ionic liquid.

[0079] The preparation method of the high-strength flame-retardant TPU material of this embodiment is as follows:

[0080] First, add ionic liquid, TPP, diphenyl isodecyl phosphite, carbodiimide, and UV-0 to PCL-1000, stir evenly, and then pour into the first zone of the twin-screw extruder with MDI, BDO, and MPO through a pouring machine for continuous polymerization. Stannous octoate is added to the first zone of the twin-screw extruder by a pouring machine (Wuyi Henghui Polyurethane Equipment Factory, model TPU-MS); after underwater cutting and granulation, aging and drying, a high-strength flame-retardant TPU material is obtained.

[0081] The twin-screw extruder is divided into twelve temperature zones. The temperatures from the first zone to the twelfth zone are 140℃, 195℃, 195℃, 200℃, 200℃, 180℃, 180℃, 175℃, 155℃, 155℃, 155℃, and 155℃ respectively; the die outlet temperature is 230℃; and the main engine speed is 190r / min.

[0082] Example 4

[0083] The high-strength flame-retardant TPU material of this embodiment includes the following components in parts by mass:

[0084] PCL-1500: 60 copies

[0085] MDI: 32 parts

[0086] BDO: 7.84 parts

[0087] MPO: 0.16 parts

[0088] Ionic liquid: 0.4 parts

[0089] TCP: 0.8

[0090] Antioxidant 168: 0.3 parts

[0091] Carbodiimide: 0.2 parts

[0092] Stannous octoate: 0.08 parts

[0093] UV-9: 0.2 parts.

[0094] Among them, the preparation method of the ionic liquid of this embodiment is: tetrabutylphosphine chloride and NSS are dissolved in 1L of deionized water in a molar ratio of 1:1.2, respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 22°C for 14h to react. After the reaction, 3L of dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 102°C for 13h to obtain an ionic liquid.

[0095] The preparation method of the high-strength flame-retardant TPU material of this embodiment is as follows:

[0096] First, add ionic liquid, TCP, antioxidant 168, carbodiimide, and UV-9 to PCL-1500, stir evenly, and then pour them into the first zone of the twin-screw extruder with MDI, BDO, and MPO through a pouring machine for continuous polymerization. Stannous octoate is added to the first zone of the twin-screw extruder by a pouring machine (Wuyi Henghui Polyurethane Equipment Factory, model TPU-MS); after underwater cutting and granulation, aging and drying, a high-strength flame-retardant TPU material is obtained.

[0097] The twin-screw extruder is divided into twelve temperature zones. The temperatures from the first zone to the twelfth zone are 110℃, 160℃, 190℃, 205℃, 210℃, 210℃, 190℃, 175℃, 170℃, 150℃, 150℃, and 150℃ respectively; the die outlet temperature is 215℃; and the main engine speed is 195r / min.

[0098] Example 5

[0099] The high-strength flame-retardant TPU material of this embodiment includes the following components in parts by mass:

[0100] PTMG-1800: 50 parts

[0101] MDI: 40 parts

[0102] BDO: 9.2 parts

[0103] MPO: 0.8 parts

[0104] Ionic liquid: 0.6 parts

[0105] TEP: 0.5 parts

[0106] PDP: 0.35 parts

[0107] Carbodiimide: 0.16 parts

[0108] Stannous octoate: 0.1 part

[0109] UV-P: 0.18 parts.

[0110] Among them, the preparation method of the ionic liquid of this embodiment is: tetrabutylphosphine chloride and NSS are dissolved in 1L of deionized water in a molar ratio of 1.2:1, respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 24°C for 15h to react. After the reaction, 3L of dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 104°C for 14h to obtain an ionic liquid.

[0111] The preparation method of the high-strength flame-retardant TPU material of this embodiment is as follows:

[0112] First, add ionic liquid, TEP, PDP, carbodiimide and UV-P to PTMG-1800, stir evenly and pour them into zone 1 of twin-screw extruder with MDI, BDO and MPO through a pouring machine for continuous polymerization. Stannous octoate is added into zone 1 of twin-screw extruder by a pouring machine (Wuyi Henghui Polyurethane Equipment Factory, model TPU-MS); after underwater cutting and granulation, aging and drying, high-strength flame-retardant TPU material is obtained.

[0113] The twin-screw extruder is divided into twelve temperature zones. The temperatures from the first zone to the twelfth zone are 130℃, 190℃, 195℃, 200℃, 205℃, 205℃, 185℃, 185℃, 175℃, 145℃, 145℃, and 145℃ respectively; the die outlet temperature is 235℃; and the main engine speed is 200r / min.

[0114] Example 6

[0115] The high-strength flame-retardant TPU material of this embodiment includes the following components in parts by mass:

[0116] PTMG-1800: 27 parts

[0117] PCL-1500: 27 copies

[0118] MDI: 37 parts

[0119] BDO: 8.91

[0120] MPO: 0.09 parts

[0121] Ionic liquid: 0.5 parts

[0122] CDP: 0.7

[0123] Isodecyl diphenyl phosphite: 0.25 parts

[0124] Carbodiimide: 0.18 parts

[0125] Stannous octoate: 0.07 parts

[0126] UV-531: 0.14 parts.

[0127] Among them, the preparation method of the ionic liquid of this embodiment is: tetrabutylphosphine chloride and NSS are dissolved in 1L of deionized water in a molar ratio of 1:1.35, respectively, and stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, and stirred at 28°C for 16h to react. After the reaction, 3L of dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 108°C for 15h to obtain an ionic liquid.

[0128] The preparation method of the high-strength flame-retardant TPU material of this embodiment is as follows:

[0129] First, add ionic liquid, CDP, diphenyl isodecyl phosphite, carbodiimide, and UV-531 to PTMG-1800 and PCL-1500, stir evenly, and then pour into the first zone of the twin-screw extruder with MDI, BDO, and MPO through a pouring machine for continuous polymerization. Stannous octoate is added to the first zone of the twin-screw extruder by a pouring machine (Wuyi Henghui Polyurethane Equipment Factory, model TPU-MS); after underwater cutting and granulation, aging and drying, a high-strength flame-retardant TPU material is obtained.

[0130] The twin-screw extruder is divided into twelve temperature zones. The temperatures from the first zone to the twelfth zone are 150℃, 210℃, 210℃, 210℃, 200℃, 180℃, 170℃, 160℃, 140℃, 140℃, 140℃, 140℃; the die outlet temperature is 210℃; the main engine speed is 230r / min.

[0131] Comparative Example 1

[0132] The difference from Example 1 is that no ionic liquid is added.

[0133] Comparative Example 2

[0134] The difference from Example 1 is that an equal amount of 1-ethyl-3-methylimidazolium bromide is used to replace the ionic liquid in Example 1.

[0135] Comparative Example 3

[0136] The difference from Example 1 is that no ionic liquid is added and the mass fraction of BDP is 33 parts.

[0137] Comparative Example 4

[0138] The difference from Example 1 is that no BDP was added.

[0139] Comparative Example 5

[0140] The difference from Example 1 is that an equal amount of MPO is used to replace the BDO in Example 1.

[0141] Comparative Example 6

[0142] The difference from Example 1 is that an equal amount of BDO is used to replace the MPO in Example 1.

[0143] Comparative Example 7

[0144] The difference from Example 1 is that the mass fraction of the ionic liquid is 5 parts.

[0145] Comparative Example 8

[0146] The difference from Example 1 is that the mass fraction of BDP is 6 parts.

[0147] The TPU materials prepared in Examples 1-6 and Comparative Examples 1-8 were subjected to performance tests, wherein:

[0148] The tensile strength, elongation at break and 100% elongation stress are tested according to the standard "ASTM-D412 Standard Test Method for Tension of Vulcanized Rubber and Thermoplastic Elastomers";

[0149] The tear strength is tested according to the standard "ASTM-D624 Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers";

[0150] The flame retardancy level is tested according to the UL94 vertical burning test method, and the flame retardancy levels are V-0, V-1, and V-2 from high to low;

[0151] The limiting oxygen index (LOI) is tested in accordance with GB / T 2406.2-2009 Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test, and the sample size is 120mm×6mm×4mm;

[0152] The light transmittance was tested using a color spectrum spectrophotometer CS-820. The specific method was as follows: the TPU material was injection molded into a 2mm thick test piece, and the light transmittance of the test piece was tested;

[0153] The test conditions for precipitation are as follows: place the sample at 80°C for 168 hours, take it out and place it at room temperature for 4 hours, observe and record the precipitation on the sample surface, and divide it into three levels according to the precipitation amount: no precipitation, slight precipitation, and obvious precipitation;

[0154] The test conditions for high temperature aging resistance are: place the sample at 100°C for 168 hours, take it out and let it stand at room temperature for 2 hours, and test the change rate of its tensile strength and elongation at break.

[0155] The performance test results are shown in Table 1:

[0156] Table 1 Performance test results of TPU materials prepared in Examples 1-6 and Comparative Examples 1-8

[0157]

[0158] As can be seen from Table 1, the ionic liquids in Examples 1-6 act as synergists, play a synergistic role with the flame retardant, and react together into TPU. The prepared TPU materials have high flame retardancy, good mechanical properties, high transparency, good heat resistance and no precipitation. Compared with Example 1, Comparative Example 1 does not add ionic liquid as a synergist, the flame retardancy of the prepared TPU material is reduced and there is precipitation, and the high temperature aging resistance is poor. This is because the ionic liquid added in Example 1 has a naphthalene ring structure, the rigidity of the chain segment is increased, microphase separation occurs, and it contains inorganic elements, which is beneficial to improve the high temperature aging resistance of the TPU material. Comparative Example 2 uses commercially available ionic liquids instead of the ionic liquid synthesized in Example 1, and the flame retardancy of the prepared TPU material is reduced. This is because the F element in the ionic liquid is unevenly distributed, which results in the flame retardant element not being able to fully exert its flame retardant effect in TPU, and the heat release of TPU during combustion cannot be alleviated. During the combustion process, the decomposition of TPU is promoted and flammable gas is generated, so the flame retardancy is reduced. In Comparative Example 3, no ionic liquid is added. Therefore, in order to achieve the same flame retardant effect, the amount of flame retardant added is much larger, but adding too much flame retardant will lead to a decrease in the mechanical properties of the TPU material and obvious precipitation. In Comparative Example 4, no flame retardant is added. The mechanical properties of the prepared TPU material are slightly improved, but the flame retardant grade is reduced. In Comparative Example 5, only a single component MPO is used as the chain extender. The mechanical properties of the prepared TPU material are reduced and the transmittance is increased. This is because there are isomers in the MDI / MPO hard segment structure, forming an irregular hard segment structure that limits the crystallization of TPU, the crystallinity is low, and the transparency is improved. In Comparative Example 6, only a single component BDO is used as the chain extender. The transmittance of the prepared TPU material is reduced. This is because the MDI / BDO hard segment structure is regular, the phase separation is good, and it is easy to crystallize. The prepared TPU has a high crystallinity and poor transparency. In Comparative Example 7, the amount of ionic liquid added is too much, and in Comparative Example 8, the amount of flame retardant added is too much. The flame retardant grade of the prepared TPU material remains unchanged, but the mechanical properties are reduced. This is because the excessive ionic liquid and flame retardant expand the intermolecular distance, reduce the intermolecular electrostatic attraction and crystallinity, and weaken the interaction between the molecular chains, thereby causing the mechanical properties of the TPU material to decrease.

Claims

1. High-strength flame-retardant TPU material, characterized by: The composition includes the following components in parts by weight: 45-67 parts of diol Isocyanate 29-43 parts Chain extender 4-12 parts Synergist 0.2-0.8 parts Flame retardant 0.4-0.9 parts Antioxidant 0.1-0.4 parts Anti-hydrolysis agent 0.1-0.25 parts Catalyst 0.03-0.12 parts 0.1-0.25 parts of ultraviolet absorber; The synergist is an ionic liquid, and the preparation method thereof is as follows: tetrabutylphosphine chloride and sodium 2-naphthalenesulfonate are dissolved in deionized water in a molar ratio of (1-1.5): (1-1.5) respectively, stirred until completely dissolved to obtain two aqueous solutions, the two aqueous solutions are mixed, stirred at 20-30°C for 11-16 hours for reaction, and after the reaction is completed, dichloromethane is added to extract the mixed aqueous solution, the extract is washed with deionized water and then rotary evaporated, and vacuum dried at 100-110°C for 10-15 hours to obtain the synergist.

2. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The diol is one or both of polycaprolactone diol and polytetramethylene ether glycol.

3. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The number average molecular weight of the diol is 1000-2500.

4. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The isocyanate is diphenylmethane diisocyanate.

5. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The chain extenders are 1,4-butanediol and 2-methyl-1,3-propanediol.

6. The high-strength flame-retardant TPU material according to claim 5, characterized in that: In the chain extender, the mass percentage of 1,4-butanediol is 90-99%.

7. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The flame retardant is triphenyl phosphate, triethyl phosphate, tricresyl phosphate, resorcinol bis(diphenyl phosphate), toluene diphenyl phosphate or bisphenol A bis(diphenyl phosphate).

8. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The antioxidant is tris(2,4-di-tert-butylphenyl)phosphite, poly(dipropylene glycol)phenylphosphite or diphenyl monoisodecylphosphite; the hydrolysis-resistant agent is carbodiimide; and the catalyst is stannous octoate.

9. The high-strength flame-retardant TPU material according to claim 1, characterized in that: The ultraviolet absorber is N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine, N-(ethoxycarbonylphenyl)-N'-ethyl-N'-phenylformamidine, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone or 2-hydroxy-4-n-octyloxybenzophenone.

10. The method for preparing the high-strength flame-retardant TPU material according to any one of claims 1 to 9, characterized in that: First, add the synergist, flame retardant, antioxidant, hydrolysis resistance agent and UV absorber to the diol, stir evenly, add them into the twin-screw extruder zone 1 together with isocyanate, chain extender and catalyst to carry out continuous polymerization reaction, and obtain high-strength flame-retardant TPU material after underwater granulation, aging and drying.