Highly hygroscopic polyacrylonitrile fiber with composite function and preparation method thereof
Through the preparation and functional treatment of polyacrylonitrile/regenerated cellulose blended fibers, the problems of flammability and poor hygroscopicity of polyacrylonitrile fibers are solved, and the versatility of high hygroscopicity, antibacterial and deodorizing and flame retardant are achieved. Reduced heat shrinkage and is suitable for sportswear and other fields.
Patent Information
- Application Number
- CN202410898033.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Polyacrylonitrile fibers are flammable, have poor hygroscopicity, and have electrostatic problems, which limit their application in sportswear, underwear and other fields. The existing modification methods have the problem of degradation of durability by using toxic substances or functional additives.
The preparation method of polyacrylonitrile/regenerated cellulose blended fiber is adopted. Itaconic acid, methyl acrylate and acrylonitrile are copolymerized, dimethylacetamide and LiCl are added as cosolvent, and wet spinning is performed, and air plasma is performed. Treatment, hydrolysis treatment and functional additive adsorption, combined with the treatment of sodium alginate, tea polyphenols and inorganic zinc antibacterial agents, to form a porous structure to improve hygroscopicity and functionality.
It realizes the versatility of high hygroscopicity, antibacterial and deodorizing, and flame retardant, reduces the heat shrinkage rate, improves the comfort and functionality of fibers, and facilitates mass production.
Smart Images

Figure O50KV0J0HUAIWOBDN4GFCQQYPE2KUNUDURH5WMZG
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyacrylonitrile fibers, and in particular relates to highly hygroscopic polyacrylonitrile fibers with composite functions and a preparation method thereof. Background Art
[0002] Polyacrylonitrile (PAN) fiber is a fiber made by spinning acrylonitrile as the main monomer (content greater than 85%) and other monomers. Because of its fluffy and soft, heat-resistant and warm, high resilience, it is known as "artificial wool" and is widely used in interior decoration and clothing, outdoor fabrics, filter materials, building composite materials and carbon fiber.
[0003] However, acrylic fibers and their fabrics are flammable, with a limiting oxygen index value of only about 18%, making them flammable fibers. In addition, the presence of highly polar and regularly arranged cyano groups in the PAN molecular chain makes PAN hygroscopic, with a moisture regain of only 1.2-2%. It is prone to static electricity and has poor wearing comfort, which greatly limits its application in sportswear, underwear and other clothing fields. Therefore, it is urgent to modify acrylic fibers in terms of hydrophilicity and other aspects to improve their wearing comfort and functionality to meet the application needs in various fields.
[0004] Patent CN101845745A discloses a method for manufacturing highly hygroscopic and flame-retardant multifunctional modified acrylic fibers, wherein acrylic fibers are first added to a copper ion aqueous solution to react and prepare copper ion-containing acrylic fibers, then added to a mixed solution of hydrazine hydrate and a reaction aid for immersion, and then squeezed or dried to prepare acrylic fibers containing a certain amount of aqueous solution, and then placed in a high-temperature and high-pressure steaming and shaping pot for dry steaming or steaming at high temperature to prepare highly hygroscopic flame-retardant acrylic fibers. The fiber preparation process uses hydrazine hydrate, which is toxic, causing certain problems in the fiber preparation process and production environment.
[0005] Patent CN102220651A discloses a hygroscopic heat-generating fiber and a preparation method thereof, wherein the fiber includes acrylonitrile, acrylamide, and acrylic acid, and the above components are stirred evenly in a high concentration of zinc chloride, sodium thiocyanate and other salt solvents, and graft copolymerization is carried out, and then the spinning solution is placed in a low concentration of zinc chloride, sodium thiocyanate and other salt solutions for coagulation and drawing to obtain a product. The hygroscopic heat-generating fiber obtained by the invention has a high hygroscopic property and has a good self-heating effect when encountering water vapor. However, it needs to be grafted and copolymerized in a redox initiation system, and the degree of improvement of the hygroscopicity of the fiber is limited by modifying acrylonitrile alone, and it is also impossible to improve the defects of polyacrylonitrile fiber such as high thermal shrinkage.
[0006] Patent CN114381820A discloses a flame retardant high hygroscopic acrylic fiber and a production method thereof. The flame retardant high hygroscopic acrylic fiber includes acrylic fiber and a flame retardant hygroscopic modifier. The functionalization of the final product is achieved through the hydrophilic group contained in the flame retardant hygroscopic modifier and the "skin-core" structure of the fiber. Although the skin-core structure reduces the amount of flame retardant hygroscopic modifier used, it causes the fiber surface to contain too much flame retardant, which not only affects the feel of the fiber, but also reduces the durability of the fiber during use as the outer flame retardant falls off.
[0007] Patent CN117248375A discloses a method for preparing warm-colored hygroscopic and heat-generating modified polyacrylonitrile fiber, which undergoes chemical crosslinking reaction, alkaline hydrolysis reaction and oxidation reaction with a crosslinking agent to prepare a modified polyacrylonitrile fiber that is golden yellow, which limits its certain applications.
[0008] Generally speaking, the structure of the fiber determines the fiber performance. By changing the fiber structure in various ways, the fiber performance can be changed or new functions can be given to the fiber. For example, by grafting modification, polar hydrophilic groups are introduced into the macromolecular structure of polyacrylonitrile to improve the hygroscopicity of the fiber; by blending modification, the fiber prepared by blending polyacrylonitrile with cellulose will further improve the water absorption of the fiber; by blending and spinning with functional substances, the fiber can be given good functionality, such as flame retardancy, antistatic, antibacterial and deodorizing. In view of this, how to modify polyacrylonitrile fiber so that it has both high hygroscopicity and multifunctional properties such as antibacterial and deodorizing, flame retardancy, and UV protection is a technical problem that needs to be solved urgently. Summary of the invention
[0009] In view of the problems existing in the prior art, the purpose of the present invention is to provide a highly hygroscopic polyacrylonitrile fiber with composite functions, which has high hygroscopicity and multifunctional properties such as antibacterial, deodorizing and flame retardant, and has low thermal shrinkage; the present invention also provides a preparation method thereof, which is feasible in process and convenient for mass production.
[0010] The method for preparing the highly hygroscopic polyacrylonitrile fiber with composite function of the present invention comprises the following steps:
[0011] (1) Preparation of polyacrylonitrile / regenerated cellulose blended fibers:
[0012] Itaconic acid, methyl acrylate and acrylonitrile are used as raw materials for copolymerization to obtain a polyacrylonitrile copolymer, the polyacrylonitrile copolymer and regenerated cellulose are activated and then dissolved in a co-solvent obtained by mixing dimethylacetamide and LiCl, a water-soluble substance is added and dissolved to obtain a blended spinning solution, and wet spinning is performed to obtain a polyacrylonitrile / regenerated cellulose blended fiber;
[0013] (2) Modification of polyacrylonitrile / regenerated cellulose blended fibers:
[0014] The polyacrylonitrile / regenerated cellulose blend fiber is first subjected to air plasma treatment, then immersed in water to dissolve water-soluble substances, and then hydrolyzed with a mixed aqueous solution of sodium hydroxide and ammonia water to obtain a modified polyacrylonitrile / regenerated cellulose blend fiber;
[0015] (3) Functional finishing of polyacrylonitrile / regenerated cellulose blended fibers:
[0016] The modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution containing sodium alginate, tea polyphenols, and a cross-linking agent to complete the first functional auxiliary agent adsorption bath treatment; then immersed in an aqueous solution containing an inorganic zinc antibacterial agent and a modifier, or first immersed in an aqueous solution containing an inorganic zinc antibacterial agent and then irradiated in an air atmosphere at room temperature to complete the second functional auxiliary agent adsorption bath treatment; finally, oiled, dried, and opened in sequence to obtain a highly hygroscopic polyacrylonitrile fiber with composite functions.
[0017] In step (1), the mass ratio of itaconic acid, methyl acrylate and acrylonitrile is 0.5-1:1-2:10.
[0018] In step (1), the preparation method of polyacrylonitrile copolymer is as follows: itaconic acid, methyl acrylate and acrylonitrile are used as polymerization monomers, the polymerization monomers are added into water, the temperature is raised to 65-75°C under stirring in a nitrogen atmosphere, and then 0.5-2.0% of the total weight of the polymerization monomer is added as an initiator, the temperature is maintained at 65-75°C for 2.5-3.5h, and after the reaction is completed, the polymer precipitate is dried at 60-80°C to a moisture content of ≤0.5wt.%, to obtain a polyacrylonitrile copolymer.
[0019] Preferably, the initiator is ammonium persulfate or azobisisobutyronitrile.
[0020] In step (1), the activation treatment method of the polyacrylonitrile copolymer is: immersing the polyacrylonitrile copolymer in a dimethylacetamide solvent, activating it at a temperature of 110-130°C for 90-120 minutes, then taking it out and drying it at 60-80°C to a moisture content of ≤0.5wt.%, thereby completing the activation of the polyacrylonitrile copolymer.
[0021] In step (1), the activation treatment method of regenerated cellulose is: the regenerated cellulose is crushed to a particle size D50 of 155.12-275.66 μm, then immersed in a dimethylacetamide solvent, activated at a temperature of 120-160° C. for 60-90 min, and finally centrifuged to remove the dimethylacetamide solvent to complete the activation of the regenerated cellulose.
[0022] The invention uses dimethylacetamide to activate the polyacrylonitrile copolymer and the regenerated cellulose, mainly by utilizing the strong polarity of dimethylacetamide to destroy the intramolecular and intermolecular hydrogen bonds of the polyacrylonitrile copolymer and the regenerated cellulose, so that part of the hydrogen bonds are broken. When the co-blended spinning stock solution is prepared, the co-solvent can more easily penetrate into the crystalline region of the fiber for contact, which not only accelerates the dissolution of the substance, but also improves the uniformity of the co-blended spinning stock solution, so that the performance of the obtained blended fiber is more stable.
[0023] In step (1), in the blended spinning stock solution, the mass ratio of the activated polyacrylonitrile copolymer and the regenerated cellulose is 10:3-5, and the concentration of the activated polyacrylonitrile copolymer and the regenerated cellulose is 12-20wt.%.
[0024] In step (1), the water-soluble substance is polyethylene glycol or polyvinyl alcohol, and the amount added is 10-18% of the total mass of the activated polyacrylonitrile copolymer and the regenerated cellulose.
[0025] Preferably, the polyethylene glycol is at least one of PEG4000, PEG6000, PEG8000, and PEG10000.
[0026] Preferably, the polyvinyl alcohol has a degree of alcoholysis of 88 and a degree of polymerization of 500-800.
[0027] In step (1), the mass ratio of dimethylacetamide to LiCl in the co-solvent is 100:8-12. The purpose of using the mixture of dimethylacetamide and LiCl as the co-solvent is to fully dissolve the regenerated cellulose.
[0028] In step (1), during wet spinning, the drafting ratio is 6-12 times; the coagulation bath is one of methanol, acetonitrile and water, and the coagulation bath temperature is 2-8°C.
[0029] In step (2), the air plasma treatment conditions are: the reaction gas is air, the power is 150-250 W, the time is 50-100 s, and the pressure is 50-90 Pa. After the air plasma treatment, the surface structure of the blended fiber is etched and the surface area is increased, which is convenient for the subsequent dissolution and hydrolysis of water-soluble substances.
[0030] In step (2), the water temperature used for dissolving the water-soluble substance is 80-100°C, and the dissolution time is 120-180 minutes. During the dissolution treatment of the water-soluble substance, the polyacrylonitrile / regenerated cellulose blended fiber is continuously turned over to dissolve the water-soluble substance in the blended fiber as quickly as possible.
[0031] In step (2), the process conditions of the hydrolysis treatment are: bath ratio 15-20:1, temperature 80-95°C, time 15-20min; the concentration of the mixed aqueous solution of sodium hydroxide and ammonia water is 10-15wt.%, and the mass ratio of sodium hydroxide to ammonia water is 1:1-2.
[0032] During the hydrolysis treatment, due to the dissolution of water-soluble substances in the blended fibers, the specific surface area of the blended fibers increases, the hydrolysis reaction becomes more intense, and it is easier to introduce hydrophilic groups into the blended fibers, which is beneficial to improving the hygroscopic properties of the blended fibers. At the same time, ammonia water can react with the unreacted carboxyl groups in the copolymer itaconic acid to form carboxylates, further improving the hydrophilicity.
[0033] In step (3), during the first functional additive adsorption bath treatment, the modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution having a sodium alginate concentration of 10-15wt.%, a tea polyphenol concentration of 10-20wt.%, and a cross-linking agent concentration of 10-20wt.%, and the pH value is adjusted to 5.5-7.0, the temperature is 90-100°C, and the treatment is performed for 60-180 minutes to complete the first functional additive adsorption bath treatment.
[0034] Preferably, the cross-linking agent is at least one of JYK LA-80 (Shanghai Jieyikang Chemical Technology Co., Ltd.), acrylic acid, and acrylamide.
[0035] Preferably, the pH value is adjusted by using one of hydrochloric acid, sulfuric acid, acetic acid and lactic acid.
[0036] The modified polyacrylonitrile / regenerated cellulose blended fibers can be continuously turned over during the treatment process and subjected to ultrasonic conditions (frequency of 6.0×10 3 -2.0×10 5 MHz) for adsorption to improve the treatment efficiency.
[0037] In step (3), during the second functional additive adsorption bath, the modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution with an inorganic zinc antibacterial agent concentration of 10-15wt.%, and a modifier concentration of 5-10wt.%, and the temperature is adjusted to 90-100°C for 30-90min; or the modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution with an inorganic zinc antibacterial agent concentration of 10-15wt.%, and the temperature is adjusted to 90-100°C for 30-90min; dried, and irradiated in an air atmosphere at room temperature to complete the second functional additive adsorption bath treatment.
[0038] Preferably, the inorganic zinc antibacterial agent is at least one of zinc chloride, zinc sulfate and zinc acetate.
[0039] Preferably, the modifier is JYK NA-30 (Shanghai Jieyikang Chemical Technology Co., Ltd.).
[0040] Preferably, the accelerator energy of the irradiation treatment is 1.0-1.5 MeV, and the absorbed dose is 50-100 kGy.
[0041] The present invention endows the blended fiber with good flame retardant, antibacterial and deodorizing functions through the complexation between sodium alginate, tea polyphenols and zinc ions, as well as the modification treatment of crosslinking agent JYK LA-80 and modifier JYK NA-30 or irradiation, and further improves the hygroscopicity of the fiber.
[0042] Among them, sodium alginate can undergo ion exchange reaction with zinc ions to generate zinc alginate, which has excellent antibacterial and flame retardant properties, thereby giving the fiber good antibacterial and flame retardant properties, and then it is finished with tea polyphenol solution. Tea polyphenol has good antibacterial and deodorizing properties, and it reacts with excess zinc ions to produce complexes, increasing the stability of tea polyphenols, thereby giving the blended fiber good antibacterial and deodorizing functions; at the same time, sodium alginate and tea polyphenols have a large number of water-absorbing groups in addition to the reactive groups, which can improve the hygroscopicity of the blended fiber; under the action of modifiers or irradiation, the cross-linking agent can undergo multiple cross-linking reactions with cyano, carboxyl or hydroxyl groups in the blended fiber through its own reactive groups, such as carboxyl and amide groups, to form a certain spatial cross-linked network structure to maintain the stability of the fiber structure.
[0043] In step (3), the oiling temperature is 55-70°C, the drying temperature is 110-150°C, and the blended fibers are dried to a moisture content of 9-12wt.%.
[0044] The highly hygroscopic polyacrylonitrile fiber with composite functions prepared by the present invention has an Escherichia coli inhibition rate of ≥91.6% (GB / T20944.3-2008), a Candida albicans inhibition rate of ≥88.5% (GB / T20944.3-2008), an ammonia reduction rate of ≥89.% (GB / T33610.2-2017), a trimethylamine reduction rate of ≥88.% (GB / T33610.3-2019), a limiting oxygen index of 27.9-30.6 (FZ / T50016-2011), a moisture regain of 25.9-29.9% (GB / T6503-2008), a temperature rise of 6.3-9.8°C after moisture absorption (GB / T 29866-2013), and a thermal shrinkage of 1.09-3% at 110°C (FZ / T 50004-2011).
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) The present invention uses itaconic acid, acrylic acid ester and acrylonitrile as comonomers to prepare polyacrylonitrile copolymer, introduces carboxyl groups to improve its hydrophilicity; at the same time, the polyacrylonitrile copolymer is blended with regenerated cellulose for spinning. Since the regenerated cellulose contains a large amount of hydroxyl groups, its water absorption is much higher than that of polyacrylonitrile of the same quality, thereby further improving the hygroscopicity of the blended fiber; in addition, the addition of regenerated cellulose can also significantly improve the defects of polyacrylonitrile fiber itself, such as high thermal shrinkage and difficulty in dyeing with reactive dyes, thereby reducing the thermal shrinkage of the blended fiber and making it easier to dye with reactive dyes, thereby expanding its application range;
[0047] (2) The present invention utilizes air plasma to treat the blended fibers, etches the surface of the blended fibers, and increases the surface area thereof, which is convenient for the subsequent dissolution of water-soluble substances, hydrolysis treatment, and increase of oxygen-containing groups, thereby improving hygroscopicity; and utilizes the dissolution of water-soluble substances to give the blended fibers a good porous structure, increase the specific surface area of the blended fibers, increase the contact and adsorption of the blended fibers with water molecules, and thus improve the hygroscopicity of the blended fibers; and also utilizes the reaction of the blended fibers with sodium hydroxide and ammonia water during the hydrolysis process to introduce more hydrophilic groups into the blended fibers, thereby greatly improving the hygroscopicity of the fibers;
[0048] (3) The present invention adopts an adsorption process, with sodium alginate, tea polyphenols and zinc-containing substances as functional components, and utilizes the interaction between a crosslinking agent and a modifier or the modification under irradiation treatment, and endows the fiber with good flame retardant and antibacterial and deodorizing functions through a complexing process, and further endows the fiber with good hygroscopicity through the crosslinking agent and the modifier or irradiation, and maintains the stability of the structure;
[0049] (4) The highly hygroscopic polyacrylonitrile fiber with composite functions prepared by the present invention has high hygroscopicity and multifunctional properties of antibacterial, deodorizing and flame retardant, and can be dyed with reactive dyes. Its Escherichia coli inhibition rate is ≥91.6%, Candida albicans inhibition rate is ≥88.5%, ammonia reduction rate is ≥89.6%, trimethylamine reduction rate is ≥88.1%, limiting oxygen index is 27.9-30.6%, regain is 25.9-29.9%, temperature rise after moisture absorption is 6.3-9.8°C, and thermal shrinkage rate at 110°C is 1.09-1.93%. DETAILED DESCRIPTION
[0050] The present invention is further described below in conjunction with the examples. The raw materials used in the examples, unless otherwise specified, are all commercially available conventional raw materials; the process methods used in the examples, unless otherwise specified, are all conventional methods in the art. The examples of the present invention do not limit the level of the amount of each raw material, and any weight level can be used for preparation, as long as the specific raw material ratio is followed.
[0051] Some of the raw materials used in the examples are described as follows:
[0052] JYK LA-80: cross-linking agent, Shanghai Jieyikang Chemical Technology Co., Ltd.;
[0053] JYK NA-30: Modifier, Shanghai Jieyikang Chemical Technology Co., Ltd.
[0054] Example 1
[0055] The highly hygroscopic polyacrylonitrile fiber with composite function is prepared according to the following steps:
[0056] (1) Preparation of polyacrylonitrile / regenerated cellulose blended fibers:
[0057] Itaconic acid, methyl acrylate and acrylonitrile in a mass ratio of 0.5:1:10 are used as polymerization monomers, the polymerization monomers are added into deionized water, nitrogen is passed for 30 minutes, the oxygen in the reactor is emptied, and the temperature is raised to 65°C while stirring, and then 0.5% of the total weight of the polymerization monomer is added as an initiator. The temperature is kept at 65°C for 3.5 hours. The sealing of the reactor is maintained during the reaction. After the reaction is completed, the polymer precipitate is washed and dried at 60°C to a moisture content of ≤0.5wt.%, thereby obtaining a polyacrylonitrile copolymer; the polyacrylonitrile copolymer is immersed in a dimethylacetamide solvent, activated at a temperature of 110°C for 120 minutes, then taken out, and dried at 60°C to a moisture content of ≤0.5wt.%, thereby obtaining an activated polyacrylonitrile copolymer;
[0058] The regenerated cellulose was crushed to a particle size D50 of 275.66 μm, then immersed in a dimethylacetamide solvent, activated at 120° C. for 90 min, and finally centrifuged to remove the dimethylacetamide solvent to obtain activated regenerated cellulose;
[0059] Dimethylacetamide and LiCl are mixed at a mass ratio of 100:8 as a co-solvent, activated polyacrylonitrile copolymer and activated regenerated cellulose are added to the co-solvent at a mass ratio of 10:3, the temperature is raised to 75° C. and stirred to dissolve, to obtain a first blended spinning stock solution with a mass concentration of 12%, and then PEG4000 accounting for 10% of the total mass of the activated polyacrylonitrile copolymer and the activated regenerated cellulose is added, stirred to dissolve, to obtain a blended spinning stock solution;
[0060] The blended spinning solution was spun by wet spinning process, the drafting ratio was 12 times, the coagulation bath was acetonitrile, the coagulation bath temperature was 2°C, and the fibers were cut into 28 mm length after spinning without refining treatment and drying to obtain polyacrylonitrile / regenerated cellulose blended fibers;
[0061] (2) Modification of polyacrylonitrile / regenerated cellulose blended fibers:
[0062] The polyacrylonitrile / regenerated cellulose blended fiber was treated with air plasma, and the air plasma treatment conditions were as follows: the reaction gas was air, the power was 150W, the time was 100s, and the pressure was 50Pa; then it was immersed in deionized water at 80°C for 120min to dissolve the water-soluble substances, and then it was hydrolyzed in a mixed solution of 10% sodium hydroxide and ammonia water (mass ratio 1:1), the bath ratio was 15:1, the temperature was 80°C, and the time was 20min, to obtain modified polyacrylonitrile / regenerated cellulose blended fiber;
[0063] (3) Functional finishing of polyacrylonitrile / regenerated cellulose blended fibers:
[0064] The modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution of 10 wt.% sodium alginate, 10 wt.% tea polyphenols, and 10 wt.% JYK LA-80, sulfuric acid is added to adjust the pH value to 5.5, and the treatment is carried out at a temperature of 90° C. for 60 minutes to complete the first functional additive adsorption bath treatment;
[0065] The modified polyacrylonitrile / regenerated cellulose blended fibers treated with the first functional additive adsorption bath were squeezed, and then immersed in an aqueous solution with a zinc sulfate concentration of 13wt.% and a JYK NA-30 concentration of 5wt.%, and treated at a temperature of 90°C for 30 minutes to complete the second functional additive adsorption bath treatment;
[0066] The modified polyacrylonitrile / regenerated cellulose blended fibers treated with the second functional additive adsorption bath are pressed, oiled at an oil bath temperature of 55°C, and then dried at a temperature of 110°C until the moisture content of the blended fibers reaches 9wt.%, and then opened to obtain highly hygroscopic polyacrylonitrile fibers with composite functions.
[0067] Example 2
[0068] The highly hygroscopic polyacrylonitrile fiber with composite function is prepared according to the following steps:
[0069] (1) Preparation of polyacrylonitrile / regenerated cellulose blended fibers:
[0070] Itaconic acid, methyl acrylate and acrylonitrile in a mass ratio of 0.65:1.2:10 are used as polymerization monomers, the polymerization monomers are added into deionized water, nitrogen is passed for 36 minutes, the oxygen in the reactor is emptied, and the temperature is raised to 68°C while stirring, and then ammonium persulfate of 1.2% of the total weight of the polymerization monomer is added as an initiator, the temperature is maintained at 68°C for reaction for 2.8 hours, and the sealing of the reactor is maintained during the reaction. After the reaction is completed, the polymer precipitate is washed and dried at 66°C to a moisture content of ≤0.5wt.%, to obtain a polyacrylonitrile copolymer; the polyacrylonitrile copolymer is immersed in a dimethylacetamide solvent, activated at a temperature of 117°C for 110 minutes, then taken out, and dried at 68°C to a moisture content of ≤0.5wt.%, to obtain an activated polyacrylonitrile copolymer;
[0071] The regenerated cellulose was crushed to a particle size D50 of 236.78 μm, then immersed in a dimethylacetamide solvent, activated at 136°C for 75 min, and finally centrifuged to remove the dimethylacetamide solvent to obtain activated regenerated cellulose;
[0072] Dimethylacetamide and LiCl are mixed at a mass ratio of 100:9 as a co-solvent, activated polyacrylonitrile copolymer and activated regenerated cellulose are added to the co-solvent at a mass ratio of 10:3.6, the temperature is raised to 79° C. and stirred to dissolve, to obtain a first blended spinning stock solution with a mass concentration of 13.5%, and then PEG6000 accounting for 11.5% of the total mass of the activated polyacrylonitrile copolymer and the activated regenerated cellulose is added, stirred to dissolve, to obtain a blended spinning stock solution;
[0073] The blended spinning solution was spun by wet spinning process, the drafting ratio was 10 times, the coagulation bath was water, the coagulation bath temperature was 4°C, no refining treatment was performed, and the fiber was dried to obtain polyacrylonitrile / regenerated cellulose blended fiber;
[0074] (2) Modification of polyacrylonitrile / regenerated cellulose blended fibers:
[0075] The polyacrylonitrile / regenerated cellulose blended fiber was treated with air plasma, and the air plasma treatment conditions were as follows: the reaction gas was air, the power was 185W, the time was 85s, and the pressure was 65Pa; then it was immersed in deionized water at 88°C for 136min to dissolve the water-soluble substances, and then it was hydrolyzed in a mixed solution of sodium hydroxide with a concentration of 12.5% and ammonia water (mass ratio 1:1.2), with a bath ratio of 17:1, a temperature of 85°C, and a time of 18min to obtain modified polyacrylonitrile / regenerated cellulose blended fiber;
[0076] (3) Functional finishing of polyacrylonitrile / regenerated cellulose blended fibers:
[0077] The modified polyacrylonitrile / regenerated cellulose blended fiber was immersed in an aqueous solution of 12.5wt.% sodium alginate, 15wt.% tea polyphenols and 15.5wt.% acrylic acid, and hydrochloric acid was added to adjust the pH value to 6.2. The fiber was treated at 96°C for 122 minutes to complete the first functional additive adsorption bath treatment.
[0078] The modified polyacrylonitrile / regenerated cellulose blended fibers treated with the first functional additive adsorption bath were squeezed, and then immersed in an aqueous solution with a zinc sulfate concentration of 13wt.% and a JYK NA-30 concentration of 10wt.%, and treated at a temperature of 93°C for 52 minutes to complete the second functional additive adsorption bath treatment;
[0079] The modified polyacrylonitrile / regenerated cellulose blended fibers treated with the second functional additive adsorption bath are pressed, oiled in an oil bath at 60°C, and then dried at 123°C until the moisture content of the blended fibers reaches 10.5wt.%, and then opened to obtain highly hygroscopic polyacrylonitrile fibers with composite functions.
[0080] Example 3
[0081] The highly hygroscopic polyacrylonitrile fiber with composite function is prepared according to the following steps:
[0082] (1) Preparation of polyacrylonitrile / regenerated cellulose blended fibers:
[0083] Itaconic acid, methyl acrylate and acrylonitrile in a mass ratio of 0.8:1.5:10 are used as polymerization monomers, the polymerization monomers are added into deionized water, nitrogen is passed for 45 minutes, the oxygen in the reactor is emptied, and the temperature is raised to 71°C while stirring, and then ammonium persulfate of 1.5% of the total weight of the polymerization monomer is added as an initiator, and the temperature is kept at 71°C for 3 hours. The sealing of the reactor is maintained during the reaction. After the reaction is completed, the polymer precipitate is washed and dried at 72°C to a moisture content of ≤0.5wt.%, to obtain a polyacrylonitrile copolymer; the polyacrylonitrile copolymer is immersed in a dimethylacetamide solvent, activated at a temperature of 122°C for 108 minutes, then taken out, and dried at 76°C to a moisture content of ≤0.5wt.%, to obtain an activated polyacrylonitrile copolymer;
[0084] The regenerated cellulose was crushed to a particle size D50 of 236.51 μm, then immersed in a dimethylacetamide solvent, activated at 136°C for 75 min, and finally centrifuged to remove the dimethylacetamide solvent to obtain activated regenerated cellulose;
[0085] Dimethylacetamide and LiCl are mixed at a mass ratio of 100:10 as a co-solvent, activated polyacrylonitrile copolymer and activated regenerated cellulose are added to the co-solvent at a mass ratio of 10:4.3, the temperature is raised to 82° C. and stirred to dissolve, to obtain a first blended spinning stock solution with a mass concentration of 16%, and then PEG8000 accounting for 13.5% of the total mass of the activated polyacrylonitrile copolymer and the activated regenerated cellulose is added, stirred to dissolve, to obtain a blended spinning stock solution;
[0086] The blended spinning solution was spun by wet spinning process, the drafting ratio was 8.5 times, the coagulation bath was methanol, the coagulation bath temperature was 5°C, no refining treatment was performed, and the fiber was dried to obtain polyacrylonitrile / regenerated cellulose blended fiber;
[0087] (2) Modification of polyacrylonitrile / regenerated cellulose blended fibers:
[0088] The polyacrylonitrile / regenerated cellulose blended fiber was treated with air plasma, and the air plasma treatment conditions were as follows: the reaction gas was air, the power was 225W, the time was 68s, and the pressure was 81Pa; then it was immersed in deionized water at 95°C for 162min to dissolve the water-soluble substances, and then it was hydrolyzed in a mixed solution of sodium hydroxide with a concentration of 13.8% and ammonia water (mass ratio 1:1.6), with a bath ratio of 18:1, a temperature of 92°C, and a time of 16.5min to obtain a modified polyacrylonitrile / regenerated cellulose blended fiber;
[0089] (3) Functional finishing of polyacrylonitrile / regenerated cellulose blended fibers:
[0090] The modified polyacrylonitrile / regenerated cellulose blended fiber was immersed in an aqueous solution of 13.8wt.% sodium alginate, 18.2wt.% tea polyphenols, and 17.5wt.% acrylic acid, acetic acid was added to adjust the pH value to 6.5, and the mixture was treated at 97°C for 158 minutes to complete the first functional additive adsorption bath treatment;
[0091] The modified polyacrylonitrile / regenerated cellulose blended fiber treated with the first functional additive adsorption bath was squeezed, immersed in an aqueous solution of zinc sulfate with a concentration of 13.8 wt.%, and treated at a temperature of 96° C. for 75 min. The blended fiber was then dried and irradiated in an air atmosphere at room temperature with an accelerator energy of 1.5 MeV and an absorbed dose of 100 kGy to complete the second functional additive adsorption bath treatment;
[0092] The modified polyacrylonitrile / regenerated cellulose blended fibers treated with the second functional additive adsorption bath are pressed, oiled at an oil bath temperature of 65°C, and then dried at a temperature of 138°C until the moisture content of the blended fibers is 11.1wt.%, and then opened to obtain highly hygroscopic polyacrylonitrile fibers with composite functions.
[0093] Example 4
[0094] The highly hygroscopic polyacrylonitrile fiber with composite function is prepared according to the following steps:
[0095] (1) Preparation of polyacrylonitrile / regenerated cellulose blended fibers:
[0096] Itaconic acid, methyl acrylate and acrylonitrile in a mass ratio of 1:2:10 are used as polymerization monomers, the polymerization monomers are added into deionized water, nitrogen is passed for 30 minutes, the oxygen in the reactor is emptied, and the temperature is raised to 75°C while stirring, and then 2.0% of the total weight of azobisisobutyronitrile is added as an initiator, the temperature is kept at 75°C for 2.5 hours, and the sealing of the reactor is maintained during the reaction. After the reaction is completed, the polymer precipitate is washed and dried at 80°C to a moisture content of ≤0.5wt.%, to obtain a polyacrylonitrile copolymer; the polyacrylonitrile copolymer is immersed in a dimethylacetamide solvent, activated at a temperature of 110°C for 120 minutes, then taken out, and dried at 80°C to a moisture content of ≤0.5wt.%, to obtain an activated polyacrylonitrile copolymer;
[0097] The regenerated cellulose was crushed to a particle size D50 of 155.12 μm, then immersed in a dimethylacetamide solvent, activated at 160°C for 60 min, and finally centrifuged to remove the dimethylacetamide solvent to obtain activated regenerated cellulose;
[0098] Dimethylacetamide and LiCl are mixed in a mass ratio of 100:12 as a co-solvent, activated polyacrylonitrile copolymer and activated regenerated cellulose are added to the co-solvent in a mass ratio of 10:5, the temperature is raised to 82° C. and stirred to dissolve, to obtain a first blended spinning stock solution with a mass concentration of 20%, and then polyvinyl alcohol (alcoholysis degree 88, polymerization degree 500) accounting for 18% of the total mass of the activated polyacrylonitrile copolymer and the activated regenerated cellulose is added, stirred to dissolve, to obtain a blended spinning stock solution;
[0099] The blended spinning solution was spun by wet spinning process, the drafting ratio was 6 times, the coagulation bath was deionized water, the coagulation bath temperature was 8°C, and the fibers were cut into 76 mm length after spinning without refining treatment and drying to obtain polyacrylonitrile / regenerated cellulose blended fibers;
[0100] (2) Modification of polyacrylonitrile / regenerated cellulose blended fibers:
[0101] The polyacrylonitrile / regenerated cellulose blended fiber was treated with air plasma, and the air plasma treatment conditions were as follows: the reaction gas was air, the power was 250W, the time was 50s, and the pressure was 90Pa; then it was immersed in deionized water at 100°C for 180min to dissolve the water-soluble substances, and then it was hydrolyzed in a mixed solution of 15% sodium hydroxide and ammonia water (mass ratio 1:2), with a bath ratio of 20:1, a temperature of 95°C, and a time of 15min to obtain modified polyacrylonitrile / regenerated cellulose blended fiber;
[0102] (3) Functional finishing of polyacrylonitrile / regenerated cellulose blended fibers:
[0103] The modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution with a sodium alginate concentration of 15wt.%, a tea polyphenol concentration of 20wt.%, and an acrylamide concentration of 20wt.%, and lactic acid is added to adjust the pH value to 7.0, and the mixture is treated at a temperature of 100°C for 180 minutes to complete the first functional additive adsorption bath treatment;
[0104] The modified polyacrylonitrile / regenerated cellulose blended fiber treated with the first functional additive adsorption bath was squeezed, immersed in an aqueous solution of zinc acetate with a concentration of 15 wt.%, and treated at a temperature of 100° C. for 90 minutes. The blended fiber was then dried and irradiated in an air atmosphere at room temperature with an accelerator energy of 1 MeV and an absorbed dose of 50 kGy to complete the second functional additive adsorption bath treatment.
[0105] The modified polyacrylonitrile / regenerated cellulose blended fibers treated with the second functional additive adsorption bath are pressed, oiled in an oil bath at 70°C, and then dried at 150°C until the moisture content of the blended fibers reaches 12wt.%, and then opened to obtain highly hygroscopic polyacrylonitrile fibers with composite functions.
[0106] Comparative Example 1
[0107] The only difference between this comparative example and Example 1 is that itaconic acid is replaced by an equal mass of methyl acrylate.
[0108] Comparative Example 2
[0109] The only difference between this comparative example and Example 1 is that the water-soluble substance PEG4000 is not added to the blended spinning solution.
[0110] Comparative Example 3
[0111] The difference between this comparative example and Example 1 is that no ammonia water is added during the hydrolysis, that is, the hydrolysis treatment is carried out in a sodium hydroxide solution with a concentration of 10%.
[0112] Comparative Example 4
[0113] The difference between this comparative example and Example 1 is that the crosslinking agent JYK LA-80 and the modifier JYK NA-30 are not added during the functional finishing.
[0114] Comparative Example 5
[0115] The difference between this comparative example and Example 1 is that regenerated cellulose is not used for co-spinning, and the preparation steps are as follows:
[0116] (1) Preparation of polyacrylonitrile fiber:
[0117] Itaconic acid, methyl acrylate and acrylonitrile in a mass ratio of 0.5:1:10 are used as polymerization monomers, the polymerization monomers are added into deionized water, nitrogen is passed for 30 minutes, the oxygen in the reactor is emptied, and the temperature is raised to 65°C while stirring, and then 0.5% of the total weight of the polymerization monomer is added as an initiator. The temperature is kept at 65°C for 3.5 hours. The sealing of the reactor is maintained during the reaction. After the reaction is completed, the polymer precipitate is washed and dried at 60°C to a moisture content of ≤0.5wt.%, thereby obtaining a polyacrylonitrile copolymer; the polyacrylonitrile copolymer is immersed in a dimethylacetamide solvent, activated at a temperature of 110°C for 120 minutes, then taken out, and dried at 60°C to a moisture content of ≤0.5wt.%, thereby obtaining an activated polyacrylonitrile copolymer;
[0118] Dimethylacetamide and LiCl are mixed at a mass ratio of 100:8 as a co-solvent, an activated polyacrylonitrile copolymer is added to the co-solvent, the temperature is raised to 75°C and stirred to dissolve, to obtain a first blended spinning stock solution with a mass concentration of 12%, and then PEG4000 accounting for 10% of the total mass of the activated polyacrylonitrile copolymer is added, stirred to dissolve, to obtain a polyacrylonitrile spinning stock solution;
[0119] The polyacrylonitrile spinning solution was spun by wet spinning process, the drafting ratio was 12 times, the coagulation bath was acetonitrile, the coagulation bath temperature was 2°C, and the fibers were cut into 28 mm length after spinning without refining treatment and drying to obtain polyacrylonitrile fibers;
[0120] (2) Modification of polyacrylonitrile fiber:
[0121] The polyacrylonitrile fiber was treated with air plasma, and the air plasma treatment conditions were as follows: the reaction gas was air, the power was 150W, the time was 100s, and the pressure was 50Pa; then it was immersed in deionized water at 80°C for 120min to dissolve the water-soluble substances, and then it was hydrolyzed in a mixed solution of 10% sodium hydroxide and ammonia water (mass ratio 1:1), the bath ratio was 15:1, the temperature was 80°C, and the time was 20min, to obtain modified polyacrylonitrile fiber;
[0122] (3) Functional finishing of polyacrylonitrile fiber:
[0123] The modified polyacrylonitrile fiber is immersed in an aqueous solution of 10 wt.% sodium alginate, 10 wt.% tea polyphenols, and 10 wt.% JYK LA-80, sulfuric acid is added to adjust the pH value to 5.5, and the treatment is carried out at a temperature of 90° C. for 60 minutes to complete the first functional additive adsorption bath treatment;
[0124] The modified polyacrylonitrile fiber treated by the first functional additive adsorption bath was squeezed, and then immersed in an aqueous solution with a zinc sulfate concentration of 13wt.% and a JYK NA-30 concentration of 5wt.%, and treated at a temperature of 90°C for 30 minutes to complete the second functional additive adsorption bath treatment;
[0125] The modified polyacrylonitrile fiber treated with the second functional additive adsorption bath was pressed, oiled at an oil bath temperature of 55°C, and then dried at a temperature of 110°C until the moisture content of the fiber reached 9wt.%, and then opened to obtain polyacrylonitrile fiber.
[0126] The polyacrylonitrile fibers prepared in the embodiments and comparative examples were subjected to performance tests, wherein the inhibition rate of Escherichia coli and the inhibition rate of Candida albicans were tested in accordance with the standard GB / T20944.3-2008; the reduction rate of ammonia was tested in accordance with the standard GB / T33610.2-2017; the reduction rate of trimethylamine was tested in accordance with the standard GB / T33610.3-2019; the limiting oxygen index was tested in accordance with the standard FZ / T50016-2011; the regain was tested in accordance with the standard GB / T6503-2008; the temperature rise after moisture absorption was tested in accordance with the standard GB / T 29866-2013; and the heat shrinkage at 110°C was tested in accordance with the standard FZ / T 50004-2011. The test results are shown in Table 1.
[0127]
[0128] As can be seen from Table 1, the moisture regain of the polyacrylonitrile fiber prepared by the present invention is higher than 25.5%, the temperature rise after moisture absorption is greater than 6.0°C, the hygroscopicity is good, and it also has the multifunctional properties of antibacterial, deodorizing and flame retardant, and the heat shrinkage rate at 110°C is lower than 2%, and the thermal stability is good.
[0129] In Comparative Example 1, itaconic acid is replaced with methyl acrylate of equal mass, thereby reducing the number of carboxyl groups that subsequently react with ammonia water and the like, and the moisture regain of the obtained polyacrylonitrile fiber is reduced, and the temperature rise value after moisture absorption is reduced.
[0130] The blended spinning solution of Comparative Example 2 does not add water-soluble substances, so that the prepared polyacrylonitrile fiber has no pore structure and the surface area is reduced, thereby reducing the adsorbed functional additives, and the antibacterial property, deodorizing property, limiting oxygen index, regain and temperature rise value after moisture absorption of the polyacrylonitrile fiber are all reduced.
[0131] In Comparative Example 3, no ammonia water was added during the hydrolysis, which reduced the generation of carboxylates with better hydrophilicity, resulting in a decrease in the moisture regain of the polyacrylonitrile fiber and a decrease in the temperature rise value after moisture absorption.
[0132] In comparative example 4, no crosslinking agent or modifier is added during the functional finishing, so that the hydrophilic groups of the fiber are reduced, resulting in a decrease in the moisture regain of the polyacrylonitrile fiber and a decrease in the temperature rise value after moisture absorption.
[0133] In Comparative Example 5, regenerated cellulose is not used for co-spinning. The prepared polyacrylonitrile fiber lacks a large number of hydroxyl groups in the regenerated cellulose, resulting in a lower moisture regain and a lower temperature rise value after moisture absorption. At the same time, the lack of regenerated cellulose also leads to a significant increase in the shrinkage rate of the polyacrylonitrile fiber.
Claims
1. A method for preparing highly hygroscopic polyacrylonitrile fiber with composite function, characterized in that: The following steps are involved: (1) Preparation of polyacrylonitrile / regenerated cellulose blended fibers: Itaconic acid, methyl acrylate and acrylonitrile are used as raw materials for copolymerization to obtain a polyacrylonitrile copolymer, the polyacrylonitrile copolymer and regenerated cellulose are activated and then dissolved in a co-solvent obtained by mixing dimethylacetamide and LiCl, a water-soluble substance is added and dissolved to obtain a blended spinning solution, and wet spinning is performed to obtain a polyacrylonitrile / regenerated cellulose blended fiber; (2) Modification of polyacrylonitrile / regenerated cellulose blended fibers: The polyacrylonitrile / regenerated cellulose blend fiber is first subjected to air plasma treatment, then immersed in water to dissolve water-soluble substances, and then hydrolyzed with a mixed aqueous solution of sodium hydroxide and ammonia water to obtain a modified polyacrylonitrile / regenerated cellulose blend fiber; (3) Functional finishing of polyacrylonitrile / regenerated cellulose blended fibers: The modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution containing sodium alginate, tea polyphenols, and a cross-linking agent to complete a first functional auxiliary agent adsorption bath treatment; then immersed in an aqueous solution containing an inorganic zinc antibacterial agent and a modifier for treatment, or first immersed in an aqueous solution containing an inorganic zinc antibacterial agent for treatment, and then irradiated in an air atmosphere at room temperature to complete a second functional auxiliary agent adsorption bath treatment; finally, oiled, dried, and opened in sequence to obtain a highly hygroscopic polyacrylonitrile fiber with composite functions; The modifier is JYK NA-30.
2. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (1), the mass ratio of itaconic acid, methyl acrylate and acrylonitrile is 0.5-1:1-2:
10.
3. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (1), the activation treatment method of the polyacrylonitrile copolymer is: immersing the polyacrylonitrile copolymer in a dimethylacetamide solvent, activating it at a temperature of 110-130°C for 90-120 minutes, then taking it out, and drying it at 60-80°C until the moisture content is ≤0.5wt.%, thereby completing the activation of the polyacrylonitrile copolymer; The activation treatment method of regenerated cellulose is as follows: the regenerated cellulose is crushed to a particle size D50 of 155.12-275.66 μm, then immersed in a dimethylacetamide solvent, activated at a temperature of 120-160° C. for 60-90 minutes, and finally centrifuged to remove the dimethylacetamide solvent to complete the activation of the regenerated cellulose.
4. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (1), in the blended spinning stock solution, the mass ratio of the activated polyacrylonitrile copolymer and the regenerated cellulose is 10:3-5, and the concentration of the activated polyacrylonitrile copolymer and the regenerated cellulose is 12-20wt.%.
5. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (1), the water-soluble substance is polyethylene glycol or polyvinyl alcohol, and the amount thereof added is 10-18% of the total mass of the activated polyacrylonitrile copolymer and the regenerated cellulose; In the co-solvent, the mixing mass ratio of dimethylacetamide and LiCl is 100:8-12.
6. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (2), the air plasma treatment conditions are: the reaction gas is air, the power is 150-250 W, the time is 50-100 s, and the pressure is 50-90 Pa; The water temperature used for dissolving water-soluble substances is 80-100°C and the dissolution time is 120-180 minutes.
7. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (2), the process conditions of the hydrolysis treatment are: bath ratio 15-20:1, temperature 80-95°C, time 15-20min; the concentration of the mixed aqueous solution of sodium hydroxide and ammonia water is 10-15wt.%, and the mass ratio of sodium hydroxide to ammonia water is 1:1-2.
8. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (3), during the first functional additive adsorption bath treatment, the modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution having a sodium alginate concentration of 10-15wt.%, a tea polyphenol concentration of 10-20wt.%, and a cross-linking agent concentration of 10-20wt.%, and the pH value is adjusted to 5.5-7.0, the temperature is 90-100°C, and the treatment is performed for 60-180 minutes to complete the first functional additive adsorption bath treatment.
9. The method for preparing highly hygroscopic polyacrylonitrile fiber with composite function according to claim 1, characterized in that: In step (3), during the second functional additive adsorption bath, the modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution with an inorganic zinc antibacterial agent concentration of 10-15wt.%, and a modifier concentration of 5-10wt.%, and the temperature is adjusted to 90-100°C for 30-90min; or the modified polyacrylonitrile / regenerated cellulose blended fiber is immersed in an aqueous solution with an inorganic zinc antibacterial agent concentration of 10-15wt.%, and the temperature is adjusted to 90-100°C for 30-90min; dried, and irradiated in an air atmosphere at room temperature to complete the second functional additive adsorption bath treatment.
10. A highly hygroscopic polyacrylonitrile fiber with composite functions prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The inhibition rate of Escherichia coli is ≥91.6%, the inhibition rate of Candida albicans is ≥88.5%, the reduction rate of ammonia is ≥89.6%, the reduction rate of trimethylamine is ≥88.1%, the limiting oxygen index is 27.9-30.6%, the moisture regain is 25.9-29.9%, the temperature rise after moisture absorption is 6.3-9.8℃, and the thermal shrinkage rate is 1.09-1.93% at 110℃.