A surface low reflection absorption film and preparation method thereof

By plating the first dielectric film, the metal film and the second dielectric film on the base substrate, combined with the anti-reflection film, the problem of imaging quality degradation caused by the high reflectivity of the metal film is solved, and better imaging effects and film layers are achieved. stability.

CN118465896BActive Publication Date: 2024-10-18DXS OPTICS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410910257.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-18
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

In optical applications, metal films cause poor imaging quality due to high surface reflection. The absorption rate of existing dielectric materials is insufficient to effectively solve this problem.

Method used

A surface low-reflection absorption film composed of a first dielectric film, a metal film and a second dielectric film is plated on a base substrate. These film layers are deposited through electron beam evaporation technology and combined with an anti-reflection film to optimize the film layer. Internal reflection and transmission properties.

Benefits of technology

It effectively reduces the high reflectivity of the metal film, improves the firmness and transmittance of the film layer, optimizes the imaging effect, enhances the bonding strength between the substrate and the dielectric film layer, and improves the stability of the film performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a surface low-reflection absorption film and a preparation method thereof, belonging to the technical field of optical thin films. The invention comprises a substrate and an absorption film, wherein the absorption film is plated on the surface of the substrate, and the absorption film comprises a first dielectric film, a metal film and a second dielectric film connected in sequence; the absorption film is plated by electron beam evaporation. The metal film provides absorption of the film layer, and the first dielectric film and the second dielectric film are used to eliminate the high reflectivity of the metal film and ensure that the internal reflection and transmission of the film layer meet the requirements of the optical system, thereby optimizing the stress of the entire film layer, making the film layer more excellent in firmness, making the bonding strength of the substrate and the dielectric film layer higher, and making the film performance stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical films, and in particular relates to a surface low-reflection absorption film and a preparation method thereof. Background Art

[0002] Metal films have unique properties in the field of optics, such as high reflectivity, cutoff bandwidth, weak polarization effect, and high absorptivity. These properties make metal films have broad application prospects in optical applications. However, metal films also have certain problems in the application process, such as the degradation of imaging quality caused by high surface reflection.

[0003] The high surface reflectivity of metal films causes part of the light to become stray light after multiple reflections and diffusion. These stray lights eventually reach the image plane, resulting in reduced image contrast, thus affecting the quality of the entire imaging system. For metal materials used alone, the reflectivity is very high after being prepared into metal films, which has a particularly significant impact on imaging quality.

[0004] Compared with metal materials, dielectric materials can be designed to achieve lower reflectivity. However, dielectric materials have only a small amount of weak absorption, which can be ignored. This makes dielectric materials unusable for the preparation of absorbing films.

[0005] In short, metal films have superior performance in the field of optics, but they also have certain problems in practical applications, such as the degradation of imaging quality caused by high reflectivity. Therefore, when designing and preparing optical systems, it is necessary to comprehensively consider the advantages and limitations of metal films to achieve better imaging effects. Summary of the invention

[0006] The object of the present invention is to provide a surface low-reflection absorption film and a preparation method thereof, so as to solve the problem of poor imaging effect caused by high surface reflection of metal films.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A surface low-reflection absorption film comprises a substrate and an absorption film, wherein the absorption film is plated on the surface of the substrate and comprises a first dielectric film, a metal film and a second dielectric film connected in sequence.

[0009] As a preferred technical solution of the present invention, the material of the metal film is any one of metals Cr, Ti, Ni, Ta, and Nb.

[0010] As a preferred technical solution of the present invention, the material of the first dielectric film is any one of the metal oxides Al2O3, SiO2, Ta2O5, Ti3O5, and ZrO2.

[0011] As a preferred technical solution of the present invention, the material of the second dielectric film is any one of the metal oxides Al2O3, SiO2, Ta2O5, Ti3O5, and ZrO2.

[0012] As a preferred technical solution of the present invention, it also includes an anti-reflection film, one side of the anti-reflection film is connected to the base substrate, and the other side of the anti-reflection film is connected to the absorption film.

[0013] As a preferred technical solution of the present invention, the anti-reflection film is connected to the first dielectric film of the absorption film.

[0014] As a preferred technical solution of the present invention, the preparation of the antireflection film comprises the following steps:

[0015] A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 20-30 min, add potassium permanganate, continue stirring for 30-40 min, then heat to 40-50 ° C and stir for 2-3 h, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, take the solid phase and freeze-dry to obtain material A; the amount ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water and hydrogen peroxide solution is 1.8-2.2 g: 100 mL: 10-12 g: 100 mL: 10-12 mL;

[0016] A2, take the material A and deionized water, mix them, ultrasonically disperse them for 1-2h, then transfer them to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir them at 120-140°C for 4-6h, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 4-6mg:100mL:0.1-0.12g:0.1-0.12g;

[0017] A3, take the material B, casein, deionized water and mix them, reflux and stir at 65 ° C for 2-3h to obtain the first sol; the amount ratio of the material B, casein, and deionized water is 1-2g: 0.4-0.6g: 50mL;

[0018] A4, mix nano titanium dioxide, nano silicon dioxide, deionized water and anhydrous ethanol, stir for 10-20 minutes, add sodium dodecyl sulfate, and ultrasonically disperse for 2-3 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol and sodium dodecyl sulfate is 0.4-0.6g: 0.5-0.7g: 20-30mL: 15-20mL: 0.04-0.06g;

[0019] A5. Mix the first sol and the second sol, stir at 45-55°C for 6-8h, cool to room temperature, add glue solution, stir for 10-20min, and then apply it on the surface of the substrate to form the anti-reflection film after curing; the volume ratio of the first sol, the second sol and the glue solution is 1-1.5:0.8-1.2:0.02-0.03.

[0020] As a preferred technical solution of the present invention, the method for preparing the glue solution comprises the following steps:

[0021] Mix Sanzan gum and deionized water, stir for 10-12 hours, keep warm at 75-90°C for 15-25 minutes, cool to 45-55°C, adjust the pH to 10-11, continue stirring for 15-25 minutes, add aluminum sulfate, sodium trimetaphosphate and hyaluronic acid, continue stirring for 20-30 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution.

[0022] As a preferred technical solution of the present invention, the dosage ratio of the tri-zan gum, deionized water, aluminum sulfate, sodium trimetaphosphate and hyaluronic acid is 0.2-0.4g:100mL:0.04-0.06g:0.02-0.03g:0.01-0.02g.

[0023] The method for preparing the above-mentioned surface low-reflection absorption film comprises the following steps:

[0024] S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it into a fixture;

[0025] S2, placing the substrate loaded into the fixture on the workpiece rack, coating the anti-reflection film, and curing;

[0026] S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and coating a first dielectric film by electron beam evaporation, with a deposition rate of 2-4 A / S and an electron beam current of 100-300 mA;

[0027] S4, using electron beam evaporation to deposit metal film, the evaporation rate is 1A / S, and the electron beam current is 60-400mA;

[0028] S5. Electron beam evaporation is used to deposit a second dielectric film at a deposition rate of 2-4A / S and an electron beam current of 100-300mA, thereby obtaining the surface low-reflection absorption film.

[0029] Beneficial effects of the present invention:

[0030] The present invention discloses a surface low-reflection absorption film and a preparation method thereof. The metal film provides absorption of the film layer, and utilizes the first dielectric film and the second dielectric film to eliminate the high reflectivity of the metal film and ensure that the internal reflection and transmission of the film layer meet the requirements of the optical system, thereby optimizing the stress of the entire film layer, making the film layer more durable, making the bonding strength between the substrate and the dielectric film layer higher, and stabilizing the film performance. DETAILED DESCRIPTION

[0031] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments. Example 1

[0032] A method for preparing a surface low-reflection absorption film comprises the following steps:

[0033] S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it into a fixture;

[0034] S2, placing the substrate loaded into the fixture on the workpiece holder, coating the anti-reflection film, and curing the anti-reflection film to obtain an anti-reflection film with a thickness of 70 nm;

[0035] S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and using electron beam evaporation to coat a first dielectric film of Al2O3 material with a thickness of 100 nm, with a deposition rate of 2A / S and an electron beam current of 100 mA;

[0036] S4, using electron beam evaporation to deposit a Cr metal film with a thickness of 100 nm, the evaporation rate is 1A / S, and the electron beam current is 60mA;

[0037] S5. Electron beam evaporation is used to deposit a second dielectric film of ZrO2 with a thickness of 100 nm, the deposition rate is 2A / S, and the electron beam current is 100 mA, thereby obtaining the surface low-reflection absorption film.

[0038] The preparation of the antireflection film comprises the following steps:

[0039] A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 20 min, add potassium permanganate, continue stirring for 30 min, then heat to 40°C and stir for 2 h, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, freeze-dry the solid phase to obtain material A; the ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water, and hydrogen peroxide solution is 1.8 g: 100 mL: 10 g: 100 mL: 10 mL; the mass fraction of sulfuric acid in the concentrated sulfuric acid is 98%; the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30%;

[0040] A2, take the material A and deionized water, mix them, ultrasonically disperse them for 1 hour, then transfer them to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir them at 120°C for 4 hours, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 4 mg: 100 mL: 0.1 g: 0.1 g;

[0041] A3, taking the material B, casein, and deionized water, mixing them, refluxing and stirring at 65° C. for 2 h, to obtain the first sol; the dosage ratio of the material B, casein, and deionized water is 1 g: 0.4 g: 50 mL;

[0042] A4, nano titanium dioxide, nano silicon dioxide, deionized water, and anhydrous ethanol were mixed, stirred for 10 minutes, sodium dodecyl sulfate was added, and ultrasonic dispersion was performed for 2 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol, and sodium dodecyl sulfate was 0.4g:0.5g:20mL:15mL:0.04g;

[0043] A5. Mix the first sol and the second sol, stir at 45°C for 6 hours, cool to room temperature, add glue solution, stir for 10 minutes, and then apply it on the surface of the substrate to form the anti-reflection film after curing; the volume ratio of the first sol, the second sol and the glue solution is 1:0.8:0.02.

[0044] The preparation method of the glue solution comprises the following steps:

[0045] Mix Tri-Zan gum and deionized water, stir for 10 hours, keep warm at 75°C for 15 minutes, cool to 45°C, adjust the pH to 10, continue stirring for 15 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 20 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Tri-Zan gum, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.2g:100mL:0.04g:0.02g:0.01g. Example 2

[0046] A method for preparing a surface low-reflection absorption film comprises the following steps:

[0047] S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it into a fixture;

[0048] S2, placing the substrate loaded into the fixture on the workpiece holder, coating the anti-reflection film, and curing the anti-reflection film to obtain an anti-reflection film with a thickness of 80 nm;

[0049] S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and using electron beam evaporation to coat a first dielectric film of SiO2 with a thickness of 200 nm, with a deposition rate of 2.5 A / S and an electron beam current of 150 mA;

[0050] S4, using electron beam evaporation to deposit a Ti metal film with a thickness of 200 nm, the evaporation rate is 1A / S, and the electron beam current is 120mA;

[0051] S5. A second dielectric film made of Ti3O5 with a thickness of 200 nm is deposited by electron beam evaporation at a deposition rate of 3A / S and an electron beam current of 150 mA, thereby obtaining the surface low-reflection absorption film.

[0052] The preparation of the antireflection film comprises the following steps:

[0053] A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 22 minutes, add potassium permanganate, continue stirring for 32 minutes, then heat to 42°C and stir for 2.5 hours, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, freeze-dry the solid phase to obtain material A; the ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water, and hydrogen peroxide solution is 1.9g:100mL:11g:100mL:11mL; the mass fraction of sulfuric acid in the concentrated sulfuric acid is 98%; the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30%;

[0054] A2, take the material A and deionized water, mix them, ultrasonically disperse them for 1.2 hours, then transfer them to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir them at 125°C for 5 hours, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 5 mg: 100 mL: 0.11 g: 0.11 g;

[0055] A3, take the material B, casein, deionized water and mix them, reflux and stir at 65 ° C for 2.5 hours to obtain the first sol; the dosage ratio of the material B, casein and deionized water is 1.5g:0.45g:50mL;

[0056] A4, nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol were mixed, stirred for 15 minutes, sodium dodecyl sulfate was added, and ultrasonic dispersion was performed for 2-3 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol, and sodium dodecyl sulfate was 0.5g: 0.58g: 25mL: 17mL: 0.05g;

[0057] A5. Mix the first sol and the second sol, stir at 50°C for 7h, cool to room temperature, add glue solution, stir for 15min, and then apply it on the surface of the substrate to form the anti-reflection film after curing; the volume ratio of the first sol, the second sol and the glue solution is 1.2:0.9:0.025.

[0058] The preparation method of the glue solution comprises the following steps:

[0059] Mix Trimethicone and deionized water, stir for 11 hours, keep warm at 85°C for 20 minutes, cool to 48°C, adjust the pH to 10.2, continue stirring for 18 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 25 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Trimethicone, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.3g:100mL:0.05g:0.025g:0.015g. Example 3

[0060] A method for preparing a surface low-reflection absorption film comprises the following steps:

[0061] S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it into a fixture;

[0062] S2, placing the substrate loaded into the fixture on the workpiece holder, coating the anti-reflection film, and curing the anti-reflection film to obtain an anti-reflection film with a thickness of 90 nm;

[0063] S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and using electron beam evaporation to coat a first dielectric film of Ta2O5 material with a thickness of 150 nm, with a deposition rate of 3.2 A / S and an electron beam current of 200 mA;

[0064] S4, using electron beam evaporation to deposit a Ni metal film with a thickness of 200 nm, the evaporation rate is 1 A / S, and the electron beam current is 200 mA;

[0065] S5. Electron beam evaporation is used to deposit a second dielectric film of Ta2O5 with a thickness of 150 nm at a deposition rate of 3.4 A / S and an electron beam current of 200 mA, thereby obtaining the surface low-reflection absorption film.

[0066] The preparation of the antireflection film comprises the following steps:

[0067] A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 28 minutes, add potassium permanganate, continue stirring for 36 minutes, then heat to 48°C and stir for 2.8 hours, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, freeze-dry the solid phase to obtain material A; the ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water, and hydrogen peroxide solution is 2g:100mL:11.2g:100mL:11.3mL; the mass fraction of sulfuric acid in the concentrated sulfuric acid is 98%; the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30%;

[0068] A2, take the material A, deionized water, mix, ultrasonically disperse for 1.7h, then transfer to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir at 137°C for 5.5h, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 5.2mg:100mL:0.11g:0.11g;

[0069] A3, take the material B, casein, deionized water and mix them, reflux and stir at 65 ° C for 2.8 hours to obtain the first sol; the dosage ratio of the material B, casein and deionized water is 1.8g:0.55g:50mL;

[0070] A4, nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol were mixed, stirred for 18 minutes, sodium dodecyl sulfate was added, and ultrasonic dispersion was performed for 2.5 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol, and sodium dodecyl sulfate was 0.55g: 0.65g: 28mL: 17mL: 0.05g;

[0071] A5. Mix the first sol and the second sol, stir at 52°C for 7h, cool to room temperature, add glue solution, stir for 18min, and then apply it on the surface of the substrate to form the anti-reflection film after curing; the volume ratio of the first sol, the second sol and the glue solution is 1.4:1.1:0.027.

[0072] The preparation method of the glue solution comprises the following steps:

[0073] Mix Sanzan gum and deionized water, stir for 11 hours, keep warm at 85°C for 22 minutes, cool to 52°C, adjust the pH to 10.8, continue stirring for 22 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 26 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Sanzan gum, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.33g:100mL:0.053g:0.027g:0.018g. Example 4

[0074] A method for preparing a surface low-reflection absorption film comprises the following steps:

[0075] S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it into a fixture;

[0076] S2, placing the substrate loaded into the fixture on the workpiece holder, coating the anti-reflection film, and curing the anti-reflection film to obtain an anti-reflection film with a thickness of 100 nm;

[0077] S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and using electron beam evaporation to coat a first dielectric film of Ti3O5 material with a thickness of 120 nm, with a deposition rate of 3.8 A / S and an electron beam current of 280 mA;

[0078] S4, using electron beam evaporation to deposit a Ta metal film with a thickness of 120 nm, the evaporation rate is 1A / S, and the electron beam current is 380mA;

[0079] S5. Electron beam evaporation is used to deposit a second dielectric film made of SiO2 with a thickness of 120 nm, the deposition rate is 3.8 A / S, and the electron beam current is 280 mA, so as to obtain the surface low reflection absorption film.

[0080] The preparation of the antireflection film comprises the following steps:

[0081] A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 28 minutes, add potassium permanganate, continue stirring for 39 minutes, then heat to 49°C and stir for 2.9 hours, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, freeze-dry the solid phase to obtain material A; the ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water, and hydrogen peroxide solution is 2.1g:100mL:11.8g:100mL:11.8mL; the mass fraction of sulfuric acid in the concentrated sulfuric acid is 98%; the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30%;

[0082] A2, take the material A, deionized water, mix, ultrasonically disperse for 1.8h, then transfer to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir at 138°C for 5.8h, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 5.8mg:100mL:0.11g:0.11g;

[0083] A3, take the material B, casein, deionized water and mix them, reflux and stir at 65 ° C for 2.6 hours to obtain the first sol; the dosage ratio of the material B, casein and deionized water is 1.8g:0.58g:50mL;

[0084] A4, nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol were mixed, stirred for 18 minutes, sodium dodecyl sulfate was added, and ultrasonic dispersion was performed for 2.8 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol, and sodium dodecyl sulfate was 0.58g: 0.68g: 28mL: 19mL: 0.058g;

[0085] A5. Mix the first sol and the second sol, stir at 53°C for 7h, cool to room temperature, add glue solution, stir for 18min, and then apply it on the surface of the substrate to form the anti-reflection film after curing; the volume ratio of the first sol, the second sol and the glue solution is 1.4:1.1:0.029.

[0086] The preparation method of the glue solution comprises the following steps:

[0087] Mix Tri-Zan gum and deionized water, stir for 11 hours, keep warm at 88°C for 24 minutes, cool to 53°C, adjust the pH to 10.8, continue stirring for 23 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 27 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Tri-Zan gum, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.38g:100mL:0.056g:0.025g:0.018g. Example 5

[0088] A method for preparing a surface low-reflection absorption film comprises the following steps:

[0089] S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it into a fixture;

[0090] S2, placing the substrate loaded into the fixture on the workpiece holder, coating the anti-reflection film, and curing the anti-reflection film to obtain an anti-reflection film with a thickness of 70 nm;

[0091] S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and using electron beam evaporation to coat a first dielectric film of ZrO2 with a thickness of 100 nm, with a deposition rate of 4 A / S and an electron beam current of 300 mA;

[0092] S4, using electron beam evaporation to deposit a metal film of Nb material with a thickness of 100 nm, the evaporation rate is 1A / S, and the electron beam current is 400mA;

[0093] S5. Electron beam evaporation is used to deposit a second dielectric film of Al2O3 with a thickness of 100 nm, the deposition rate is 4A / S, and the electron beam current is 300 mA, so as to obtain the surface low reflection absorption film.

[0094] The preparation of the antireflection film comprises the following steps:

[0095] A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 30 min, add potassium permanganate, continue stirring for 40 min, then heat to 50°C and stir for 3 h, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, freeze-dry the solid phase to obtain material A; the ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water, and hydrogen peroxide solution is 2.2 g: 100 mL: 12 g: 100 mL: 12 mL; the mass fraction of sulfuric acid in the concentrated sulfuric acid is 98%; the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30%;

[0096] A2, take the material A and deionized water, mix them, ultrasonically disperse them for 2 hours, then transfer them to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir them at 140°C for 6 hours, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 6 mg: 100 mL: 0.12 g: 0.12 g;

[0097] A3, taking the material B, casein, and deionized water, mixing them, refluxing and stirring at 65° C. for 3 h, to obtain the first sol; the dosage ratio of the material B, casein, and deionized water is 2g:0.6g:50mL;

[0098] A4, nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol were mixed, stirred for 20 minutes, sodium dodecyl sulfate was added, and ultrasonic dispersion was performed for 3 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol, and sodium dodecyl sulfate was 0.6g: 0.7g: 30mL: 20mL: 0.06g;

[0099] A5. Mix the first sol and the second sol, stir at 55°C for 8h, cool to room temperature, add glue solution, stir for 20min, and then apply it on the surface of the substrate to form the anti-reflection film after curing; the volume ratio of the first sol, the second sol and the glue solution is 1.5:1.2:0.03.

[0100] The preparation method of the glue solution comprises the following steps:

[0101] Mix Trimethicone and deionized water, stir for 12 hours, keep warm at 90°C for 25 minutes, cool to 55°C, adjust the pH to 11, continue stirring for 25 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 30 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Trimethicone, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.4g:100mL:0.06g:0.03g:0.02g.

[0102] Comparative Example 1

[0103] The difference from Example 1 is that hydroxylated double-walled carbon nanotubes are not added in the preparation of the antireflection film.

[0104] Comparative Example 2

[0105] The difference from Example 1 is that no graphite powder is added in the preparation of the antireflection film.

[0106] Comparative Example 3

[0107] The difference from Example 1 is that casein is not added in the preparation of the antireflection film.

[0108] Comparative Example 4

[0109] The difference from Example 1 is that the first sol is not added in the preparation of the antireflection film.

[0110] Comparative Example 5

[0111] The difference from Example 1 is that the second sol is not added in the preparation of the antireflection film.

[0112] Comparative Example 6

[0113] The difference from Example 1 is that nano titanium dioxide is not added in the preparation of the antireflection film.

[0114] Comparative Example 7

[0115] The difference from Example 1 is that nano-silicon dioxide is not added in the preparation of the antireflection film.

[0116] Comparative Example 8

[0117] The difference from Example 1 is that the preparation method of the glue solution comprises the following steps:

[0118] Mix Trimethicone and deionized water, stir for 10 hours, keep warm at 75°C for 15 minutes, cool to 45°C, adjust the pH to 10, continue stirring for 15 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 20 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Trimethicone, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.2g:100mL:0.06g:0g:0.01g.

[0119] Comparative Example 9

[0120] The difference from Example 1 is that the preparation method of the glue solution comprises the following steps:

[0121] Mix Sanzan gum and deionized water, stir for 10 hours, keep warm at 75°C for 15 minutes, cool to 45°C, adjust the pH to 10, continue stirring for 15 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 20 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Sanzan gum, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.2g:100mL:0g:0.06g:0.01g.

[0122] Comparative Example 10

[0123] The difference from Example 1 is that the preparation method of the glue solution comprises the following steps:

[0124] Mix Tri-Zan gum and deionized water, stir for 10 hours, keep warm at 75°C for 15 minutes, cool to 45°C, adjust the pH to 10, continue stirring for 15 minutes, add aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid, continue stirring for 20 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution; the dosage ratio of Tri-Zan gum, deionized water, aluminum sulfate, sodium trimetaphosphate, and hyaluronic acid is 0.2g:100mL:0.04g:0.03g:0g.

[0125] Performance Testing

[0126] The surface low-reflection absorption films prepared in Examples 1-5 and Comparative Examples 1-10 were tested for internal reflectivity, external reflectivity, transmittance, and absorptivity of the film layer under a light wave condition of a wavelength of 632.8 nm. The adhesion was tested by pulling the same position 10 times with 3M tape. The test results are shown in Table 1 below.

[0127] Table 1

[0128]

[0129] From Table 3, we can see that:

[0130] The diaphragms prepared in Examples 1-5 of the present application have appropriate internal reflectivity and absorptivity of the film layer for a light wave of 632.8 nm; have a lower external reflectivity and a higher film transmittance; the anti-reflection films prepared in Examples 1-5 of the present application have excellent transmission effects on light waves of 632.8 nm; the anti-reflection films prepared in Examples 1-5 of the present application have excellent absorption effects on light waves of 632.8 nm, and the absorptivity of the film layer light is improved through the synergistic effect between the first sol, the second sol, and hyaluronic acid; the diaphragms prepared in Examples 1-5 of the present application have excellent film layer firmness, and a supporting film layer is formed through the interaction between carbon nanotubes and graphene, so that the first dielectric film is firmly deposited on the anti-reflection film, and SiO2-TiO2 is used as an intermediate layer, which synergistically increases the bonding performance with the glue to improve the firmness between the film layers.

[0131] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A surface low reflection absorption film, comprising a substrate, characterized in that: It also includes an absorption film, which is plated on the surface of the substrate, and includes a first dielectric film, a metal film, and a second dielectric film connected in sequence; It also includes an anti-reflection film, one side of the anti-reflection film is connected to the substrate, and the other side of the anti-reflection film is connected to the absorption film; The antireflection film is connected to the first dielectric film of the absorption film; The preparation of the antireflection film comprises the following steps: A1. Mix graphite powder and concentrated sulfuric acid, stir in an ice-water bath for 20-30 min, add potassium permanganate, continue stirring for 30-40 min, then heat to 40-50 ° C and stir for 2-3 h, add deionized water, cool to room temperature, add hydrogen peroxide solution, centrifuge, take the solid phase and freeze-dry to obtain material A; the amount ratio of graphite powder, concentrated sulfuric acid, potassium permanganate, deionized water and hydrogen peroxide solution is 1.8-2.2 g: 100 mL: 10-12 g: 100 mL: 10-12 mL; A2, take the material A and deionized water, mix them, ultrasonically disperse them for 1-2h, then transfer them to a polytetrafluoroethylene hydrothermal reactor, add hydroxylated double-walled carbon nanotubes and sodium ascorbate, stir them at 120-140°C for 4-6h, cool, filter, wash the solid phase, freeze-dry, and obtain material B; the dosage ratio of the material A, deionized water, hydroxylated double-walled carbon nanotubes, and sodium ascorbate is 4-6mg:100mL:0.1-0.12g:0.1-0.12g; A3, take the material B, casein, deionized water and mix them, reflux and stir at 65 ° C for 2-3h to obtain the first sol; the amount ratio of the material B, casein, and deionized water is 1-2g: 0.4-0.6g: 50mL; A4, mix nano titanium dioxide, nano silicon dioxide, deionized water and anhydrous ethanol, stir for 10-20 minutes, add sodium dodecyl sulfate, and ultrasonically disperse for 2-3 hours to obtain a second sol; the dosage ratio of the nano titanium dioxide, nano silicon dioxide, deionized water, anhydrous ethanol and sodium dodecyl sulfate is 0.4-0.6g: 0.5-0.7g: 20-30mL: 15-20mL: 0.04-0.06g; A5, mixing the first sol and the second sol, stirring at 45-55°C for 6-8h, cooling to room temperature, adding the glue solution, stirring for 10-20min, and then coating the surface of the substrate, and forming the antireflection film after curing; the volume ratio of the first sol, the second sol, and the glue solution is 1-1.5:0.8-1.2:0.02-0.03; The preparation method of the glue solution comprises the following steps: Mix Sanzan gum and deionized water, stir for 10-12 hours, keep warm at 75-90°C for 15-25 minutes, cool to 45-55°C, adjust the pH to 10-11, continue stirring for 15-25 minutes, add aluminum sulfate, sodium trimetaphosphate and hyaluronic acid, continue stirring for 20-30 minutes, cool to room temperature, filter, take the liquid phase and adjust the pH to neutral to obtain the glue solution.

2. A surface low reflection absorption film according to claim 1, characterized in that: The material of the metal film is any one of metals Cr, Ti, Ni, Ta, and Nb.

3. The surface low reflection absorption film according to claim 1, characterized in that: The material of the first dielectric film is any one of metal oxides Al2O3, SiO2, Ta2O5, Ti3O5, and ZrO2.

4. The surface low reflection absorption film according to claim 1, characterized in that: The material of the second dielectric film is any one of metal oxides Al2O3, SiO2, Ta2O5, Ti3O5, and ZrO2.

5. The surface low reflection absorption film according to claim 1, characterized in that: The dosage ratio of the tri-zan gum, deionized water, aluminum sulfate, sodium trimetaphosphate and hyaluronic acid is 0.2-0.4g:100mL:0.04-0.06g:0.02-0.03g:0.01-0.02g.

6. A method for preparing a surface low-reflection absorption film according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Wipe the polished substrate clean with a mixture of ethanol and ether and place it in a fixture; S2, placing the substrate loaded into the fixture on the workpiece rack, coating the anti-reflection film, and curing; S3, placing the substrate coated with the antireflection film into a vacuum coating machine and starting to evacuate the air until the vacuum degree is less than or equal to 3 Pa, and coating a first dielectric film by electron beam evaporation; S4, depositing a metal film by electron beam evaporation; S5. Form a second dielectric film by electron beam evaporation to obtain the surface low-reflection absorption film.

Citation Information

Patent Citations

  • Electric control terahertz antireflection film based on graphene, manufacturing method and using method

    CN103984051A

  • Preparation method for N-doped grapheme / carbon nano tube aerogel electrode

    CN107622879A