Solid oxide fuel cell with gradient structure and preparation method thereof

By introducing a transition layer and a composite cathode layer between the cathode layer and barrier layer of SOFC, the problem of mismatch in thermal expansion performance of each layer structure of SOFC is solved, the reliability and durability of the battery are improved, and its service life is extended.

CN118472276BActive Publication Date: 2024-10-29CHINA UNIV OF PETROLEUM (EAST CHINA)

Patent Information

Application Number
CN202410926077.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-29
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

In solid oxide fuel cells (SOFC), under high-temperature continuous operation and hot and cold cycle conditions, due to mismatch in thermal expansion performance of each layer structure, electrode materials fall off and the structure is broken, affecting power generation performance and life.

Method used

A transition layer with a moderate thermal expansion coefficient is introduced between the cathode layer and the barrier layer, and a composite cathode layer matching the thermal expansion coefficient of the transition layer is prepared. The LSC/GDC ratio is optimized through a multi-criteria decision analysis method to improve thermal expansion performance and electrical conductivity. Inhibits the diffusion of strontium elements.

Benefits of technology

It effectively solves the problem of thermal expansion mismatch between the various layers of SOFC, improves the reliability and durability of single cells, and extends the service life under continuous operation and hot and cold cycle conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118472276B_ABST
    Figure CN118472276B_ABST
Patent Text Reader

Abstract

The present invention discloses a solid oxide fuel cell with a gradient structure and a preparation method thereof, belonging to the technical field of fuel cells. The fuel cell comprises a plurality of layers of single cells stacked in sequence, wherein the single cell comprises an anode support layer, an anode functional layer, an electrolyte layer, a barrier layer, a transition layer and a composite cathode layer stacked in sequence; the anode support layer and the anode functional layer are NiO-3YSZ layer and NiO-8YSZ layer respectively, the electrolyte layer is a YSZ layer, the barrier layer is a GDC layer, and the transition layer is an LSC x GDC 1‑x layer, 0.5≤x<1, the composite cathode layer is LSC y GDC 1‑y Layer, 0.5≤y<1, and x<y. The present invention introduces a transition layer with a moderate thermal expansion coefficient between the cathode layer and the barrier layer, and prepares a composite cathode layer whose thermal expansion coefficient matches that of the transition layer, thereby effectively solving the problem of mismatched thermal expansion performance between the layers of the single cell structure, and significantly enhancing the reliability and durability of the SOFC single cell while ensuring high power generation performance, thereby improving the service life of the SOFC.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid oxide fuel cells, and in particular to a solid oxide fuel cell with a gradient structure and a preparation method thereof. Background Art

[0002] Solid Oxide Fuel Cell (SOFC) is an electrochemical device that directly converts the chemical energy in fossil fuels into electrical energy under medium-high temperature (600-1000℃) conditions. There is no combustion process and mechanical movement, and the reaction product is only water. It has the advantages of high efficiency, zero pollution, and low noise. In order to meet the demand for long-life SOFC in commercial applications, SOFC must be able to withstand temperature fluctuations caused by long-term continuous operation and frequent start-stop conditions. When SOFC is in service under high-temperature continuous operation and hot and cold cycle conditions, a temperature gradient will form inside the SOFC stack and cause uneven temperature distribution. In addition, due to the mismatch of thermal expansion behavior between the layers of the single cell structure (electrolyte, cathode, barrier layer and anode), large stress and strain will be introduced. The electrode material, electrolyte and connector will undergo different degrees of volume expansion, which can easily cause the electrode material to fall off from the electrolyte. In addition, the fragility of ceramic materials will cause sudden failures such as deformation, delamination and cracking of the single cell, and structural fragmentation, which will eventually cause the SOFC power generation performance to decline, seriously affecting the operating life and safety and stability of SOFC.

[0003] Since LSC (La 0.6 Sr 0.4 CoO 3-δ , referred to as LSC material) has a high catalytic performance for O2 and is often used as the cathode material of SOFC; in addition, the electrolyte of SOFC often uses YSZ material. During service, LSC cathode is prone to interface reaction and element diffusion with YSZ electrolyte, which affects battery performance and life. In order to solve these problems, GDC (Ce 0.9 G 0.1 O 1.95 CeO2-based materials such as GDC (Gel-free DC) are often used to prepare barrier layers between electrolytes and cathodes, which can prevent the formation of high-impedance reactants and the diffusion of Sr elements. However, there is still a significant difference in the thermal expansion properties of the GDC barrier layer and the LSC cathode layer material, which leads to electrode material cracking and electrode damage in SOFC cells under long-term high-temperature continuous operation and hot and cold cycle conditions. Therefore, it is urgent to develop a high-performance and long-life SOFC cell with a gradient structure to alleviate the mismatch in the thermal expansion coefficients of the LSC cathode material and the GDC barrier layer, and to improve the reliability and durability of the SOFC cell while ensuring high power generation performance. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a solid oxide fuel cell with a gradient structure and a preparation method thereof, which effectively solves the problem of mismatch in thermal expansion performance between the various layer structures of a SOFC single cell by introducing a transition layer with a moderate thermal expansion coefficient between the cathode layer and the barrier layer and preparing a composite cathode layer with a thermal expansion coefficient matching that of the transition layer.

[0005] The technical solution adopted by the present invention is:

[0006] The present invention provides a solid oxide fuel cell with a gradient structure, wherein the fuel cell is composed of a plurality of layers of single cells, a sealing layer and a connector stacked together, wherein each layer of the single cell comprises an anode support layer, an anode functional layer, an electrolyte layer, a barrier layer, a transition layer and a composite cathode layer stacked in sequence;

[0007] The anode support layer and the anode functional layer are respectively a NiO-3YSZ layer and a NiO-8YSZ layer;

[0008] The electrolyte layer is a YSZ layer;

[0009] The barrier layer is a GDC layer;

[0010] The transition layer is LSC x GDC 1-x Layer, 0<x<1;

[0011] The composite cathode layer is LSC y GDC 1-y Layer, 0<y<1.

[0012] Furthermore, in the transition layer, 0.5≤x<1, in the composite cathode layer, 0.5≤y<1, and x<y.

[0013] Furthermore, the thickness of the anode support layer is 300-500 μm;

[0014] The thickness of the anode functional layer is 5-20 μm;

[0015] The thickness of the electrolyte layer is 5 to 20 μm;

[0016] The thickness of the barrier layer is 5-20 μm;

[0017] The thickness of the transition layer is 2-10 μm;

[0018] The thickness of the composite cathode layer is 10-50 μm.

[0019] The present invention also provides a method for preparing a solid oxide fuel cell having a gradient structure, comprising the steps of:

[0020] S1. Determine the constituent materials, dimensions and preparation process of each layer structure of the single cell, and prepare the corresponding powder materials and slurries of the anode support layer, anode functional layer, electrolyte layer, barrier layer, transition layer with different LSC / GDC ratios, and composite cathode layer with different LSC / GDC ratios;

[0021] S2. Prepare test samples with different LSC / GDC ratios and barrier layer test samples, and test the physical properties of the test samples with different LSC / GDC ratios, including thermal expansion coefficient, electrical conductivity, activation energy, phase transition temperature and mechanical strength, and the thermal expansion coefficient of the barrier layer test samples;

[0022] S3, according to the thermal expansion coefficient, electrical conductivity, activation energy, phase transition temperature and mechanical strength parameters of the test samples with different LSC / GDC ratios obtained in step S2, the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer are determined by a multi-criteria decision analysis method;

[0023] S4, determining the size and preparation process of the single cell, and preparing an anode-supported flat-plate single cell with a gradient structure according to the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer determined in step S3;

[0024] S5. Perform hot and cold cycle and continuous operation tests on the single cell prepared in step S4, monitor the temperature, voltage and current curves during the hot and cold cycle and continuous operation as a function of the operation time, monitor the polarization curves and electrochemical impedance spectrum during the hot and cold cycle and continuous operation, and evaluate the performance at a current density of 300 mA / cm 2 When the voltage attenuation rate is ≤50%, whether the number of hot and cold cycle services of the single cell is ≥50 times and the continuous operation time is ≥2500h. If it does not meet the set requirements, adjust the LSC / GDC ratio of the transition layer and the composite cathode layer in step S3, and re-prepare a new gradient structure SOFC single cell until it meets the set requirements.

[0025] Further, the step S3 is specifically: by analyzing the thermal expansion coefficient, conductivity, activation energy, phase transition temperature and mechanical strength of the test samples with different LSC / GDC ratios in step S2, the weighted summation model method in the multi-criteria decision analysis method is used to perform weighted scoring on the comprehensive performance of the test samples with different LSC / GDC ratios, so as to determine the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer in the gradient structure single cell. The specific implementation steps are as follows:

[0026] (1) Determine the evaluation parameters: conductivity (σ), thermal expansion coefficient difference (Δα), activation energy (E a), phase transition temperature (T0), mechanical strength (R), where the thermal expansion coefficient difference (Δα) refers to the percentage difference between the test sample and the barrier layer at different LSC / GDC ratios;

[0027] (2) Weight assignment: Assign a weight w to each evaluation parameter i , the weight reflects the importance of each evaluation parameter in the decision-making, and the sum of all weights is 1, that is:

[0028] ;

[0029] in, is the weight of the evaluation parameter, is the serial number of the evaluation parameter, is the total number of evaluation parameters;

[0030] (3) Evaluation parameter scoring: For each alternative material or solution Each evaluation parameter in Score, record ;

[0031] (4) Calculate weighted scores: For each alternative Calculating weighted scores ,Right now:

[0032] ;

[0033] in, For the The weighted scores of the alternative materials or alternative solutions, For each alternative material or alternative Each evaluation parameter in Ratings;

[0034] (5) Scheme ranking and selection: based on the calculated weighted score All alternatives are ranked, and the one with the highest weighted score is selected as the optimal solution, thereby determining the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer.

[0035] Furthermore, the step S4 is specifically as follows:

[0036] S41, preparing a half-cell consisting of an anode support layer, an anode functional layer, and an electrolyte layer;

[0037] S42, screen printing 1 to 3 layers of barrier layer slurry on the electrolyte layer of the half-cell, drying for 5 to 20 minutes after each screen printing, and sintering at 1000 to 1500° C. for 2 to 8 hours after all screen printing;

[0038] S43, screen printing 1 to 3 layers of transition layer slurry on the sintered barrier layer, drying for 5 to 20 minutes after each screen printing, and sintering at 1000 to 1500° C. for 2 to 8 hours after all screen printing;

[0039] S44. Screen print 1 to 3 layers of composite cathode layer slurry on the sintered transition layer, dry for 5 to 20 minutes after each screen printing, and sinter at 1000 to 1500°C for 2 to 8 hours after all screen printing; then, after debinding, sintering and leveling, a gradient structured anode-supported flat-plate solid oxide fuel cell is obtained.

[0040] Furthermore, the step S41 is specifically as follows: firstly, an anode supporting layer is prepared by a tape casting method or an immersion precipitation phase inversion method, and after it is formed, it is cut and dried for 5 to 20 minutes to obtain an anode supporting layer blank; then, 1 to 3 layers of anode functional layer slurry are screen-printed on the anode supporting layer blank, and each screen printing is followed by drying for 5 to 20 minutes, and then 1 to 3 layers of electrolyte layer slurry are screen-printed on the anode functional layer, and each screen printing is followed by drying for 5 to 20 minutes to obtain a half-cell blank, and the half-cell blank is subjected to binder removal and sintering and leveling to obtain a half-cell.

[0041] Furthermore, in step S41, the debinding temperature of the half-cell blank is 1000-1500° C., the debinding time is 2-8 hours, the sintering temperature is 1000-1500° C., and the sintering time is 5-10 hours.

[0042] Furthermore, in step S44, the debinding temperature is 1000-1500° C., the debinding time is 2-8 hours, and the sintering temperature after debinding is 1000-1500° C., and the sintering time is 5-10 hours.

[0043] The beneficial effects of the present invention are:

[0044] (1) The present invention relates to a solid oxide fuel cell with a gradient structure and a preparation method thereof. By introducing a transition layer with a moderate thermal expansion coefficient between the cathode layer and the barrier layer and preparing a composite cathode layer whose thermal expansion coefficient matches that of the transition layer, the problem of thermal expansion performance mismatch between the layers of the SOFC single cell structure is effectively solved. In addition, during the determination process of the transition layer and the composite cathode layer, five key parameters, namely, conductivity, thermal expansion coefficient, activation energy, phase change temperature and mechanical strength, are analyzed and evaluated to ensure that they have good comprehensive performance.

[0045] (2) The transition layer and the composite cathode layer of the present invention both use LSC-GDC materials in different proportions. This design optimizes the interface between the cathode layer and the barrier layer, improves the microstructure of the single cell, promotes the transmission and adsorption of oxygen on the cathode side, and enhances the electrochemical reaction activity of the cathode layer material, effectively inhibits the migration and segregation of strontium (Sr) elements in the cathode layer, and reduces the interface polarization impedance. Under the premise of ensuring high power generation performance, the reliability and durability of the SOFC single cell are enhanced, and the service life of the SOFC under continuous operation and hot and cold cycle conditions is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0047] Figure 1 A process flow chart for preparing a single cell according to the present invention;

[0048] Figure 2 A schematic diagram of the structure of a single cell prepared according to an embodiment of the present invention;

[0049] Figure 3 This is a schematic diagram of the structure of a single cell prepared in Comparative Example 1 of the present invention;

[0050] Figure 4 This is a schematic diagram of the structure of a single cell prepared in Comparative Example 2 of the present invention;

[0051] Figure 5 This is a schematic diagram of the structure of a single cell prepared in Comparative Example 3 of the present invention;

[0052] Figure 6 IVP curves of the single cells prepared in the embodiment of the present invention and comparative examples 1-3 cycled 10 times, 5 times, 10 times, and 10 times respectively under hot and cold cycle conditions;

[0053] Figure 7 The IVP curves of the embodiment of the present invention are 1, 30 and 50 cycles under the hot and cold cycle conditions;

[0054] Figure 8 The microstructure of the single cells prepared in the embodiment of the present invention and comparative examples 1-3 after being used in hot and cold cycle conditions;

[0055] Fig. 9 The voltage-time curves of the single cells prepared in the embodiment of the present invention and comparative examples 1-3 under continuous operation conditions. DETAILED DESCRIPTION

[0056] The present invention provides a solid oxide fuel cell with a gradient structure and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0057] The present invention is described in detail below with reference to the accompanying drawings.

[0058] Example

[0059] Reference Figure 1 This embodiment provides a method for preparing a solid oxide fuel cell having a gradient structure, comprising the steps of:

[0060] S1. Determine the constituent materials of each layer structure of a single cell, and prepare the corresponding powder materials and slurry of anode support layer, anode functional layer, electrolyte layer, barrier layer, transition layer with different LSC / GDC ratios, and composite cathode layer with different LSC / GDC ratios.

[0061] The single cell structure in this embodiment specifically includes an anode support layer, an anode functional layer, an electrolyte layer, a barrier layer, a transition layer and a composite cathode layer stacked in sequence; wherein the anode support layer is NiO-3YSZ, the anode functional layer is NiO-8YSZ, the electrolyte layer is a YSZ layer, the barrier layer is a GDC layer, and the transition layer is LSC x GDC 1-x layer, 0<x<1, preferably 0.5≤x<1, the composite cathode layer is LSC y GDC 1-y Layer, 0<y<1, preferably 0.5≤y<1, and x<y.

[0062] In addition, the slurry preparation process of each layer structure of the single cell includes three steps: powder proportioning, ball milling and filtration, namely:

[0063] (1) Powder proportioning and weighing process: The powders of each layer of SOFC material were weighed and proportioned using an electronic scale. The anode support layer slurry consisted of NiO powder, TZ-3YS powder, pore former, binder and water, and the mass ratio of NiO powder, TZ-3YS powder and binder was 3:2:7; the anode functional layer slurry consisted of NiO powder, TZ-8YS powder, pore former, binder and water, and the mass ratio of NiO powder, TZ-8YS powder and binder was 3:2:7; the electrolyte slurry consisted of TZ-8YS powder, binder and water. Composition, the mass ratio of TZ-8YS powder to binder is 1:1; the barrier layer slurry is composed of GDC powder, pore former, binder and water, and the mass ratio of GDC powder to binder is 2:1; the transition layer slurry and the composite cathode layer slurry are composed of LSC powder, GDC powder, pore former, binder and water, and the mass ratio of LSC powder, GDC powder and binder is x:1-x:1, and the composite cathode layer is composed of LSC powder, GDC powder, pore former E, binder and water, and the mass ratio of LSC powder, GDC powder and binder is y:1-y:1;

[0064] (2) Ball milling process: put the powders into the ball milling jar of the planetary mill according to the above ratio and tighten them, turn on the planetary ball mill, set the speed to 100-300 rpm, and the ball milling time to 12-48 hours; the ball milling speed is 100-300 r / min;

[0065] (3) Filtration process: Use the disposable filter screen of the filter to filter out the mixed slurry in the planetary ball mill to obtain the slurry of each layer structure of SOFC.

[0066] S2. Prepare LSC / GDC layer test samples and barrier layer test samples with different ratios using the slurry of step (1). The test samples are cylindrical samples with a size of φ5 mm × 50 mm. Test the physical properties of the LSC / GDC layer test samples with different ratios, including thermal expansion coefficient, electrical conductivity, activation energy, phase change temperature and mechanical strength, and test the thermal expansion coefficient of the barrier layer.

[0067] It should be noted that since the transition layer and the composite cathode layer are both made of LSC and GDC, the two are only different in ratio. When determining the LSC / GDC ratio of the transition layer and the composite cathode layer, in order to simplify the testing process, when preparing the test samples, there is no need to separately prepare transition layer and composite cathode layer samples with different LSC / GDC ratios.

[0068] Specifically, in this step, when using a thermal expansion meter to measure the thermal expansion coefficient, it is necessary to convert the linear thermal expansion coefficient of the cylindrical sample obtained from the test into an average volume expansion coefficient. Specifically: install the cylindrical sample in the test fixture of the thermal expansion meter, ensure that the sample to be tested is fixed and stable, set the temperature range and heating rate required for the test, the test temperature of the SOFC electrode material usually needs to cover its operating temperature range, and set the test environment as needed, such as testing in high-purity air or inert gas to simulate actual working conditions; start the thermal expansion meter, start recording the dimensional changes of the sample to be tested during the heating process, and calculate the linear thermal expansion coefficient based on the length change data of the sample at different temperatures. The above test temperature range is 25~1100℃, and the heating rate is 5℃ / min. In this embodiment, the linear expansion coefficient of the barrier layer (GDC) test sample was tested using a thermal expansion meter, and the linear expansion coefficient of the LSC / GDC layer test samples with different ratios were tested, and the average volume expansion coefficient of the material was obtained based on the linear expansion coefficient analysis. The specific calculation formula is: Linear expansion coefficient It indicates the relative elongation (or contraction) along a certain direction when the temperature of the sample rises by 1°C. When the temperature changes from Rise to When Changes to , then its linear expansion coefficient for:

[0069]

[0070] in, is the test starting temperature, is the test end temperature, is the temperature difference of the sample, The change in length in the case.

[0071] Based on the linear expansion coefficient Get the average volume expansion coefficient of the material :

[0072]

[0073] Among them, T2 is the end temperature of the test, and T1 is the start temperature of the test.

[0074] The average volume expansion coefficient of the barrier layer test samples and the LSC / GDC layer test samples with different ratios at different temperatures (unit: 1×10 -6 K -1 ) as shown in Table 1.

[0075] Table 1

[0076]

[0077] It can be seen from Table 1 above that the average volume expansion coefficient of the barrier layer and the LSC / GDC layer with different ratios gradually increases with increasing temperature, and at the same temperature, the average volume expansion coefficient of the LSC / GDC layer decreases with increasing GDC specific gravity.

[0078] The performance of SOFC at 750℃ was analyzed. At 750℃, the thermal expansion coefficients of LSC / GDC=10 / 0, LSC / GDC=9 / 1, LSC / GDC=8 / 2, LSC / GDC=7 / 3, LSC / GDC=6 / 4 and LSC / GDC=5 / 5 were 17.954×10 -6 K -1 , 17.644×10 -6 K -1 ,16.408×10 -6 K -1 ,15.059×10 -6 K -1 , 14.529×10 -6 K -1 , 14.144×10 -6 K -1 ; The conductivity at 750℃ was 1918.59S·cm -1 、1440.81S·cm -1 、923.92S·cm -1 、793.00S·cm -1 、614.47S·cm -1 、80.58 S·cm -1 ; In addition, the activation energy, phase transition temperature and mechanical strength were detected. The activation energy was 0.0288 eV, 0.0334 eV, 0.0357 eV, 0.0368 eV, 0.0391 eV and 0.0426 eV, respectively; the phase transition temperatures were 850 ℃, 839 ℃, 824 ℃, 811 ℃ and 800 ℃, respectively; and the mechanical strengths were 151.14 MPa, 175.32 MPa, 187.41 MPa, 193.46 MPa, 205.55 MPa and 223.69 MPa, respectively.

[0079] The above-mentioned mechanical strength refers to the bending strength. All parts of the SOFC single cell are made of ceramic materials. The mechanical strength of ceramic materials is mainly based on bending strength, which is tested using a small punch testing machine.

[0080] S3. Based on the thermal expansion coefficient, electrical conductivity, activation energy, phase change temperature and mechanical strength parameters of the LSC / GDC layers with different ratios obtained in step S2 and the thermal expansion coefficient of the barrier layer, a multi-criteria decision analysis method is used to evaluate the performance of the transition layer and the composite cathode layer with different LSC / GDC ratios, and the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer are determined.

[0081] The step S3 specifically comprises: analyzing the conductivity (σ), thermal expansion coefficient difference (Δα), activation energy (E a ), phase transition temperature (T0), mechanical strength (R), and weighted scoring of the comprehensive performance of test samples with different LSC / GDC ratios using the weighted summation model method in the multi-criteria decision analysis method, so as to determine the LSC / GDC ratio of the transition layer in the gradient structure single cell and the LSC / GDC ratio of the composite cathode layer. The specific implementation steps are as follows:

[0082] (1) Determine the evaluation parameters: conductivity (σ), thermal expansion coefficient difference (Δα), activation energy (E a ), phase transition temperature (T0), mechanical strength (R), where the thermal expansion coefficient difference (Δα) refers to the percentage difference between the test sample and the barrier layer at different LSC / GDC ratios;

[0083] (2) Weight assignment: assign weights to each evaluation parameter , and the sum of all weights is 1, that is:

[0084]

[0085] in, is the weight of the evaluation parameter, which reflects the importance of each evaluation parameter in decision making. is the serial number of the evaluation parameter, is the total number of evaluation parameters;

[0086] (3) Evaluation parameter scoring: For each alternative material or alternative solution Each evaluation parameter in Score, record ;

[0087] (4) Calculate weighted scores: For each alternative material or alternative solution Calculating weighted scores ,Right now:

[0088]

[0089] in, For the The weighted score of each alternative material or alternative solution takes into account the influence of all evaluation parameters. For each alternative material or alternative Each evaluation parameter in The score indicates that the alternative materials or alternative solutions In the evaluation parameters Performance on

[0090] (5) Scheme ranking and selection: based on the calculated weighted score All alternatives are ranked, and the one with the highest weighted score is selected as the optimal solution, thereby determining the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer.

[0091] Among the above evaluation parameters, the conductivity (σ) of the electrode material directly affects the electrochemical performance of the single cell. The range of conductivity (σ) is 500~2000 S·cm -1 , the weight range of conductivity (σ) is 0.10~0.30; the thermal expansion coefficient is crucial to ensure the thermal matching between the materials of each layer of SOFC single cell, and directly affects the electrochemical and mechanical properties of the single cell during continuous operation and after continuous operation. The thermal expansion coefficient difference (Δα) refers to the difference between the transition layer with different LSC / GDC ratios and the composite cathode layer with different LSC / GDC ratios and the barrier layer. The range of the thermal expansion coefficient difference (Δα) is 0~100%, and the weight setting range is 0.10~0.50; the activation energy (E a ) refers to the minimum energy required for ions or electrons to jump from one position to another in an electrochemical reaction. The activation energy affects the conductivity of the electrode material. The activation energy (E a ) is set to 0.05~0.20; the phase change temperature affects the stability and durability of the material. In order to ensure the stability of the material, the phase change temperature (T0) needs to be higher than the maximum operating temperature of the single cell of 750℃ and the reduction temperature of 800℃. The range of the phase change temperature (T0) is 600℃~1000℃, and the weight is set to 0.05~0.20; good mechanical strength can ensure the reliability of the electrode material during the assembly and operation of the single cell. The range of mechanical strength (R) is 50~300 MPa, and the weight is set to 0.10~0.30.

[0092] The five key parameters of conductivity, thermal expansion coefficient, activation energy, phase transition temperature and mechanical strength of the test samples with different LSC / GDC ratios were analyzed and evaluated by multi-criteria decision analysis method (MCDAM) to screen out the transition layer and composite cathode layer that are most suitable for gradient structure cells. In addition, the weights of the above five key factors can be set according to the cell structure, operating conditions, performance requirements and cost-effectiveness.

[0093] The specific calculation process of this embodiment is:

[0094] First, the above five evaluation parameters are scored according to different evaluation parameter ranges, as shown in Table 2.

[0095] Table 2

[0096]

[0097] Secondly, the weights of the evaluation parameters are set according to the single cell structure, operating conditions, and performance requirements. Among the above evaluation parameters, the weight of the conductivity (σ) of the electrode material is set to 0.35; the weight of the difference in thermal expansion coefficient (Δα) is set to 0.25, and the weight of the activation energy (E a ) is set to 0.15, the weight of the phase transition temperature (T0) is set to 0.05; the weight of the mechanical strength (R) is set to 0.20, and the corresponding scores are determined according to the thermal expansion coefficient, electrical conductivity, activation energy, phase transition temperature and mechanical strength data of the LSC / GDC layers with different ratios at 750°C obtained in step S2, as shown in Table 3.

[0098] Table 3

[0099]

[0100] Calculate the weighted score based on Table 3 above :

[0101] LSC / GDC=9 / 1: S1=(0.35×0.8)+(0.25×0.4)+(0.15×0.6)+(0.05×0.7)+(0.20×0.6)=0.625

[0102] LSC / GDC=8 / 2: S2=(0.35×0.5)+(0.25×0.5)+(0.15×0.6)+(0.05×0.6)+(0.20×0.6)=0.540

[0103] LSC / GDC=7 / 3: S3=(0.35×0.4)+(0.25×0.7)+(0.15×0.6)+(0.05×0.5)+(0.20×0.6)=0.550

[0104] LSC / GDC=6 / 4: S4=(0.35×0.3)+(0.25×0.8)+(0.15×0.5)+(0.05×0.5)+(0.20×0.7)=0.545

[0105] LSC / GDC=5 / 5: S5=(0.35×0.1)+(0.25×0.8)+(0.15×0.5)+(0.05×0.5)+(0.20×0.7)=0.475.

[0106] According to the calculation results, LSC / GDC=9 / 1 has the highest weighted score and the best overall performance; LSC / GDC=7 / 3 has a weighted score second only to LSC / GDC=9 / 1, which means it ranks second in overall performance. Therefore, when preparing transition layers and composite cathode layers with different LSC / GDC ratios, LSC / GDC=9 / 1 and LSC / GDC=7 / 3 are preferred. In addition, during the service process of SOFC, the gas introduced into the cathode is oxygen, which requires that the cathode material must have efficient oxygen reduction reaction (ORR) catalytic activity, thereby accelerating the electrode reaction and reducing the polarization resistance of SOFC. LSC (La 1-x Sr x CoO 3-δ ) has a high catalytic activity for oxygen reduction reaction due to its perovskite structure and abundant active sites brought by cobalt, especially for oxygen. In contrast, GDC (Ce 0.9 G 0.1 O 2-δ ) has a high oxygen ion conductivity and is usually used to prepare a barrier layer between the electrolyte and the cathode. Although the oxygen catalytic activity of GDC is not as good as that of LSC, by combining with LSC materials, the catalytic activity of GDC in oxygen reduction reactions can be effectively improved. Therefore, when screening transition layer and composite cathode layer materials with different LSC / GDC ratios, materials with a higher LSC ratio are selected as composite cathode materials for SOFC, while materials with a lower LSC ratio are suitable as transition layer materials, and the conductivity of the cathode layer at 750°C is required to be 1000 S·cm -1 Only when the above is achieved can the initial power generation performance of the single cell reach 0.8V@300 mA / cm 2 Current density. Through the above calculation and analysis, it was finally determined that the LSC / GDC ratio of the transition layer was 7:3, and the LSC / GDC ratio of the composite cathode layer was 9:1.

[0107] S4. Determine the size and preparation process of the single cell, and prepare a gradient structured anode-supported flat-plate single cell according to the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer determined in step S3.

[0108] The structure and materials of the single cell are shown in Table 4 below.

[0109] Table 4

[0110]

[0111] The thickness of each layer structure of the above-mentioned single cell can be adjusted according to actual needs. In other embodiments, the thickness of the anode support layer can be selected in the range of 300~500μm, preferably 400~450μm; the thickness of the anode functional layer can be selected in the range of 5~20μm, preferably 8~10μm; the thickness of the electrolyte layer can be selected in the range of 5~20μm, preferably 6~8μm; the thickness of the barrier layer can be selected in the range of 5~20μm, preferably 6~8; the thickness of the transition layer can be selected in the range of 2~10μm, preferably 6~8μm; the thickness of the composite cathode layer can be selected in the range of 10~50μm, preferably 20~40μm.

[0112] Reference Figure 1 , the above single cell preparation process is:

[0113] S41. Prepare a half-cell consisting of an anode support layer, an anode functional layer, and an electrolyte layer. Specifically, firstly, an anode support layer is prepared by a tape casting method, and after it is formed, it is cut and dried to obtain an anode support layer blank; then, two layers of anode functional layer slurry are screen-printed on the anode support layer blank, and each screen printing is followed by drying at 40-60°C for 15 minutes, and then one layer of electrolyte layer slurry is screen-printed on the anode functional layer, and each screen printing is followed by drying for 15 minutes to obtain a half-cell blank, and the half-cell blank is subjected to debinding and sintering and leveling to obtain a half-cell; the above-mentioned half-cell blank is debinded in a debinding furnace, the debinding temperature is 1100°C, and the debinding time is 4 hours; it is sintered in a sintering furnace, the sintering temperature is 1400°C, and the sintering time is 8 hours; and during the sintering process, the temperature is increased from room temperature to 1400°C at a heating rate of 1°C / min, and sintered at 1400°C for 8 hours; and then the temperature is cooled from 1400°C to room temperature at a cooling rate of 1°C / min to complete the sintering;

[0114] S42, screen printing a layer of barrier layer slurry on the electrolyte layer of the half-cell, drying for 15 min after screen printing, and then sintering at 1200° C. for 5 h;

[0115] S43, screen printing a layer of transition layer slurry on the sintered barrier layer, drying for 15 minutes after screen printing, and then sintering at 1200° C. for 5 hours;

[0116] S44. Screen print 2 layers of composite cathode layer slurry on the sintered transition layer, dry for 15 minutes after each screen printing, and sinter at 1050°C for 5 hours after all screen printing; then perform debinding and sintering and leveling. The debinding temperature is 1200°C and the debinding time is 5 hours; the sintering temperature is 1000°C and the sintering time is 4 hours; after the above debinding and sintering and leveling, a gradient structure anode-supported flat-plate solid oxide fuel cell single cell is obtained.

[0117] In the above-mentioned single cell preparation process, the debinding temperature, debinding time, sintering temperature and sintering time are set according to actual needs. In other embodiments, the debinding temperature can be selected from 1000 to 1500°C, the debinding time can be selected from 2 to 8 hours, the sintering temperature can be selected from 1000 to 1500°C, and the sintering time can be selected from 2 to 10 hours.

[0118] S5. Perform hot and cold cycle and continuous operation tests on the SOFC single cell prepared in step S4, monitor the temperature, voltage and current curves during the hot and cold cycle and continuous operation as a function of the operation time, monitor the polarization curves and electrochemical impedance spectrum during the hot and cold cycle and continuous operation, and evaluate the performance at a current density of 300 mA / cm 2 When the voltage attenuation rate is ≤50%, whether the number of hot and cold cycle services of the single cell is ≥50 times and the continuous operation time is ≥2500h. If it does not meet the set requirements, adjust the LSC / GDC ratio of the transition layer and the composite cathode layer in step S3, and re-prepare a new gradient structure SOFC single cell until it meets the set requirements.

[0119] The above method is used to prepare a gradient structure single cell consisting of an anode support layer, an anode functional layer, an electrolyte layer, a barrier layer, a transition layer, and a composite cathode layer, with an area of ​​100 mm*100 mm. The structure of the single cell prepared in the above embodiment is as follows: Figure 2 shown.

[0120] A solid oxide fuel cell with a gradient structure can be prepared by stacking several layers of the above-prepared single cells, sealing layers, and connectors.

[0121] Comparative Example 1

[0122] like Figure 3 As shown, the difference between this comparative example and the embodiment is that the single cell structure of this comparative example is: an anode support layer (NiO-3YSZ), an anode functional layer (NiO-8YSZ), an electrolyte layer (YSZ), a barrier layer (GDC), and a cathode layer (LSC) stacked in sequence.

[0123] Comparative Example 2

[0124] like Figure 4 As shown, the difference between this comparative example and the embodiment is that the single cell structure of this comparative example is: an anode support layer (NiO-3YSZ), an anode functional layer (NiO-8YSZ), an electrolyte layer (YSZ), a barrier layer (GDC), and a composite cathode layer (LSC / GDC=9:1) stacked in sequence.

[0125] Comparative Example 3

[0126] like Figure 5As shown, the difference between this comparative example and the embodiment is that the single cell structure of this comparative example is: an anode support layer (NiO-3YSZ), an anode functional layer (NiO-8YSZ), an electrolyte layer (YSZ), a barrier layer (GDC), a transition layer (LSC / GDC=7:3), and a cathode layer (LSC) stacked in sequence.

[0127] At least 4 groups of single cell samples prepared in the above-mentioned embodiment and comparative examples 1-3 are prepared and used for the following detection and analysis, namely, thermal cycle test, continuous operation test, and mechanical strength test.

[0128] The four SOFC cells prepared in the above embodiments and comparative examples 1-3 were subjected to a hot and cold cycle test using a SOFC electrochemical testing device, and the curves of temperature, voltage and current changing with the operating time were collected. The polarization curves and electrochemical impedance spectra (EIS) of the four cells during each hot and cold cycle test were collected using an electrochemical workstation, and the IVP curves of the above four cells under hot and cold cycle conditions were obtained as shown in FIG. Figure 6 As shown. Figure 6 It can be seen that the single cell prepared in comparative example 1 showed obvious performance degradation after 5 hot and cold cycles. Due to the setting of the protection voltage, the current can only be pulled to 24A after the 5th cycle, and the output voltage is 0.602V; the single cells prepared in comparative example 2, comparative example 3 and the embodiment have output voltages of 0.789V, 0.766V and 0.844V at a current of 24A after 10 cycles, and output voltages of 0.603V, 0.598V and 0.664V at a current of 44A, respectively. This shows that the single cell prepared in the embodiment still has good power generation performance, good heat cycle resistance and durability during the hot and cold cycle service. In addition, referring to Figure 6 The single cell prepared in the embodiment was also subjected to 1, 30, and 50 cold and hot cycle tests. After 50 cycles, the voltage decay rate of the single cell prepared in the embodiment was 14.014% at a current of 30A, that is, at 300 mA / cm 2 At a current density of , after 50 cycles, the voltage decay rate is 14.014%, indicating that the single cell prepared in the embodiment meets the set requirements.

[0129] In addition, in order to reveal the mechanism of SOFC electrode degradation caused by thermal cycling, the SOFC cell was dismantled after the thermal cycling test, and the microstructure of the material of the SOFC cell after the thermal cycling test was tested using a scanning electron microscope (SEM), and the attenuation mechanism of the mechanical and electrochemical properties of the SOFC cell was analyzed. Small punch, three-point bending, four-point bending or nanoindentation tests were carried out using corresponding mechanical testing equipment to obtain the mechanical properties of the cell material.

[0130] Specifically, the microstructure (SEM) of the single cells of the above-mentioned embodiment and comparative examples 1-3 after cold and hot cycle service (the number of cycles is 10 times, 5 times, 10 times, and 10 times, respectively) is as follows: Figure 8 As shown. Among them, (a), (b), (c) are the single cell microstructures of comparative examples 1-3 respectively, (d) is the single cell microstructure of the embodiment, and the numbers ① in the figure are cathode layer, ② are transition layer, ③ are barrier layer, ④ are electrolyte layer, ⑤ are anode functional layer, ⑥ are anode support layer, and ⑦ are composite cathode layer. Figure 8 It can be seen that the cathode layer and composite cathode layer of the above four single cells all contain a large number of micropores, and Ni-YSZ particles and micropores are densely distributed in AFL and ASL, with uniform porosity; the microstructure of ASL contains not only dense Ni-YSZ particles and micropores, but also a large proportion of macropores to promote the diffusion of hydrogen; but the cathode side area of ​​comparative example 1 changed significantly after 5 thermal cycles, the LSC cathode layer fell off, there were many cracks at the junction of the cathode layer and the barrier layer, and the cathode layer and the barrier layer were severely damaged, which accelerated the diffusion of elements between the LSC cathode layer and the GDC barrier layer, and after thermal cycle service, the NiO-YSZ of AFL and ASL was reduced to Ni-YSZ, and the porosity of the anode functional layer and the anode support layer was significantly increased; microstructural damage was also observed in the cathode layer of comparative example 3; the composite cathode layer of comparative example 2 and the embodiment did not change significantly. This indicates that the single cell prepared in the example has only a slight decrease in the power generation voltage. While maintaining efficient power generation performance, the mechanical strength and resistance to cold and hot cycles of the single cell are enhanced, effectively solving the problem of reduced mechanical strength and easy rupture of SOFC single cells during cold and hot cycles.

[0131] The mechanical properties of a single cell include mechanical strength, elastic modulus and hardness. The mechanical strength is tested by a small punch test (SPT) using a small punch testing machine, while the elastic modulus and hardness are tested using a high-precision nanoindentation instrument.

[0132] Test of the mechanical strength of single cells: Before the SPT test, laser cutting was used to process the single cells into disc-shaped specimens with a diameter of 10 mm, and then they were ground and polished. In order to improve the reliability of the mechanical strength test results, 25 specimens of each type of single cell were tested, and the dispersion of their mechanical strength was analyzed using the Weibull statistical method. The overall average mechanical strength of the four single cells of Comparative Examples 1-3 and the embodiment when not in service was 161.15 MPa, 156.88 MPa, 159.63 MPa and 159.03 MPa, respectively. The average mechanical strength of the single cells after different numbers of hot and cold cycles is shown in Table 5. It can be seen from Table 5 that the average mechanical strength of the single cell of Comparative Example 1 after 5 thermal cycles is 62.533 MPa, and the attenuation rate reaches 61.196%; the average mechanical strength of the single cells of Comparative Examples 2, 3 and the embodiment after 10 thermal cycles is 84.193 MPa, 91.514 MPa and 93.804 MPa, and the attenuation rates are 46.332%, 42.672% and 41.015%, respectively.

[0133] Table 5

[0134]

[0135] In addition to the hot and cold cycle test, the present invention also uses the single cells prepared in Comparative Examples 1-3 and Examples to carry out continuous operation tests. The test conditions are an operating temperature of 750°C and a current density of 300 mA / cm 2 , fuel utilization rate 43.35%, the voltage-time curves of the four single batteries under continuous operation conditions are as follows Fig. 9 As shown. At the initial moment, the operating voltages of the four single cells are basically the same, and the voltages are 0.847V, 0.851V, 0.850V and 0.852V respectively. Since a protection voltage of 0.6V is set in the SOFC electrochemical testing equipment, the continuous operation time for the output voltage to decay from the initial voltage to the protection voltage of 0.6V is taken as the operating life of the four single cells. The operating lives of the four single cells prepared by Comparative Examples 1-3 and the embodiment are 279h, 855h, 1556h and 2539.5h respectively. The growth rates of the operating life of the embodiment compared with those of Comparative Example 1, Comparative Example 2 and Comparative Example 3 are 810.22%, 197.02% and 63.21% respectively; and the operating life of this embodiment exceeds 2500h, which meets the set requirements.

[0136] Through the above analysis, the single battery prepared in the embodiment of the present invention has better comprehensive performance and longer life.

[0137] It should be noted that some parts not described in the present invention can be implemented by adopting or drawing on existing technologies.

[0138] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for preparing a solid oxide fuel cell with a gradient structure, wherein the fuel cell is composed of a plurality of layers of single cells, a sealing layer and a connector stacked together, wherein each layer of the single cell comprises an anode support layer, an anode functional layer, an electrolyte layer, a barrier layer, a transition layer and a composite cathode layer stacked in sequence; the anode support layer and the anode functional layer are NiO-3YSZ layers and NiO-8YSZ layers respectively; the electrolyte layer is a YSZ layer; the barrier layer is a GDC layer; the transition layer is an LSC x GDC 1-x layer, 0.5≤x<1; the composite cathode layer is LSC y GDC 1-y layer, 0.5≤y<1, and x<y; characterized in that, Includes steps: S1. Determine the constituent materials of each layer structure of the single cell, and prepare the corresponding anode support layer, anode functional layer, electrolyte layer, barrier layer, transition layer with different LSC / GDC ratios, and composite cathode layer powder materials and slurry with different LSC / GDC ratios; S2. Prepare test samples with different LSC / GDC ratios and barrier layer test samples, and test the physical properties of the test samples with different LSC / GDC ratios, including thermal expansion coefficient, electrical conductivity, activation energy, phase transition temperature and mechanical strength, and the thermal expansion coefficient of the barrier layer test samples; S3, according to the thermal expansion coefficient, electrical conductivity, activation energy, phase transition temperature and mechanical strength parameters of the test samples with different LSC / GDC ratios obtained in step S2, the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer are determined by a multi-criteria decision analysis method; S4, determining the size and preparation process of the single cell, and preparing an anode-supported flat-plate single cell with a gradient structure according to the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer determined in step S3; S5. Perform hot and cold cycle and continuous operation tests on the SOFC single cell prepared in step S4, monitor the temperature, voltage and current curves during the hot and cold cycle and continuous operation as a function of the operation time, monitor the polarization curves and electrochemical impedance spectrum during the hot and cold cycle and continuous operation, and evaluate the performance at a current density of 300 mA / cm 2 When the voltage attenuation rate is ≤50%, whether the number of hot and cold cycle service of the single cell is ≥50 times and whether the continuous operation time is ≥2500h. If it does not meet the set requirements, adjust the LSC / GDC ratio of the transition layer and the composite cathode layer in step S3, and re-prepare a new gradient structure SOFC single cell until it meets the set requirements; The step S3 is specifically: by analyzing the thermal expansion coefficient, conductivity, activation energy, phase transition temperature and mechanical strength of the test samples with different LSC / GDC ratios in step S2, the weighted summation model method in the multi-criteria decision analysis method is used to perform weighted scoring on the comprehensive performance of the test samples with different LSC / GDC ratios, so as to determine the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer in the gradient structure single cell. The specific implementation steps are as follows: (1) Determine the evaluation parameters: electrical conductivity, thermal expansion coefficient difference, activation energy, phase transition temperature, and mechanical strength. The thermal expansion coefficient difference refers to the percentage difference between the test sample and the barrier layer at different LSC / GDC ratios. (2) Weight assignment: assign weights to each evaluation parameter , and the sum of all weights is 1, that is: ; in, is the weight of the evaluation parameter, is the serial number of the evaluation parameter, is the total number of evaluation parameters; (3) Evaluation parameter scoring: For each alternative material or alternative solution Each evaluation parameter in Score, recorded as ; (4) Calculate weighted scores: For each alternative material or alternative solution Calculating weighted scores ,Right now: ; in, For the The weighted scores of the alternative materials or alternative solutions, For each alternative material or alternative Each evaluation parameter in Ratings; (5) Scheme ranking and selection: based on the calculated weighted score All alternatives are ranked, and the one with the highest weighted score is selected as the optimal solution, thereby determining the LSC / GDC ratio of the transition layer and the LSC / GDC ratio of the composite cathode layer.

2. The method for preparing a solid oxide fuel cell having a gradient structure according to claim 1, characterized in that: The thickness of the anode support layer is 300-500 μm; The thickness of the anode functional layer is 5-20 μm; The thickness of the electrolyte layer is 5 to 20 μm; The thickness of the barrier layer is 5-20 μm; The thickness of the transition layer is 2-10 μm; The thickness of the composite cathode layer is 10-50 μm.

3. The method for preparing a solid oxide fuel cell having a gradient structure according to claim 1, characterized in that: The step S4 is specifically as follows: S41, preparing a half-cell consisting of an anode support layer, an anode functional layer, and an electrolyte layer; S42, screen printing 1 to 3 layers of barrier layer slurry on the electrolyte layer of the half-cell, drying for 5 to 20 minutes after each screen printing, and sintering at 1000 to 1500° C. for 2 to 8 hours after all screen printing; S43, screen printing 1 to 3 layers of transition layer slurry on the sintered barrier layer, drying for 5 to 20 minutes after each screen printing, and sintering at 1000 to 1500° C. for 2 to 8 hours after all screen printing; S44, screen printing 1 to 3 layers of composite cathode layer slurry on the sintered transition layer, drying for 5 to 20 minutes after each screen printing, sintering at 1000 to 1500°C for 2 to 8 hours after all screen printing; then, after debinding, sintering and leveling, a gradient structure anode-supported flat-plate single cell is obtained.

4. The method for preparing a solid oxide fuel cell having a gradient structure according to claim 3, characterized in that: The step S41 is specifically as follows: firstly, an anode supporting layer is prepared by a tape casting method or an immersion precipitation phase inversion method, and after being formed, the anode supporting layer is cut and dried for 5 to 20 minutes to obtain an anode supporting layer blank; then, 1 to 3 layers of anode functional layer slurry are screen-printed on the anode supporting layer blank, and each screen printing is followed by drying for 5 to 20 minutes, and then 1 to 3 layers of electrolyte layer slurry are screen-printed on the anode functional layer, and each screen printing is followed by drying for 5 to 20 minutes to obtain a half-cell blank, and the half-cell blank is subjected to binder removal and sintering and leveling to obtain a half-cell.

5. The method for preparing a solid oxide fuel cell having a gradient structure according to claim 4, characterized in that: In the step S41, the debinding temperature of the half-cell blank is 1000-1500° C., the debinding time is 2-8 hours, the sintering temperature is 1000-1500° C., and the sintering time is 5-10 hours.

6. The method for preparing a solid oxide fuel cell having a gradient structure according to claim 3, characterized in that: In the step S44, the debinding temperature is 1000-1500° C., the debinding time is 2-8 hours, and the sintering temperature after debinding is 1000-1500° C., and the sintering time is 5-10 hours.

Citation Information

Patent Citations

  • Preparation method of cathode barrier layer of metallic-propping solid oxide fuel cell

    CN104269563A

  • Gradient functional anode electrode for carbon-based solid oxide fuel battery and preparation method of gradient functional anode electrode

    CN104638277A

  • Novel low-stress thin film solid oxide fuel cell and preparation method thereof

    CN110400934A

  • LSCF-GDC cathode functional layer for solid oxide fuel cell and preparation method

    CN113299940A

  • High-strength and heat-resistant circulating fuel cell

    CN114188579A

Cited By

  • A SOFC bifunctional gradient composite support layer and a preparation method and application thereof

    CN123143437A