Wire core processing equipment and wire core processing method
By using an extrusion die and a heating device in the flat wire processing to form an uneven bite surface, the problem of the flat wire being easily cracked during the bending process is solved, and the insulation performance of the wire core is improved through oxidation treatment and the current loss is reduced. .
Patent Information
- Application Number
- CN202410939700.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing flat wires are prone to cracks during the bending and forming process, resulting in low wire core yield, and the skin effect increases current loss when alternating current passes through.
Using wire core processing equipment, the single module conductors are spliced in parallel and formed into a rectangular cross-section through an extrusion die. The extrusion die and heating device are used to form an uneven bite surface on the splicing surface, reducing cracks, and improving the conductor's strength through heating and oxidation treatments. Hardness and interface resistance.
The reliability and insulation performance of the wire core are improved, the risk of cracking is reduced, and the current loss is reduced.
Smart Images

Figure CN118473166B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of wire processing, and in particular to a wire core processing device and a wire core processing method. Background Art
[0002] The wire involved in the present application is a wire with a substantially rectangular cross-section, which is usually used in the stator of a motor and is also called a flat wire in the industry.
[0003] Flat wires are used in motor stators to greatly increase the slot fill rate of the stator, thereby improving the efficiency of the motor. However, since the flat wires are thicker, the alternating current of the motor will produce a skin effect when passing through the flat wires during operation, resulting in increased current loss. The higher the AC frequency inside the motor, the higher the AC copper loss of the flat copper wire windings.
[0004] The applicant has proposed a flat wire motor stator in the previously applied Chinese patent CN115276288B, in which the core of a single flat wire used is made of multiple conductor modules spliced together, and the outside of the core is covered with a paint layer to act as an insulator. The splicing of multiple conductor modules can disperse and effectively reduce the skin effect of a single flat wire. This kind of core has good performance in theory, but in actual processing, the flat wire needs to be bent into shape, such as into a U shape. During the bending process, cracks are easily generated between the multiple conductor modules of the core, and the cracks will further damage the insulation layer on the outside of the core, resulting in a low yield rate of the core. Summary of the invention
[0005] The purpose of the present invention is to overcome or at least alleviate the deficiencies of the above-mentioned prior art and to provide a wire core processing device and a wire core processing method.
[0006] According to a first aspect of the present invention, a wire core processing device is provided, which is used to splice at least two single-module conductors together to form a multi-module conductor, and extrude and stretch the multi-module conductor into a wire core with a rectangular cross-section, wherein the splicing of the two single-module conductors is performed by being arranged in parallel and contacting each other to form a splicing surface, wherein:
[0007] The processing equipment includes an extrusion die, and the extrusion die includes:
[0008] a first extrusion die having a first extrusion space for the multi-module conductor to pass through, wherein at least one convex portion is formed in the first extrusion space, and when the multi-module conductor passes through the first extrusion space, the convex portion can align with and extrude the splicing surface, so that the splicing surface is squeezed and shrunk into an uneven occlusal surface; and
[0009] The second extrusion die is arranged downstream of the first extrusion die and has a second extrusion space for passing the multi-module conductor. The cross-sectional profile of the outlet of the second extrusion space is adapted to the cross-sectional profile of the wire core.
[0010] In at least one embodiment, the extrusion die further comprises a front extrusion die disposed upstream of the first extrusion die, the front extrusion die having a front adjustment extrusion space for allowing the multi-module conductor to pass through.
[0011] The front adjustment extrusion space can extrude the multi-module conductor in a direction perpendicular to the splicing surface, so that the splicing surface is extended.
[0012] In at least one embodiment, the extrusion die also includes at least one adjustment extrusion die arranged between the first extrusion die and the second extrusion die, and the adjustment extrusion die has an adjustment extrusion space for allowing the multi-module conductor to pass through, and the adjustment extrusion space can make the passing multi-module conductor tend to the contour of the wire core.
[0013] In at least one embodiment, the extrusion die can be heated, and the heating temperature is 700-950°C.
[0014] In at least one embodiment, the wire core processing equipment further comprises a heating device for heating the multi-module conductor, and the heating temperature of the heating device is 550-650°C.
[0015] In at least one embodiment, the heating device is an induction heating device.
[0016] According to a second aspect of the present invention, a method for processing a wire core is provided, the processing method comprising:
[0017] Step S01, splicing at least two single-module conductors together to form a multi-module conductor, wherein adjacent single-module conductors are in contact with each other to form a splicing surface,
[0018] Step S02, extruding the multi-module conductor at least at the splicing surface, so that the splicing surface is squeezed and contracted into an uneven occlusal surface,
[0019] Step S03: extruding the multi-module conductor once or multiple times, so that the multi-module conductor is extruded and elongated into a wire core with a rectangular cross-section.
[0020] In at least one embodiment, before the step S02, extruding the multi-module conductor at least at the splicing surface so that the splicing surface is squeezed and shrunk into an uneven occlusal surface, step S11 is performed:
[0021] The multi-module conductor is extruded in a direction perpendicular to the splicing surface so that the splicing surface is extended.
[0022] In at least one embodiment, the multi-module conductor is heated before and / or during extrusion.
[0023] In at least one embodiment, step S01 further includes:
[0024] Polydimethylsiloxane or dimethylsiloxane or glass powder is coated on the mutually adjacent surfaces of at least two adjacent single module conductors; or
[0025] When the multi-module conductor is first extruded, oxygen is supplied to the surface of the multi-module conductor.
[0026] The wire core processed by the wire core processing equipment and processing method of the present invention is not easy to crack, has high reliability and good insulation performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the wire core processing equipment according to the first embodiment of the present application during the wire core processing process.
[0028] Figure 2 is a schematic diagram of a wire core processing device according to a first embodiment of the present application.
[0029] Figure 3 and Figure 4 It is a schematic diagram of multiple extrusion dies of the wire core processing equipment according to the first embodiment of the present application at two different viewing angles.
[0030] Figure 5 yes Figure 4 Schematic diagram of a partial cutaway of .
[0031] Figure 6 It is a schematic diagram of the cross section of a multi-module conductor at different stages of extruding the multi-module conductor using the wire core processing equipment according to the first embodiment of the present application.
[0032] Figure 7 It is a schematic diagram of the cross section of a multi-module conductor at different stages of extruding the multi-module conductor using the wire core processing equipment according to the second embodiment of the present application.
[0033] Figure 8 1 is a schematic diagram of two different situations of extruding a multi-module conductor using the wire core processing equipment according to the third embodiment of the present application.
[0034] Fig. 9 4 is a schematic diagram of extruding a multi-module conductor using a wire core processing device according to a fourth embodiment of the present application.
[0035] Description of reference numerals:
[0036] W wire core; W1 single module conductor; W2 multi-module conductor;
[0037] M1 first extrusion die; M11 convex part; M2 second extrusion die; M01 adjustment extrusion die;
[0038] R1 first extrusion space; R2 second extrusion space; R01 adjustment extrusion space;
[0039] H heating device; F joint surface; F1 occlusal surface. DETAILED DESCRIPTION
[0040] The exemplary embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood that these specific descriptions are only used to teach those skilled in the art how to implement the present invention, and are not intended to exhaust all possible modes of the present invention, nor to limit the scope of the present invention.
[0041] First embodiment
[0042] Reference Figures 1 to 6 , introduces the wire core processing equipment and the wire core processing method according to the first embodiment of the present application.
[0043] The wire core processing device according to the present application is used to process the wire core W of the flat wire mentioned in the background technology. When an insulating layer is provided on the outer surface of the wire core W, a flat wire commonly used in a motor stator is formed. The wire core W is formed by splicing at least two single-module conductors W1 in parallel, and the splicing surface F of the two single-module conductors W1 is parallel to the length direction of the wire core W. The single-module conductor W1 is, for example, a copper wire. Figure 1 The state of the wire core processing equipment in this embodiment during processing of the wire core W is shown.
[0044] The wire core processing equipment of this embodiment includes three extrusion dies and three heating devices H. A heating device H is provided upstream of each extrusion die.
[0045] Two single-module conductors W1 are spliced into a multi-module conductor W2, which passes through the first extrusion die M1, the adjustment extrusion die M01 and the second extrusion die M2 in sequence to finally form a wire core W. The two single-module conductors W1 in the wire core W are tightly combined together at the occlusal surface and are not easy to crack each other.
[0046] Reference Figure 2Each extrusion die has an extrusion space, and the multi-module conductor W2 is pulled or pushed through the multiple extrusion spaces. Each time it passes through an extrusion space, the cross-sectional area of the multi-module conductor W2 is extruded to be smaller, and since the volume does not change, the length of the multi-module conductor W2 becomes longer.
[0047] During the extrusion process, the multi-module conductor W2 is kept at a relatively high temperature. On the one hand, a heating device H is provided upstream of each extrusion die, and the heating device H can heat the multi-module conductor W2 by induction heating or radiation heating, for example, at a heating temperature of 550-650°C. On the other hand, each extrusion die itself can also be heated and transfer heat to the multi-module conductor W2 by heat conduction, for example, at a heating temperature of 700-950°C. The high temperature makes it easier for the multi-module conductor W2 to deform with the shape of the extrusion space and be gradually molded into the designed shape.
[0048] It should be understood that in other possible implementations, the heating device H may also directly contact the multi-module conductor W2 to achieve heating. For example, the heating device H may be formed as a pressing roller.
[0049] The heating device H also plays the role of heat treating the extruded and deformed multi-module conductor W2 during the wire core forming process, such as causing recrystallization annealing in the multi-module conductor W2, thereby reducing the hardness of the extruded and deformed multi-module conductor W2, increasing its elongation, eliminating internal residual stress, stabilizing its dimensions, reducing deformation and cracking tendencies, and reducing resistivity. By adjusting different heating temperatures of different heating devices H, appropriate heat treatment temperatures can be provided for the multi-module conductor W2 at different stages of processing and according to different deformation amounts of the multi-module conductor W2.
[0050] Reference Figures 3 to 6 , it is introduced how the three extrusion dies according to this embodiment gradually extrude the multi-module conductor W2 into the final shape.
[0051] Figure 3 It is a schematic diagram of three extrusion dies observed along the moving direction of the multi-module conductor W2, and what is seen in the definition figure is the back, top and side of the extrusion die. Figure 4 It is a schematic diagram of three extrusion dies observed against the moving direction of the multi-module conductor W2, and what is seen in the definition figure is the front, top and side of the extrusion die. Figure 5 It is along Figure 4 The hollow arrow in the figure indicates the movement direction of the multi-module conductor W2.
[0052] It can be found from the figure that the contours of the extrusion space on the front and back sides of each extrusion die are different. This is because the cross-section of the extrusion space is changing along the movement direction of the multi-module conductor W2, thereby gradually extruding the multi-module conductor W2 passing through it.
[0053] The first extrusion die M1 has a first extrusion space R1, in which two convex parts M11 are formed. The convex parts M11 are aligned with the splicing surface F, and the convex parts M11 can extrude the splicing surface F in a direction parallel to the splicing surface F and perpendicular to the moving direction of the multi-module conductor W2.
[0054] Also refer to Figure 6 , state a and state b in the figure are respectively the states of the multi-module conductor W2 before and after being extruded by the first extrusion die M1. Before entering the first extrusion space R1, the splicing surface F in the multi-module conductor W2 is relatively flat, and the two single-module conductors W1 in this state are easier to split apart. After passing through the first extrusion space R1, the splicing surface F in the multi-module conductor W2 is squeezed by the convex portion M11 to form a wrinkled or uneven bite surface F1. The uneven and relatively interlocking structure of the bite surface F1 makes the two single-module conductors W1 more tightly combined together and less likely to crack each other.
[0055] The adjustment extrusion die M01 downstream of the first extrusion die M1 plays a role in adjusting the cross-sectional shape of the multi-module conductor W2 to the cross-sectional shape of the finished product. The shape of the adjustment extrusion space R01 is between the shape of the first extrusion space R1 and the shape of the second extrusion space R2 to be described below. Figure 6 State c in FIG. 1 is the cross-sectional shape of the multi-module conductor W2 after adjusting the extrusion space R01. By comparing state b and state c, it can be found that after adjusting the extrusion space R01, the cross-sectional shape of the multi-module conductor W2 is further compressed, and the concave and convex outer contour formed by the extrusion of the convex portion M11 is adjusted.
[0056] Adjusting the second extrusion die M2 downstream of the extrusion die M01 plays a role in finally shaping the multi-module conductor W2 into a finished wire core W. The second extrusion die M2 has a second extrusion space R2, and the cross-sectional profile of the second extrusion space R2 at the outlet is adapted to the cross-sectional profile of the finished wire core W. Figure 6 State d in FIG. 1 is the cross-sectional shape of the multi-module conductor W2 after passing through the second extrusion space R2.
[0057] It is understandable that, according to the needs of the process, multiple adjustment extrusion dies can be set between the first extrusion die M1 and the second extrusion die M2. Along the movement direction of the multi-module conductor W2, the cross-section of the extrusion adjustment extrusion space in the multiple adjustment extrusion dies gradually approaches the cross-sectional shape at the entrance of the second extrusion die M2.
[0058] Optionally, in order to ensure that a high interface resistance is formed between adjacent single-module conductors W1 in each wire core W, before splicing, the surface of each single-module conductor W1 in this embodiment, especially the surface for splicing with adjacent single-module conductors W1, is coated with, for example, liquid polydimethylsiloxane or a precursor of dimethylsiloxane. The precursor will decompose and form a silicon dioxide layer on the splicing surface F during the process of the multi-module conductor W2 being heated by the wire core processing equipment, thereby increasing the interface resistance of the splicing surface F and reducing the eddy current in the wire core W.
[0059] Alternatively, instead of coating the precursor, oxygen may be applied into the extrusion space or onto the surface of the multi-module conductor W2 when the multi-module conductor W2 passes through the first extrusion die, so that the surface of the single-module conductor W1 made of copper wire, for example, is oxidized to form copper oxide. Alternatively, solid glass powder may be coated on the spliced surface of the single-module conductor W1, so that an oxide ceramic layer is formed on the spliced surface F of the multi-module conductor W2 formed by splicing.
[0060] It is worth noting that although multiple extrusion dies are spaced apart in the present embodiment, it is understandable that since the cross-sectional shape of the extrusion space in each extrusion die gradually changes along the movement direction of the multi-module conductor, the multiple extrusion dies can also be formed as an integral arrangement, which is equivalent to forming a longer large extrusion die having a longer large extrusion space.
[0061] Second embodiment
[0062] Reference Figure 7 The second embodiment of the present application is introduced. The second embodiment is a modification of the first embodiment, and components having the same or similar structures or functions as those in the first embodiment are marked with the same reference numerals, and detailed descriptions of these components are omitted.
[0063] The main difference between this embodiment and the first embodiment is that the multi-module conductor W2 passes through at least one pre-extrusion die before being extruded by the convex portion M11 of the first extrusion die M1. The pre-extrusion die has a pre-adjustment extrusion space, which can extrude the multi-module conductor W2 in a direction perpendicular to the splicing surface F, so that the splicing surface F is extended.
[0064] Figure 7State a and state b in the figure are the states of the multi-module conductor W2 before and after being extruded by the front extrusion die. Before entering the front adjustment extrusion space, the surface area of the splicing surface F is small; after passing through the front adjustment extrusion space, the splicing surface F is extended, so that the area of the splicing surface F is large, which is conducive to the subsequent large bite deformation when the splicing surface F is squeezed by the convex part M11 of the first extrusion die M1, forming an uneven bite surface F1.
[0065] Third embodiment
[0066] Reference Figure 8 The third embodiment of the present application is introduced. The solid line in the figure represents the cross-sectional profile of the conductor, and the dotted line represents the cross-sectional profile of the extrusion space in the extrusion die.
[0067] The third embodiment is a variation of the first embodiment. The main difference between this embodiment and the first embodiment is that the multi-module conductor W2 is formed by splicing more than two (four in this embodiment) single-module conductors W1, so the number of splicing surfaces F formed in each multi-module conductor W2 is more than one.
[0068] For the multi-module conductor W2 in this embodiment, as in case (a), there can be multiple protrusions M11 in the first extrusion die M1 in the wire core processing equipment, so that after the multi-module conductor W2 passes through the first extrusion die M1, each splicing surface F forms an uneven bite surface F1.
[0069] For the multi-module conductor W2 in this embodiment, as in case (b), the processing equipment may include multiple first extrusion dies M1. For example, the figure includes two first extrusion dies M1, and the shapes of the two first extrusion dies M1 may be different. The multi-module conductor W2 passes through the two first extrusion dies M1 in sequence, forming a bite surface F1 each time, and two bite surfaces F1 are formed by two extrusions.
[0070] Fourth embodiment
[0071] Reference Fig. 9 The fourth embodiment of the present application is introduced. The fourth embodiment is another variation of the first embodiment.
[0072] In this embodiment, the shapes of the two single-module conductors W1 constituting the multi-module conductor W2 are different, and adjacent single-module conductors W1 have a splicing structure that engages with each other at the beginning of splicing without passing through an extrusion die. This construction method of the single-module conductor W1 makes the structure of the final core W more stable and less prone to cracking.
[0073] It should be understood that the above-mentioned embodiments and some aspects or features thereof may be appropriately combined.
[0074] This application has at least one of the following advantages:
[0075] (i) According to the wire core processing equipment of the present application, in the early stage of pulling or pressing the wire core, the splicing surface inside the wire core is emphatically extruded, so that an uneven bite surface is formed at the splicing surface, so that the multiple single-module conductors inside the wire core can be tightly combined together, and the wire core is not easy to crack.
[0076] (ii) Before the splicing surface is extruded to form wrinkles, the multi-module conductor can be extruded in a direction perpendicular to the splicing surface so that the splicing surface is first extended to provide a larger deformation space for the subsequent formation of the bite surface.
[0077] (iii) Polydimethylsiloxane or a precursor such as dimethylsiloxane may be disposed on the adjacent surface of each single-module conductor, or oxygen may be introduced into the extrusion space when the multi-module conductor passes through the first extrusion die, so that the formed wire core has a larger interface resistance at the bite surface, thereby reducing the eddy current inside the wire core under working conditions.
[0078] Of course, the present invention is not limited to the above-mentioned embodiments, and those skilled in the art may make various modifications to the above-mentioned embodiments of the present invention under the guidance of the present invention without departing from the scope of the present invention.
Claims
1. A wire core processing device, used for splicing at least two single-module conductors (W1) together to form a multi-module conductor (W2), and extruding and stretching the multi-module conductor (W2) into a wire core (W) with a rectangular cross-section, wherein the splicing of the two single-module conductors (W1) is performed by being arranged in parallel and contacting each other to form a splicing surface (F), characterized in that: The processing equipment includes an extrusion die, and the extrusion die includes: a first extrusion die (M1) having a first extrusion space (R1) for allowing the multi-module conductor (W2) to pass through, at least one convex portion (M11) being formed in the first extrusion space (R1), and when the multi-module conductor (W2) passes through the first extrusion space (R1), the convex portion (M11) can align with and extrude the splicing surface (F), and the extrusion direction is parallel to the splicing surface (F), so that the splicing surface (F) is squeezed and shrunk into an uneven occlusal surface (F1); and The second extrusion die (M2) is arranged downstream of the first extrusion die (M1), and has a second extrusion space (R2) for passing the multi-module conductor (W2), and the cross-sectional profile of the outlet of the second extrusion space (R2) is adapted to the cross-sectional profile of the wire core (W). The extrusion die further comprises a front extrusion die arranged upstream of the first extrusion die (M1), the front extrusion die having a front adjustment extrusion space for allowing the multi-module conductor (W2) to pass through. The front adjustment extrusion space can extrude the multi-module conductor (W2) in a direction perpendicular to the splicing surface (F), so that the splicing surface (F) is extended, and the area of the splicing surface (F) becomes larger than before the multi-module conductor (W2) passes through the front adjustment extrusion space.
2. The wire core processing equipment according to claim 1, characterized in that: The extrusion die also includes at least one adjustment extrusion die (M01) arranged between the first extrusion die (M1) and the second extrusion die (M2), and the adjustment extrusion die (M01) has an adjustment extrusion space (R01) for allowing the multi-module conductor (W2) to pass through, and the adjustment extrusion space (R01) can make the passing multi-module conductor (W2) tend to the contour of the wire core (W).
3. The wire core processing equipment according to any one of claims 1 to 2, characterized in that: The extrusion die can be heated at a temperature of 700-950°C.
4. The wire core processing equipment according to any one of claims 1 to 2, characterized in that: The wire core processing equipment further comprises a heating device (H) for heating the multi-module conductor (W2), and the heating temperature of the heating device (H) is 550-650°C.
5. The wire core processing equipment according to claim 4, characterized in that: The heating device (H) is an induction heating device.
6. A method for processing a wire core, characterized in that: The processing method uses the wire core processing equipment according to any one of claims 1 to 5, and the processing method includes: Step S01, splicing at least two single-module conductors (W1) together to form a multi-module conductor (W2), wherein adjacent single-module conductors (W1) are in contact with each other to form a splicing surface (F), Step S11, extruding the multi-module conductor (W2) in a direction perpendicular to the splicing surface (F), so that the splicing surface (F) is extended and the area of the splicing surface (F) becomes larger, Step S02, extruding the multi-module conductor (W2) at least at the splicing surface (F), wherein the extrusion direction is parallel to the splicing surface (F), so that the splicing surface (F) is squeezed and contracted into an uneven occlusal surface (F1), Step S03, extruding the multi-module conductor (W2) once or multiple times, so that the multi-module conductor (W2) is extruded and elongated into a wire core (W) with a rectangular cross section, The step S11 is prior to the step S02.
7. The method for processing a wire core according to claim 6, characterized in that: The multi-module conductor (W2) is heated before and / or during extrusion.
8. The method for processing a wire core according to claim 7, characterized in that: The step S01 further includes: Polydimethylsiloxane or dimethylsiloxane or glass powder is coated on the mutually adjacent surfaces of at least two adjacent single module conductors (W1); or When the multi-module conductor (W2) is first pressed, oxygen is supplied to the surface of the multi-module conductor (W2).
Citation Information
Patent Citations
A flat wire motor stator and a flat wire motor
CN115276288B
Flat wire processing method and flat wire conductor
CN118173323A