A polyaniline membrane sponge composite material for seawater desalination and preparation method thereof

Through the polyaniline film sponge composite material and non-solvent phase separation technology, the problems of poor self-supporting and uneven thickness of polyaniline film are solved, efficient water evaporation and high mechanical strength are achieved, and performance and stability in seawater desalination are improved. .

CN118478574BActive Publication Date: 2024-11-26WUHAN UNIV OF TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410537590.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-26
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

The existing polyaniline film preparation methods have problems such as poor film self-supporting, uneven thickness and poor film quality, and poor solubility limits its application in seawater desalination.

Method used

Polyaniline film sponge composite material is used to uniformly fill the polyaniline into the pores of the sponge matrix, and combine non-solvent phase separation technology to prepare a polyaniline film with high porosity and high mechanical strength to achieve self-support and efficient water evaporation. .

Benefits of technology

It improves the mechanical strength and water evaporation performance of the polyaniline film, reduces salt barrier and maintenance requirements, enhances the stability and service life of the film, and solves the problems of low heat transfer efficiency and easy film fall off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118478574B_ABST
    Figure CN118478574B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of seawater desalination treatment, and in particular to a polyaniline membrane sponge composite material for seawater desalination and a preparation method thereof. The polyaniline membrane sponge composite material comprises a sponge matrix and a polyaniline membrane, and the polyaniline on the side of the polyaniline membrane close to the sponge matrix is ​​uniformly filled into the pores on the surface of the sponge matrix. The present invention prepares the polyaniline membrane with a porosity of more than 80% by compounding a solvent, a swelling agent and polyaniline by a coagulation bath method, and its microstructure distribution is more uniform, the porosity is high, and it is more conducive to the evaporation of water, so that the polyaniline membrane has a high water evaporation efficiency; at the same time, by adjusting the amount of swelling agent added, its microstructure distribution can be more uniform, the porosity is high, and it is more conducive to the evaporation of water, so that the polyaniline membrane has a high water evaporation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of seawater desalination treatment, in particular to a polyaniline membrane sponge composite material for seawater desalination and a preparation method thereof. Background Art

[0002] With the proposal and popularization of the concept of green development, solar energy, as a clean, safe and green energy, has brought new development opportunities for seawater desalination technology. Traditional seawater desalination methods include distillation, ion exchange, electrodialysis, reverse osmosis, nanofiltration and other important methods for purifying water from seawater and wastewater sources, which are accompanied by high energy consumption and the need for external forces. Using solar energy to evaporate water to solve the problem of seawater desalination is a low-energy, green and environmentally friendly method. Since natural water has low solar light absorption rate and poor energy conversion efficiency, it is necessary to place materials with high photothermal conversion performance, namely solar evaporation membrane, on the surface of the water body to achieve interface heating. Interface photothermal materials are usually derived from photothermal functional molecules or nanomaterials, such as plasma metals, semiconductors, carbon nanotubes, and conjugated polymers. Typical solar evaporation membranes include photothermal aerogels, hydrogels, porous polymer networks, foams, membranes, etc.

[0003] Polyaniline (PANI) is a promising material for solar water evaporation. The functionality of PANI itself can be used to achieve solar-driven water evaporation by photothermal conversion. Zhang et al. published a research paper entitled "Solar-driven membrane separation for direct lithium extraction from artificial salt-lake brine" in the journal Nature Communications with a DOI of "10.1038 / s41467-023-44625-w". The nano-matrix composed of PANI and PES was composited with polyamide to prepare a composite film that achieved photothermal conversion and lithium extraction from salt lakes. Li et al. published a research paper entitled "Multifunctional cotton with polyaniline-Ag NPs heterojunction for solar-driven water evaporation" in the journal Journal of Hazardous Materials with a DOI of "10.1016 / j.jhazmat.2021.127367". Polyaniline foam sponge was prepared using polyaniline and Ag composite functional cotton for solar evaporation. Li et al. published a research paper titled "Acid-doped polyaniline membranes for solar-driven interfacial evaporation" in the journal "Korean Journal of Chemical Engineering" and DOI "10.1007 / s11814-022-1283-0". They used a technical method to combine polyaniline solution with fabric fiber cloth and then with polystyrene foam layer and cotton to use pure polyaniline membrane for solar water evaporation. However, these research methods failed to obtain independent self-supporting polyaniline membranes.

[0004] Because the polyaniline chain exhibits strong rigidity, resulting in poor solubility, the difficulty in processing polyaniline limits its wider application. At present, the preparation of polyaniline film mainly includes scraping method, dipping method, suction filtration method, etc. Among them, the dipping method is to dipping film on glass while synthesizing polyaniline, but this method has problems such as unsatisfactory thickness control of polyaniline film and difficulty in large-scale film preparation; and the scraping method is difficult to achieve self-support of polyaniline film, needs to rely on the substrate, and the preparation process requires the assistance of scraper external force; the suction filtration method prepares polyaniline film by solution filtration precipitation, but it also has the problem of poor self-support. In addition, the dissolution of intrinsic polyaniline is also a technical problem. The only good solvent for intrinsic polyaniline is 1-methyl-2-pyrrolidone (NMP), and the dissolution rate is not high enough, generally less than 80%. This low dissolution rate seriously limits the preparation of polyaniline film, making the structural integrity of polyaniline film highly dependent on the substrate used during film formation. Although the emerging droplet superspreading technology can achieve substrate-free self-supporting polymer membranes, in order to prepare high-quality polyaniline membranes, the droplet superspreading technology is highly dependent on the solubility rate of the polymer in the polymer solution. The polymer needs to be highly soluble in the solvent and will be affected by the diffusion rate of the solvent, thereby affecting the film formation rate of the polymer membrane and the morphology and porosity of the internal pore structure of the membrane. Summary of the invention

[0005] In view of this, the present invention proposes a polyaniline membrane sponge composite material for seawater desalination and a preparation method thereof, so as to solve the problems of poor film self-support, uneven thickness and poor film quality existing in the existing polyaniline membrane preparation method.

[0006] The technical solution of the present invention is achieved in this way:

[0007] In a first aspect, the present invention provides a polyaniline membrane sponge composite material for seawater desalination, comprising a sponge matrix and a polyaniline membrane, wherein the polyaniline on a side of the polyaniline membrane close to the sponge matrix is ​​uniformly filled into pores on the surface of the sponge matrix.

[0008] In the present application, the polyaniline on the side of the polyaniline film close to the sponge matrix is ​​uniformly filled into the pores on the surface of the sponge matrix. This structural design enhances the interfacial bonding force between the polyaniline film and the sponge matrix, thereby improving the overall mechanical strength and stability of the composite material, while exhibiting efficient water evaporation and salt barrier properties during the seawater desalination process; the conductive properties of polyaniline may also help to improve thermal efficiency and further promote the water evaporation process. The polyaniline membrane prepared in the present application has a high porosity of 70% to 85%, and the average pore size of the pores contained in the polyaniline membrane is 1.5 to 2.0 μm, so that the film has a higher water permeability and better water evaporation performance; under the condition of sunlight, the polyaniline membrane can generate a temperature of 42.6°C to 60.1°C, so that the seawater absorbed by the sponge on the polyaniline membrane is evaporated to produce fresh water; in this process, since the temperature does not reach the boiling point of water, the high-salinity seawater remaining in the polyaniline membrane after the fresh water is produced can be quickly diluted by the fresh seawater absorbed by the sponge, preventing the crystallization of sea salt, thereby reducing the pollution and maintenance requirements of the membrane.

[0009] In a second aspect, the present invention provides a method for preparing a polyaniline membrane sponge composite material for seawater desalination, comprising the following steps:

[0010] S1, mixing NMP and a swelling agent, adding polyaniline, and dissolving to obtain a polyaniline casting solution;

[0011] S2, spreading the polyaniline casting solution on the surface of the coagulation bath solution to obtain a semi-solidified polyaniline film;

[0012] S3, placing the semi-cured polyaniline film on a sponge substrate, and curing it to obtain a polyaniline film sponge composite material.

[0013] Specifically, in step S1, NMP and swelling agent are mixed in a certain ratio and heated to 40-60°C. Heating can increase the thermal kinetic energy and molecular motion speed of the solvent, thereby accelerating the interaction process between the solvent molecules and polyaniline. Then add polyaniline, which is a high molecular polymer with a long molecular chain. Directly adding a large amount may cause entanglement between polymer molecules or form aggregates in the solvent. Therefore, polyaniline is added in batches in this application, at least 3-5 times. Adding in batches can significantly reduce uneven dissolution and aggregation, ensuring that each batch of polyaniline can be fully dissolved after addition. After the addition of polyaniline is completed, ultrasonic dissolution is performed for 22-26 hours to promote the dissolution of polyaniline. Ultrasonic treatment can generate tiny bubbles and strong local shear force through its high-frequency vibration, which helps to break the aggregation between polyaniline molecules and promote its dispersion in the solvent, so that polyaniline can be fully dissolved in the solvent to form a uniform solution.

[0014] In step S2, the polyaniline casting liquid is discharged to the liquid surface of the coagulation bath at room temperature to form a semi-cured polyaniline film. In step S3, after the semi-cured polyaniline film contacts with the sponge matrix, during the curing process, the uncured polyaniline film can be partially and evenly filled into the pores of the sponge matrix, thereby achieving a good combination between the polyaniline film and the sponge matrix, wherein the sponge matrix can be any one or more of polyurethane sponge, polyethylene sponge, silicone sponge, natural sponge and polypropylene foam. There are few porous polyaniline films prepared in the prior art that use a non-solvent phase separation method to prepare such a polyaniline film with self-supporting performance. The present invention can obtain a polyaniline film using the principle of non-solvent phase separation without a substrate during film formation.

[0015] On the basis of the above technical solution, preferably, in step S2, the side of the semi-cured polyaniline film close to the surface of the coagulation bath solution is solid, and the side away from the surface of the coagulation bath solution is liquid.

[0016] Specifically, when the polyaniline solution contacts the coagulation bath, the solvent (NMP) in the polyaniline casting solution begins to exchange with the liquid (water) in the coagulation bath, resulting in a decrease in the solvent concentration in the polyaniline solution, thereby affecting the dissolved state of the polyaniline molecules; as the solvent is gradually replaced by the liquid in the coagulation bath, the polyaniline molecules lose sufficient solvent support and begin to aggregate to form a solid structure, which first occurs at the interface where the solution contacts the coagulation bath, i.e., the side close to the surface of the coagulation bath solution. During the curing process, the polyaniline molecular chains may be partially reorganized to form a more compact or ordered structure, thereby improving the mechanical strength and stability of the film. The polyaniline film prepared by the prior art has poor bonding to the hydrophilic substrate, resulting in easy detachment of the film, low evaporation efficiency, and poor heat transfer effect.

[0017] On the basis of the above technical solution, preferably, placing the semi-solid polyaniline film on the sponge matrix in step S3 specifically includes: placing the sponge matrix on the liquid side of the semi-solid polyaniline film, allowing the semi-solid polyaniline film to partially penetrate into the sponge matrix, and drying at a constant temperature of 25 to 35° C. to obtain a polyaniline film sponge composite material.

[0018] Specifically, in the semi-cured state, one side of the polyaniline membrane has been partially cured while the other side remains in a liquid state, which allows the polyaniline membrane to better combine with the surface and internal structure of the sponge matrix. The polyaniline on the liquid side can penetrate into the pores of the sponge matrix and form a relatively uniform coverage and combination with the matrix material. Constant temperature drying at 25-35°C is to ensure that the penetration and curing process of the polyaniline membrane is carried out uniformly, avoiding the polyaniline from curing too quickly and losing its permeability due to too high a temperature, or incomplete curing due to too low a temperature. The appropriate temperature can help the polyaniline membrane form a stable structure in the sponge matrix while keeping the pore structure of the matrix intact. In this way, the polyaniline membrane and the sponge matrix are not only combined on the surface, but also penetrate and combine with each other at the microscopic level, so that the formed polyaniline membrane sponge composite material combines the chemical and physical properties of polyaniline and the structural advantages of the sponge matrix, showing excellent comprehensive performance.

[0019] On the basis of the above technical solution, preferably, in step S1, the volume ratio of NMP to the swelling agent is 87:13 to 97:3. NMP is an efficient solvent that can quickly dissolve polyaniline, but its rapid diffusion may lead to uneven film formation. By appropriately increasing the proportion of the swelling agent, the diffusion rate of NMP can be slowed down, the distance between polyaniline chains can be adjusted, and the microstructure and porosity of the film can be affected; at the same time, the film can form a special film-forming state in the coagulation bath, that is, the upper surface remains relatively liquid, while the lower surface solidifies rapidly.

[0020] On the basis of the above technical solution, preferably, the swelling agent is tetramethyl piperidine. By regulating the content of tetramethyl piperidine in the polyaniline casting solution, the diffusion rate of NMP in the polyaniline solution to the coagulation bath can be slowed down, so that the film presents a special state of uncured upper surface and fully cured lower surface on the coagulation bath surface during film formation. Tetramethyl piperidine can not only play the original effect of swelling intrinsic polyaniline, but also reduce the concentration difference of NMP in the polyaniline solution and the coagulation bath solution by diluting the NMP concentration in the polyaniline solution, thereby forming the technical effect of the above-mentioned special film-forming state.

[0021] On the basis of the above technical solution, preferably, the swelling agent is tetramethylpiperidine and dibutyl phthalate (DBP), and the volume ratio of the tetramethylpiperidine to dibutyl phthalate is 67:33 to 71:29.

[0022] For the intrinsic polyaniline polymer that is difficult to dissolve, the general strategy adopted is to add a swelling agent in an organic solvent, first fully swell the polymer, and then dissolve under the further action of the solvent. However, the swelling effect of the single-component swelling agent, tetramethyl piperidine, is not good enough, resulting in the poor quality of the polyaniline film after film formation, and the brittleness is very high. Therefore, the present invention uses tetramethyl piperidine and dibutyl phthalate (DBP) to improve the swelling behavior of intrinsic polyaniline as much as possible in a composite manner, thereby ensuring that NMP can fully dissolve the swollen body of the intrinsic polyaniline polymer. This helps to improve the mechanical flexibility of the polyaniline film and reduce the risk of film brittle cracking.

[0023] On the basis of the above technical solution, preferably, in step S1, the concentration of the polyaniline casting solution is 0.04-0.06 g / ml.

[0024] On the basis of the above technical solution, preferably, in step S2, the coagulation bath solution comprises NMP and pure water, and the volume ratio of NMP to pure water is 1:2.5-3.5.

[0025] Using NMP in the coagulation bath can help regulate the transition speed of the polymer from the solution state to the solid state, because NMP has a high compatibility with the polymer, which can slow down the coagulation process of the polymer and help form a more uniform microstructure. Pure water is added as a non-solvent mainly to promote the precipitation and solidification of the polymer chain. Water can quickly diffuse into the polymer solution, displace NMP, accelerate the coagulation process of the polymer, and help form a porous structure.

[0026] In a third aspect, the present invention provides an application of a polyaniline membrane sponge composite material for seawater desalination in the field of seawater desalination.

[0027] The polyaniline membrane sponge composite material for seawater desalination and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:

[0028] (1) The present invention prepares a polyaniline membrane with a porosity of more than 80% by compounding a solvent, a swelling agent and polyaniline by a coagulation bath method. The microstructure distribution is more uniform, the porosity is high, and the evaporation of water is more convenient, so that the polyaniline membrane has a high water evaporation efficiency. At the same time, by adjusting the amount of swelling agent added, the microstructure distribution is more uniform, the porosity is high, and the evaporation of water is more convenient, so that the polyaniline membrane has a high water evaporation efficiency, thereby solving the problems of multiple thickness control parameters, long control time, low porosity and poor hydrophilicity of the polyaniline membrane in the prior art.

[0029] (2) The present invention can slow down the diffusion rate of NMP in the polyaniline solution into the coagulation bath by adjusting the amount of swelling agent added, so that the film presents a special state on the surface of the coagulation bath when forming a film, in which the upper surface is uncured and the lower surface is fully cured; through the synergistic effect of tetramethylpiperidine and dibutyl phthalate, an efficient swelling effect can be achieved, so that the intrinsic polyaniline is fully dissolved, so that the final product polyaniline film is not easy to be brittle;

[0030] (3) The present invention achieves the technical effect of partially penetrating the uncured polyaniline film with the sponge surface by preparing a semi-cured polyaniline film floating on the surface of the coagulation bath, so that the polyaniline film can be firmly attached to the sponge surface, thereby improving the interfacial bonding force between the polyaniline film and the sponge substrate, and at the same time significantly improving the contact area between the polyaniline film and the sponge, thereby improving the heat generation and heat transfer efficiency of the polyaniline film, thereby improving the treatment efficiency of water evaporation; at the same time, it is beneficial to prevent the formation of salt crystals at the interface between the film and the sponge, enhance the stability and service life of the film, and solve the problem that the polyaniline film prepared by the prior art has poor bonding with the hydrophilic substrate, thereby causing the film to fall off easily, the evaporation efficiency to be low, and the heat transfer effect to be poor;

[0031] (4) In the prior art, porous polyaniline membranes are rarely prepared by using a non-solvent phase separation method. In order to prepare such a self-supporting polyaniline membrane, the present invention can obtain a polyaniline membrane by using the principle of non-solvent phase separation without using a substrate during membrane formation;

[0032] (5) The heat transfer capacity and water evaporation efficiency of the porous polyaniline membrane prepared by the prior art are not good enough. The present invention greatly improves the water evaporation efficiency of the porous polyaniline film. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 The present invention is a flow chart of the preparation of the polyaniline membrane sponge composite material;

[0035] Figure 2 A diagram of a device for testing the seawater evaporation efficiency of the polyaniline membrane sponge composite material of the present invention;

[0036] Figure 3 This is a physical picture of the semi-cured polyaniline film of Example 2 of the present invention;

[0037] Figure 4is a side view of the polyaniline membrane sponge composite material of Example 2 of the present invention;

[0038] Figure 5 It is a side view and a microscopic magnified view of the polyaniline membrane sponge composite material of Example 3 of the present invention;

[0039] Figure 6 This is a scanning electron microscope image of the polyaniline membrane sponge composite material of Example 2-4 of the present invention;

[0040] Figure 7 This is a test diagram of the surface water contact angle of the cured polyaniline film of Example 3 of the present invention;

[0041] Figure 8 This is a sedimentation experiment diagram of the cured polyaniline film of Example 3 of the present invention;

[0042] Fig. 9 This is an infrared thermal image of the temperature of the polyaniline membrane sponge composite material of Example 2-4 of the present invention;

[0043] Fig.10 This is a physical picture of the polyaniline film in step S2 of comparative example 1 of the present invention;

[0044] Fig.11 This is a physical picture of the polyaniline film of Comparative Example 2 of the present invention;

[0045] Fig.12 This is a temperature infrared thermal image of the polyaniline membrane sponge composite material of Comparative Example 2 of the present invention;

[0046] Fig.13 It is a temperature comparison diagram of the polyaniline membrane sponge composite material of Examples 2-4 of the present invention and Comparative Example 2;

[0047] Fig.14 This is a diagram of the evaporation efficiency of the polyaniline membrane sponge composite material of Examples 2-4 of the present invention and Comparative Example 2. DETAILED DESCRIPTION

[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The preparation process is as follows: Figure 1 As shown, the specific steps include:

[0051] S1, weigh 87ml 1-methyl-2-pyrrolidone (NMP) and 13ml tetramethylpiperidine and add them to a volumetric flask, and place the volumetric flask in a constant temperature water bath at 50°C, weigh 1g PANI (PANI) powder and add it to the volumetric flask, add magnetic stirring, and then add 1g of PANI powder every 5 hours until 5g PANI powder is added to 100ml solution, stir for another 5 hours, put it into an ultrasonic cleaner, and ultrasonically dissolve it for 24 hours to obtain 0.05g / ml PANI casting solution;

[0052] S2, using a coagulation bath prepared by mixing NMP and pure water in a volume ratio of 25:75, using a rubber-tipped dropper to draw the above-prepared 0.05 g / ml PANI casting solution and placing it on the liquid surface of the coagulation bath at room temperature, the PANI solution spreads on the coagulation bath liquid surface and presents a semi-cured PANI film with an upper liquid layer and a lower solidified state;

[0053] S3. Pick up the semi-cured PANI liquid film prepared in step S2 with a sponge and let it stand for 30 minutes to allow the semi-cured PANI film to partially penetrate into the sponge and combine with the sponge; then dry it at a constant temperature of 30° C. for 6 hours to allow the semi-cured PANI liquid film to completely cure to form a PANI thin film attached to the sponge.

[0054] Example 2

[0055] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method is the same as that in Example 1, except that: in step S1, the swelling agent is 8.7 ml of tetramethylpiperidine and 4.3 ml of dibutyl phthalate.

[0056] Example 3

[0057] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method comprises the following steps:

[0058] S1, weigh 92ml NMP, 5.5ml 4-MP and 2.5ml dibutyl phthalate and add them into a volumetric flask, and place the volumetric flask in a constant temperature water bath at 50°C, weigh 1g PANI powder and add it into the volumetric flask, add magnetic stirring, and then add 1g PANI powder every 5 hours until 5g PANI powder is added to 100ml solution, stir for another 5 hours, put it into an ultrasonic cleaner, and ultrasonically dissolve it for 24 hours to obtain 0.05g / ml PANI casting solution;

[0059] S2, using a coagulation bath prepared by mixing NMP and pure water in a volume ratio of 28:72, using a rubber-tipped dropper to draw the above-prepared 0.05 g / ml PANI casting solution and placing it on the liquid surface of the coagulation bath at room temperature, the PANI solution spreads on the coagulation bath liquid surface and presents a semi-cured PANI film with an upper liquid layer and a lower solidified state;

[0060] S3. Pick up the semi-cured PANI liquid film with a sponge and let it stand for 30 minutes to allow the semi-cured PANI film to partially penetrate into the sponge and combine with the sponge; then dry it at a constant temperature of 30°C for 6 hours to allow the semi-cured PANI to completely cure to form a PANI film attached to the sponge.

[0061] Example 4

[0062] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method comprises the following steps:

[0063] S1, weigh 97ml NMP, 2.1ml 4-MP and 0.9ml dibutyl phthalate and add them into a volumetric flask, and place the volumetric flask in a constant temperature water bath at 50°C, weigh 1g PANI powder and add it into the volumetric flask and stir it with a magnetic bar, then add 1g of PANI powder every 5 hours until 5g PANI powder is added to 100ml solution, stir for another 5 hours, put it into an ultrasonic cleaner, and ultrasonically dissolve it for 24 hours to obtain 0.05g / ml PANI casting solution;

[0064] A coagulation bath was prepared by mixing S2, NMP and pure water in a volume ratio of 22:78. A rubber-tipped dropper was used to pipette the above-prepared 0.05 g / ml PANI casting solution and placed it on the liquid surface of the coagulation bath at room temperature. The PANI solution spread on the surface of the coagulation bath liquid and formed a semi-solidified PANI film with a liquid upper layer and a solidified lower layer.

[0065] S3. Pick up the semi-cured PANI liquid film with a sponge and let it stand for 30 minutes to allow the semi-cured PANI film to partially penetrate into the sponge and combine with the sponge; then dry it at a constant temperature of 30°C for 6 hours to allow the semi-cured PANI to completely cure to form a PANI film attached to the sponge.

[0066] Example 5

[0067] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method is the same as that of Example 2, except that: in step S1, 84 ml of NMP, 10.7 ml of 4-MP and 5.3 ml of dibutyl phthalate are measured and added into a volumetric flask.

[0068] Example 6

[0069] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method is the same as that of Example 2, except that: in step S1, 87 ml of NMP, 8.06 ml of 4-MP and 4.94 ml of dibutyl phthalate are measured and added into a volumetric flask.

[0070] Example 7

[0071] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method is the same as that of Example 2, except that: in step S1, 87 ml of NMP, 10.4 ml of 4-MP and 2.6 ml of dibutyl phthalate are measured and added into a volumetric flask.

[0072] Example 8

[0073] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method is the same as that of Example 2, except that: in step S1, 4 g of PANI is added, and the concentration of the PANI casting solution is 0.04 g / ml.

[0074] Example 9

[0075] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method is the same as that of Example 2, except that: in step S1, 6 g of PANI is added, and the concentration of the PANI casting solution is 0.06 g / ml.

[0076] Comparative Example 1

[0077] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method comprises the following steps:

[0078] S1, weigh 82ml NMP, 12.8ml 4-MP and 5.2ml dibutyl phthalate and add them into a volumetric flask, and place the volumetric flask in a constant temperature water bath at 50°C, weigh 1g PANI powder and add it into the volumetric flask, add magnetic stirring, and then add 1g PANI powder every 5 hours until 5g PANI powder is added to 100ml solution, stir for another 5 hours, put it into an ultrasonic cleaner, and ultrasonically dissolve it for 24 hours to obtain 0.05g / ml PANI casting solution;

[0079] S2. Prepare a coagulation bath by mixing NMP and pure water in a mass ratio of 25:75. Use a rubber-tipped dropper to draw the 0.05 g / ml PANI casting solution prepared above and place it on the liquid surface of the coagulation bath at room temperature to observe the film-forming state of the PANI solution on the liquid surface of the coagulation bath.

[0080] S3. The PANI solution prepared above cannot form a film on the surface of the coagulation bath and cannot proceed to the next step.

[0081] Comparative Example 2

[0082] This embodiment provides a PANI membrane sponge composite material for seawater desalination and a preparation method thereof. The specific preparation method comprises the following steps:

[0083] S1, weigh 100 ml of NMP solution and add it to a volumetric flask, and place the volumetric flask in a constant temperature water bath at 50°C, weigh 1 g of PANI powder and add it to the volumetric flask, add magnetic stirring, and then add 1 g of PANI powder every 5 hours until 5 g of PANI powder is added to 100 ml of NMP, stir for another 5 hours, put it into an ultrasonic cleaner, and ultrasonically dissolve it for 24 hours to obtain 0.05 g / ml PANI casting solution;

[0084] S2, NMP and pure water are mixed in a volume ratio of 25:75 to prepare a coagulation bath, and the 0.05 g / ml PANI casting solution prepared above is pipetted with a rubber-tipped dropper and placed on the liquid surface of the coagulation bath at room temperature. The PANI solution spreads on the surface of the coagulation bath liquid and quickly solidifies into a film;

[0085] S3. The PANI film prepared as above was scooped up with a sponge. After standing for 30 minutes, the PANI film did not bond with the sponge. It was then kept at a constant temperature of 30°C for 6 hours to completely solidify the PANI film. It can be seen that there are many gaps between the PANI film and the sponge after drying, and the direct bonding state with the sponge is poor.

[0086] Application Examples

[0087] The PANI membrane sponge composite materials prepared in Examples 1-9 and Comparative Examples 1-2 were floated in artificial seawater with a NaCl concentration of 35 g / L and continuously irradiated with a standard sunlight (device such as Figure 2 The temperature was measured with an infrared thermal imager. The weight of the remaining artificial seawater was recorded every 15 minutes, and the evaporation efficiency of the film was calculated. The results are shown in Table 1.

[0088] Table 1

[0089]

[0090]

[0091] As can be seen from the table, compared with Example 1 and Example 2, a semi-cured PANI film can be obtained by using tetramethyl piperidine as a swelling agent, and the preparation of a PANI film sponge composite material is also realized. However, compared with pure tetramethyl piperidine, the PANI powder can be completely dissolved by using tetramethyl piperidine composite dibutyl phthalate. Pure tetramethyl piperidine causes insufficient dissolution of PANI powder, poor mechanical properties of PANI film, and low evaporation efficiency. Comparison of Examples 2-4 shows that the PANI film sponge composite material prepared by the technical solution of the present invention has good evaporation efficiency. Comparison of Example 2 and Example 5 shows that when the swelling agent is added excessively, the film is too thick, the porosity decreases, and the concentration of the PANI solution is low, resulting in a decrease in the photothermal conversion efficiency, and the evaporation efficiency decreases. Comparison of Example 2 and Examples 6 and 7 shows that when the ratio of tetramethyl piperidine and dibutyl phthalate in the swelling agent is too much or too little, the film-forming state of the PANI film is affected, and there is too much tetramethyl piperidine, and the PANI film is too brittle and has poor contact with the sponge. Too much dibutyl phthalate reduces the photothermal conversion efficiency of the PANI film. Both cases lead to reduced evaporation efficiency of the polyaniline film. Comparing Example 2 with Examples 8 and 9, it can be seen that the concentration of the PANI casting solution affects the film structure. When the PANI solution concentration is 0.04 g / ml, the PANI film is too thin, the photothermal conversion efficiency is low, and salt is easily precipitated to block the pores; when the PANI solution concentration is 0.06 g / ml, the PANI film is too thick and has a low porosity, resulting in a long water transport distance in the film. Both cases lead to reduced evaporation efficiency.

[0092] Figure 3 A photograph showing a semi-cured PANI film prepared in Example 2 of the present invention floating on the surface of a coagulation bath is shown. It can be seen from the figure that the PANI solution forms a film during the spreading process on the surface of the coagulation bath; Figure 4 A side view of the PANI membrane sponge composite material prepared in Example 2 of the present invention is shown. It can be seen from the figure that the bottom surface of the PANI membrane partially penetrates into the sponge.

[0093] Figure 5 The side view of the PANI membrane sponge composite material prepared in Example 3 of the present invention is shown, wherein Figure 5 (a) is a side optical image of the PANI film-sponge composite material. It can be seen from the figure that when bent downward, the PANI film is still completely and firmly attached to the sponge surface; Figure 5 (b) is to use an optical microscope to Figure 5 (a) is a 500-fold magnification of the interface area circled by the dotted line. It can be seen from the figure that dark-colored PANI polymer is attached to the surface of the yellow sponge network skeleton.

[0094] Figure 6The scanning electron microscope images of the PANI membrane sponge composite materials prepared in Examples 2-4 are shown, wherein Figure 6 (a), (b) and (c) are cross-sectional SEM images of the PANI films prepared in Example 2, Example 3 and Example 4 after they are completely cured. It can be seen from the figures that their thicknesses are 26.1 μm, 13.1 μm and 5.2 μm, respectively; Figure 6 (d), (e), and (f) are plane scanning electron microscope images of the fully cured PANI films prepared in Example 2, Example 3, and Example 4, respectively. It can be seen from the figures that their surfaces all present a loose and porous microscopic state. It can be seen from the above cross-sections and plane scanning electron microscope images that the PANI films prepared in Example 2, Example 3, and Example 4 can still maintain a loose and porous microscopic state after being fully cured.

[0095] Figure 7 The surface water contact angle test of the fully cured PANI film prepared in Example 3 is shown. As can be seen from the figure, the water drop can quickly and completely spread out within 0.6 seconds, indicating that the PANI film has extremely strong hydrophilicity.

[0096] Figure 8 The figure shows the sedimentation experiment of the fully cured PANI film prepared in Example 3 in water. It can be seen from the figure that the PANI film can almost completely sink in 13 seconds. Based on the above experimental results, it can be seen that the PANI film has extremely strong hydrophilicity.

[0097] Fig. 9 The infrared thermal images of the temperature of the PANI membrane sponge composite material prepared in Examples 2 to 4 after being irradiated for 20 seconds under simulated sunlight are shown, wherein: Fig. 9 (a) is the temperature infrared thermal image of the PANI sponge composite material of Example 2, Fig. 9 (b) is the temperature infrared thermal image of the PANI sponge composite material of Example 3; Fig. 9 (c) is the infrared thermal image of the temperature of the PANI sponge composite material of Example 4. It can be seen from the figure that the highest temperatures generated by the PANI sponge composite materials prepared in Examples 2-4 under the condition of sunlight irradiation are 60.1°C, 55.2°C, and 43.3°C, respectively. This shows that the PANI films prepared in Examples 2, 3, and 4 can efficiently use sunlight to generate heat.

[0098] Fig.10 An optical photograph of the PANI film prepared in Comparative Example 1 floating on the surface of the coagulation bath is shown. It can be seen from the figure that the film-forming quality of the PANI film is extremely low and it is almost impossible to form a film.

[0099] Fig.11 The optical photograph of the PANI film prepared in Comparative Example 2 floating on the surface of the coagulation bath is shown. Fig.11 (a) It can be seen that the PANI film can be formed relatively completely on the surface of the coagulation bath; Fig.11 (b) is a sponge with a PANI film on the surface after being treated in steps 2 and 3. As can be seen from the figure, there are many gaps between the sponge and the film after drying, and the direct bonding state with the sponge is poor.

[0100] Fig.12 This is the infrared thermal image of the temperature of the PANI membrane sponge composite material prepared in Comparative Example 2 after being irradiated under simulated sunlight for 20 seconds. It can be seen from the figure that the highest temperature generated by the membrane is 36.9°C.

[0101] Fig.13 This is a comparison chart of the maximum temperatures generated under simulated sunlight conditions when the PANI films prepared in Examples 2-4 and Comparative Example 2 are attached to the surface of a sponge. Fig.14 The relationship between the water evaporation per unit area of ​​the PANI film attached to the sponge surface prepared in Examples 2-4 and Comparative Example 2 and the evaporation time; As can be seen from the figure, the evaporation efficiency of the three films prepared in Examples 2-4 is 4.98 kg / m 2 h, 5.21kg / m 2 h, 4.13kg / m 2 h, indicating that as the thickness of the film increases, the heat transfer temperature is higher, but the increase in film thickness will also affect the water vapor transmission rate. The PANI film of Example 3 is not much different from the PANI film of Example 2 in terms of light-to-heat conversion, but the PANI film of Example 3 has a better water evaporation rate; the PANI film prepared in Comparative Example 2 has poor heat transfer to the sponge surface, with a maximum temperature of only 36.9°C, far lower than 55.2°C, and a low water evaporation efficiency of only 2.71 kg / m 2 ·h, the water evaporation efficiency of Comparative Example 2 is significantly lower than that of Examples 2-4.

[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A polyaniline membrane sponge composite material for seawater desalination, characterized in that: It comprises a sponge matrix and a polyaniline membrane, wherein the polyaniline on the side of the polyaniline membrane close to the sponge matrix is ​​uniformly filled into the pores on the surface of the sponge matrix; The preparation method of the polyaniline film sponge composite material comprises the following steps: S1, mixing NMP and a swelling agent, adding polyaniline, and dissolving to obtain a polyaniline casting solution; S2, spreading the polyaniline casting solution on the surface of the coagulation bath solution to obtain a semi-solidified polyaniline film; S3, placing the semi-cured polyaniline film on a sponge substrate, and curing to obtain a polyaniline film sponge composite material; In step S1, the volume ratio of NMP to the swelling agent is 87:13 to 97:3; In step S2, the side of the semi-cured polyaniline film close to the surface of the coagulation bath solution is solid, and the side away from the surface of the coagulation bath solution is liquid; In step S2, the coagulation bath solution includes NMP and pure water; Placing the semi-cured polyaniline film on the sponge matrix in step S3 specifically includes: placing the sponge matrix on the liquid side of the semi-cured polyaniline film, allowing the semi-cured polyaniline film to partially penetrate into the sponge matrix, and drying at a constant temperature of 25 to 35° C. to obtain a polyaniline film sponge composite material.

2. The polyaniline membrane sponge composite material for seawater desalination according to claim 1, characterized in that: The swelling agent is tetramethylpiperidine.

3. The polyaniline membrane sponge composite material for seawater desalination according to claim 1, characterized in that: The swelling agent is tetramethyl piperidine and dibutyl phthalate, and the volume ratio of the tetramethyl piperidine to dibutyl phthalate is 67:33-71:

29.

4. The polyaniline membrane sponge composite material for seawater desalination according to claim 1, characterized in that: In step S1, the concentration of the polyaniline casting solution is 0.04-0.06 g / ml.

5. The polyaniline membrane sponge composite material for seawater desalination according to claim 1, characterized in that: The volume ratio of the NMP to pure water is 1:2.5-3.

5.

6. Use of the polyaniline membrane sponge composite material for seawater desalination as claimed in claim 1 in the field of seawater desalination.

Citation Information

Patent Citations

  • Preparing method of easy-to-recover and recyclable polyaniline loading polyurethane sponge adsorption material

    CN105148875A

  • Solar photothermal conversion material and preparation method thereof

    CN109206553A

  • Photothermal evaporation system with self-desalting surface and preparation method thereof

    CN109422317A

  • Preparation method of seawater desalination material based on polyurethane foam

    CN110511558A

  • Super-hydrophobic photo-thermal adsorption material capable of treating viscous crude oil and preparation method of super-hydrophobic photo-thermal adsorption material