Preparation method of polyimide nanoporous film regulated by amphiphilic polymer

Through the preparation method of polyamide nanoporous film regulated by amphiphilic polymer, the hydrogen bonding effect and high-temperature heat treatment of block copolymers were used to solve the problems of poor pore size control and insufficient strength of polyimide porous films, and PI nanometers were realized High-performance preparation of porous films, suitable for lithium-ion battery separators.

CN118480208BActive Publication Date: 2024-11-05FUYOUTE (SHANDONG) NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410931049.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The pore size control and strength of the existing polyimide porous films is poor, the preparation method is complex and costly, and it is difficult to meet the high performance needs of lithium-ion battery separators.

Method used

The preparation method of polyamide nanoporous film regulated by amphiphilic polymer is adopted to form PI nanoporous films by preparing polyamic acid solution, induction liquid and spin coating. The hydrogen bonding effect of block copolymers and high-temperature heat treatment are used to achieve pore size Controllability and performance optimization.

Benefits of technology

The prepared PI nanoporous film has excellent pore size controllability, low dielectric constant and high thermal decomposition temperature. It is suitable for large-scale industrial production and is simple to operate. The pore size is 23-34nm and the porosity is 33-39%, which is relatively medium. The electrical constant is 2.20-2.36, and the thermal decomposition temperature of 5 wt% is 533-542℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118480208B_ABST
    Figure CN118480208B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a polyimide nanoporous film regulated by an amphiphilic polymer, and belongs to the technical field of polyimide films. The preparation method comprises the following steps: preparing a polyamic acid solution, inducing, and forming a film; in the preparation of the polyamic acid solution, dissolving a diamine in a solvent, adding a dianhydride in batches under nitrogen protection, and then continuing to stir at room temperature for 20-25 hours under nitrogen protection to obtain a polyamic acid solution; in the induction, dissolving an amphiphilic polymer in a solvent, then adding the amphiphilic polymer to the polyamic acid solution, and stirring at room temperature for 10-15 hours under nitrogen protection to obtain an induced liquid; the invention can overcome the shortcomings of poor pore size controllability and poor strength of the PI film in the prior art, and the prepared PI film has an adjustable pore size, a low dielectric constant, and excellent high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyimide films, and in particular to a method for preparing a polyimide nanoporous film regulated by an amphiphilic polymer. Background Art

[0002] Polyimide (PI) porous film has good high temperature resistance, flame retardancy, radiation resistance, low dielectric constant and smoke emission rate, and has attracted increasing attention in the field of lithium-ion battery separators in recent years.

[0003] At present, the main methods for preparing PI porous films include porogen method, coagulation bath method, breath plot method, supercritical carbon dioxide method and block copolymer template method.

[0004] However, the pore size of the PI porous film prepared by the porogen method is large and uneven, and the mechanical strength is poor. The coagulation bath method is to scrape the PI precursor polyamic acid (PAA) solution into a film, immerse it in a coagulation bath of a poor solvent of PAA to cause phase separation, and then perform high-temperature thermal imidization to obtain a PI porous film. The disadvantage of this method is that the interaction between PAA and its good solvent is strong, and the separation process of immersion in a poor solvent takes a long time, which easily causes PAA to hydrolyze, resulting in poor mechanical properties of the PI porous film. In the breath diagram method, water vapor condenses into small spherical droplets on the surface of the PAA solution. An ordered arrangement is formed through self-assembly by capillary force. After the solvent and water are completely evaporated, the ordered structure is replicated and fixed to form an ordered porous film, but most of the pores are micron-sized. The supercritical carbon dioxide method is to use supercritical carbon dioxide technology to dry PI or PAA gel, and a porous structure is obtained after supercritical carbon dioxide treatment, but the pores in the porous structure are disordered and have poor controllability. The block copolymer template method is to introduce PAA or PI into a block copolymer, and then remove the other block at high temperature to obtain a PI porous film. Although a nanoporous structure can be obtained, the preparation method is complicated and the cost is high. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of poor pore size controllability and poor strength of polyimide porous films in the prior art, and to provide a method for preparing a polyimide nanoporous film regulated by an amphiphilic polymer. The prepared PI film has adjustable pore size, low dielectric constant and excellent high temperature resistance.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] The method for preparing a polyimide nanoporous film regulated by an amphiphilic polymer comprises the following steps: preparing a polyamic acid solution, inducing, and forming a film;

[0008] The polyamic acid solution is prepared by dissolving diamine in a solvent, adding dianhydride in batches under nitrogen protection, and then continuing to stir at room temperature for 20-25 hours under nitrogen protection to obtain a polyamic acid solution;

[0009] In the preparation of the polyamic acid solution, the diamine is one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 2,2-bis[(4-aminophenoxy)phenyl]propane, bis[4-(4-phenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)-2-tert-butylbenzene, 1,4-bis(4-aminophenoxy)-2,5-di-tert-butylbenzene, m-phenylenediamine, 4,4'-bis(3-aminophenoxy)benzophenone, hexafluoromethylbenzene diamine, and 4,4'-diaminobenzanilide;

[0010] The dianhydride is one or more of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenyl)hexafluoropropane tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, and 2,2'-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane tetracarboxylic dianhydride;

[0011] The mass ratio of diamine, solvent and dianhydride is 0.54-1.46:40-70:1.09-2.22;

[0012] The induction comprises dissolving the amphiphilic polymer in a solvent, then adding the mixture into the polyamic acid solution, and stirring the mixture at room temperature for 10-15 hours under nitrogen protection to obtain an induction solution;

[0013] The solvent used in preparing the polyamic acid solution and inducing the polyamic acid solution is one of dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide, and γ-butyrolactone;

[0014] In the induction, the amphiphilic polymer is composed of a carboxyl-philic block and a carboxyl-phobic block;

[0015] The carboxyl-philic block in the amphiphilic polymer is polymerized by a tertiary amine-containing monomer, and the tertiary amine-containing monomer is one of dimethylaminoethyl methacrylate, 2-vinyl pyridine, 4-vinyl pyridine, and dimethylaminoethyl acrylate;

[0016] The monomer in the hydrophobic carboxyl block in the amphiphilic polymer is one of styrene, methyl methacrylate, L-lactic acid, caprolactone and glycolic acid;

[0017] The thermal decomposition temperature of the amphiphilic polymer is lower than that of polyimide;

[0018] The number average molecular weight of the amphiphilic polymer is 20,000-100,000, and the molecular weight distribution index (PDI) is 1.08-1.21;

[0019] The ratio of the number average molecular weight of the carboxyl-phobic block to the number average molecular weight of the carboxyl-philic block is 50-60%;

[0020] The mass ratio of the amphiphilic polymer to the solvent is 0.8-1.2:16-23;

[0021] The mass ratio of the diamine in the polyamic acid solution to the amphiphilic polymer in the induction is 0.54-1.46:0.8-1.2;

[0022] The film preparation comprises spin coating the induction liquid on a silicon wafer, and then drying and heat treating to obtain a PI nanoporous film;

[0023] In the film preparation, the coating thickness during spin coating is 90-105 nm;

[0024] The drying temperature is 65-75°C and the drying time is 20-25h;

[0025] The heat treatment is performed at 95-105°C for 50-70 min, at 190-210°C for 50-70 min, at 290-310°C for 50-70 min, and at 340-360°C for 100-140 min.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The preparation method of the polyimide nanoporous film regulated by the amphiphilic polymer of the present invention uses an amphiphilic block copolymer of a specific composition as a microscopic morphology control agent, fixes the microstructure formed by the self-assembly of the amphiphilic block copolymer by means of the hydrogen bonding force formed between the amphiphilic block copolymer and PAA, and then obtains a PI nanoporous film with excellent performance while pyrolyzing the amphiphilic block copolymer at high temperature;

[0028] (2) The method for preparing the polyimide nanoporous film regulated by the amphiphilic polymer of the present invention has good controllability of pore size, simple operation, uniform thickness, low dielectric constant, and is conducive to large-scale industrial production;

[0029] (3) The preparation method of the polyimide nanoporous film regulated by the amphiphilic polymer of the present invention is to form an ordered structure by self-assembly of the block copolymer itself, and then remove one block of the block copolymer to obtain the ordered porous structure of the remaining block; in addition, the block copolymer used in the present invention contains a component that can form a strong hydrogen bond with the carboxyl group in the polyamic acid, and the block copolymer and the polyamic acid are fully reacted in a common solvent for a long enough time to ensure that the two form an effective hydrogen bond force, and then as the solvent evaporates, the block copolymer self-assembles to form an ordered nanostructure. Due to the hydrogen bond force between the polyamic acid and the block copolymer, the polyamic acid is adsorbed by the block copolymer to induce the formation of the same ordered nanostructured complex, and finally the high-temperature heat treatment is imidized, which not only removes the block copolymer but also converts the polyamic acid into polyimide. Because the ordered structure of the block copolymer is removed, an ordered porous polyimide is finally formed. By adjusting the composition of the two blocks in the block copolymer, the total molecular weight, and the ratio of the block copolymer to the polyamic acid, the pore size of the final ordered porous polyimide film can be controlled;

[0030] (4) The method for preparing the polyimide nanoporous film regulated by the amphiphilic polymer of the present invention has an average pore size of 23-34 nm, a porosity of 33-39%, a relative dielectric constant (1 MHz) of 2.20-2.36, and a 5 wt% thermal decomposition temperature of 533-542 °C. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of the PI nanoporous film prepared in Example 1;

[0032] Figure 2 This is a scanning electron microscope image of the PI nanoporous film prepared in Example 2;

[0033] Figure 3 This is a scanning electron microscope image of the PI nanoporous film prepared in Example 3;

[0034] Figure 4 This is a scanning electron microscope image of the PI nanoporous film prepared in Example 4;

[0035] Figure 5 This is a scanning electron microscope image of the PI nanoporous film prepared in Comparative Example 1;

[0036] Figure 6 This is a scanning electron microscope image of the PI nanoporous film prepared in Comparative Example 2. DETAILED DESCRIPTION

[0037] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0038] Example 1

[0039] 1g 4,4'-diaminodiphenyl ether was dissolved in 40g dimethylacetamide, and 1.09g pyromellitic anhydride was added one by one in 4 batches under N2 protection, and then stirred at room temperature for 24h under N2 protection to obtain a viscous PAA solution; 1.1g polystyrene-block-poly(dimethylaminoethyl methacrylate) (PS-b-PDMAEMA, where the number average molecular weight is 27390, PDI is 1.21, the number average molecular weight of PS is 9390, and the number average molecular weight of PDMAEMA is =18000) was dissolved in 20.9g dimethylacetamide, and the aforementioned PAA solution was added. The mixture was stirred at room temperature for 12h under N2 protection. An appropriate amount of the obtained mixed solution was spin-coated on a silicon wafer at 2000rpm for 2min. The coating thickness during spin coating was controlled to be 93nm. The mixture was then placed in a forced air drying oven at 70℃ for 24h. The mixture was then treated in a muffle furnace at 100℃ for 1h→200℃ for 1h→300℃ for 1h→350℃ for 2h to obtain a PI nanoporous film. The scanning electron microscope image is shown in Figure 1 .

[0040] Example 2

[0041] 0.54g p-phenylenediamine was dissolved in 40g dimethylformamide, and 1.47g 3,3',4,4'-biphenyltetracarboxylic anhydride was added one by one in 4 batches under N2 protection, and then stirred at room temperature for 24h under N2 protection to obtain a viscous PAA solution; 1.02g polymethyl methacrylate-block-poly (2-vinylpyridine) (PMMA-b-P2VP, wherein the number average molecular weight = 54450, PDI = 1.08, the number average molecular weight of PMMA = 20150, the number average molecular weight of P2VP = 34300) was dissolved in 19g dimethylformamide, and the aforementioned PAA solution was added. The subsequent treatment was the same as in Example 1, and the coating thickness during spin coating was controlled to be 102nm. The scanning electron microscope image of the final PI nanoporous film is shown in Figure 2 .

[0042] Example 3

[0043] 0.99g 4,4'-diaminodiphenylmethane was dissolved in 48g N-methylpyrrolidone, and 1.55g 3,3',4,4'-diphenyl ether tetracarboxylic anhydride was added in 4 batches under N2 protection, and stirred at room temperature for 24h under N2 protection to obtain a viscous PAA solution; 1.2g poly (L-lactic acid-block-poly (4-vinylpyridine) (PLLA-b-P4VP, wherein the number average molecular weight = 98260, PDI = 1.14, the number average molecular weight of PLLA = 35370, the number average molecular weight of P4VP = 62890) was dissolved in 23g N-methylpyrrolidone, and the aforementioned PAA solution was added. The subsequent treatment was the same as in Example 1, and the coating thickness during spin coating was controlled to be 100nm. The scanning electron microscope image of the final PI nanoporous film is shown in Figure 3 .

[0044] Example 4

[0045] 1.46g 1,4-bis(4-aminophenoxy)benzene was dissolved in 70g dimethyl sulfoxide, and 2.22g 2,2'-bis(3,4-dicarboxyphenyl)hexafluoropropane tetracarboxylic dianhydride was added in 4 batches under N2 protection, and stirred at room temperature for 24h under N2 protection to obtain a viscous PAA solution; 0.8g polycaprolactone-block-poly(dimethylaminoethyl acrylate) (PCL-b-PDMAEA, wherein the number average molecular weight = 44330, PDI = 1.08, the number average molecular weight of PCL = 15500, the number average molecular weight of PDMAEA = 28830) was dissolved in 16g dimethyl sulfoxide, and the aforementioned PAA solution was added. The subsequent treatment was the same as in Example 1, and the coating thickness during spin coating was controlled to be 97nm. The scanning electron microscope image of the final PI nanoporous film is shown in Figure 4 .

[0046] Comparative Example 1

[0047] 1.51 g of polystyrene-block-poly L-lactic acid (PS-b-PLLA, wherein the number average molecular weight = 55600, PDI = 1.24, the number average molecular weight of PS = 32400, the number average molecular weight of PLLA = 23200) was dissolved in 43 g of dimethylacetamide, and the dimethylacetamide solution of PS-b-PDMAEMA was added to the PAA solution in Example 1. The subsequent treatment was the same as in Example 1, and the coating thickness during spin coating was controlled to be 99 nm. The scanning electron microscope image of the finally obtained PI nanoporous film is shown in FIG. Figure 5 .

[0048] Comparative Example 2

[0049] 0.98 g of polystyrene-block-polycaprolactone (PS-b-PCL, wherein the number average molecular weight = 74400, PDI = 1.17, the number average molecular weight of PS = 45000, the number average molecular weight of PCL = 29400) was dissolved in 18 g of dimethylformamide, and the PAA solution in Example 2 was added instead of the dimethylformamide solution of PMMA-b-P2VP. The subsequent treatment was the same as in Example 2, and the coating thickness of the spin coating was ~100 nm. The scanning electron microscope image of the final PI nanoporous film is shown in Figure 6 .

[0050] The average pore size, porosity, relative dielectric constant, and 5wt% thermal decomposition temperature of the PI nanoporous films prepared in Examples 1-4 and Comparative Examples 1-2 were tested, and the test results are as follows:

[0051]

[0052] pass Figure 1-6 It can be seen from the scanning electron microscope images that, relative to Examples 1-4, the pore sizes of Comparative Examples 1 and 2 are randomly distributed, indicating that the pore size distribution of the porous films obtained by the preparation methods of Comparative Examples 1 and 2 is uneven; and compared with Examples 1 and 2, the average pore size and porosity of Comparative Examples 1 and 2 are relatively small, and the relative dielectric constant is large, indicating that the preparation methods of Examples 1 and 2 can increase the average pore size and porosity, and reduce the relative dielectric constant.

[0053] Unless otherwise specified, all percentages used in the present invention are by mass.

[0054] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a polyimide nanoporous film regulated by an amphiphilic polymer, characterized in that: The method comprises the following steps: preparing polyamic acid solution, inducing, and forming a film; The polyamic acid solution is prepared by dissolving diamine in a solvent, adding dianhydride in batches under nitrogen protection, and then continuing to stir at room temperature for 20-25 hours under nitrogen protection to obtain a polyamic acid solution; In the preparation of the polyamic acid solution, the diamine is one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 2,2-bis[(4-aminophenoxy)phenyl]propane, bis[4-(4-phenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)-2-tert-butylbenzene, 1,4-bis(4-aminophenoxy)-2,5-di-tert-butylbenzene, m-phenylenediamine, 4,4'-bis(3-aminophenoxy)benzophenone, hexafluoromethylbenzene diamine, and 4,4'-diaminobenzanilide; The dianhydride is one or more of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenyl)hexafluoropropane tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, and 2,2'-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane tetracarboxylic dianhydride; The mass ratio of diamine, solvent and dianhydride is 0.54-1.46:40-70:1.09-2.22; The induction comprises dissolving the amphiphilic polymer in a solvent, then adding the mixture into the polyamic acid solution, and stirring the mixture at room temperature for 10-15 hours under nitrogen protection to obtain an induction solution; In the induction, the amphiphilic polymer is composed of a carboxyl-philic block and a carboxyl-phobic block; The carboxyl-philic block in the amphiphilic polymer is polymerized by a tertiary amine-containing monomer, and the tertiary amine-containing monomer is one of dimethylaminoethyl methacrylate, 2-vinyl pyridine, 4-vinyl pyridine, and dimethylaminoethyl acrylate; The monomer in the hydrophobic carboxyl block in the amphiphilic polymer is one of styrene, methyl methacrylate, L-lactic acid, caprolactone and glycolic acid; The thermal decomposition temperature of the amphiphilic polymer is lower than that of polyimide; The number average molecular weight of the amphiphilic polymer is 20000-100000, and the molecular weight distribution index is 1.08-1.21; The ratio of the number average molecular weight of the carboxyl-phobic block to the number average molecular weight of the carboxyl-philic block is 50-60%.

2. The method for preparing the polyimide nanoporous film regulated by an amphiphilic polymer according to claim 1, characterized in that: The solvent used in preparing the polyamic acid solution and inducing the polyamic acid solution is one of dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide and gamma-butyrolactone.

3. The method for preparing the polyimide nanoporous film regulated by an amphiphilic polymer according to claim 1, characterized in that: In the induction, the mass ratio of the amphiphilic polymer to the solvent is 0.8-1.2:16-23.

4. The method for preparing the amphiphilic polymer-regulated polyimide nanoporous film according to claim 1, characterized in that: The mass ratio of the diamine in the polyamic acid solution to the amphiphilic polymer in the induction is 0.54-1.46:0.8-1.

2.

5. The method for preparing the amphiphilic polymer-regulated polyimide nanoporous film according to claim 1, characterized in that: The film-making process includes spin coating the induction liquid on a silicon wafer, followed by drying and heat treatment to obtain a PI nanoporous film.

6. The method for preparing the amphiphilic polymer-regulated polyimide nanoporous film according to claim 5, characterized in that: In the film preparation, the coating thickness during spin coating is 90-105 nm; The drying temperature is 65-75°C and the drying time is 20-25h; The heat treatment is performed at 95-105°C for 50-70 min, at 190-210°C for 50-70 min, at 290-310°C for 50-70 min, and at 340-360°C for 100-140 min.