A low-stress additive, a low-stress chemical nickel plating solution and its application

By using the coordinated combination of sodium m-nitrobenzenesulfonate and complexing agent M in the electroless nickel plating potion, the stress of the nickel plating layer is reduced, and the problem of brittle cracking when nickel-plated palladium is bound to copper or aluminum wire is solved. , achieving improved uniformity and corrosion resistance.

CN118480772BActive Publication Date: 2024-12-03ZHUHAI SMART ELECTRONIC MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410656610.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-12-03
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

Electrochemical nickel-palladium is prone to brittle cracks when binding copper or aluminum wires, mainly due to the high brittleness of the nickel-plated layer.

Method used

Low-stress additives, including sodium m-nitrobenzenesulfonate and complexing agent M (the product of deHCl after reaction of diethylene triamine pentaacetic acid and allyl chloride), improve the stability of electroless nickel plating agent through synergistic cooperation. and dispersibility, reduce stress of nickel plating layer and reduce brittleness.

Benefits of technology

The problem of brittle cracking when electroless nickel-palladium is effectively solved when binding copper or aluminum wire is bonded, and a nickel-plated layer with good uniformity, high corrosion resistance and low brittleness is obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118480772B_ABST
    Figure CN118480772B_ABST
Patent Text Reader

Abstract

The invention discloses a low-stress additive, a low-stress chemical nickel plating solution and an application thereof, and relates to the field of chemical plating. The low-stress additive comprises sodium m-nitrobenzene sulfonate and a complexing agent M, and the complexing agent M is a reaction product of dehydrochlorination after the reaction of diethylenetriaminepentaacetic acid and allyl chloride. The low-stress chemical nickel plating solution comprises a composite complexing agent, a reducing agent, a water-soluble nickel salt, a water-soluble lead compound, polyethylene glycol, a low-stress additive and deionized water. In the chemical nickel palladium gold plating process, the chemical nickel deposition step adopts a low-stress chemical nickel plating solution for chemical nickel deposition, and the obtained chemical nickel plating layer has good uniformity and low brittleness, which can solve the problem of easy brittle cracking when the chemical nickel palladium gold is bound to the copper wire or the aluminum wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of chemical plating, and in particular to a low-stress additive, a low-stress chemical nickel plating solution and applications thereof. Background Art

[0002] Chemical nickel-palladium-gold plating technology has been widely used in the surface treatment process of IC substrates. However, due to the high price of gold, the cost of binding gold wires is high. In order to save costs, copper wires or aluminum wires are chosen instead of gold wires. However, the conditions for binding copper wires or wires are high, and the pressure of the splitter is high. Ordinary chemical nickel-palladium-gold plating is prone to brittle cracking. According to analysis, the root cause of binding brittle cracking lies in the brittleness of the chemical nickel plating layer. Summary of the invention

[0003] In order to improve the problem of chemical nickel-palladium-gold plating in the related art that chemical nickel layer is highly brittle and prone to brittle cracking when binding copper wire, the present application provides a low-stress additive, a low-stress chemical nickel plating solution and applications thereof.

[0004] In the first aspect, the present application provides a low stress additive using the following technical solution:

[0005] A low stress additive comprises sodium m-nitrobenzene sulfonate and a complexing agent M, wherein the complexing agent M is a reaction product of diethylenetriaminepentaacetic acid and allyl chloride after the HCl is removed.

[0006] In the present application, the complexing agent M is the reaction product of dehydrochlorination after the reaction of diethylenetriaminepentaacetic acid and allyl chloride. Through the synergistic combination of sodium m-nitrobenzenesulfonate and the complexing agent M, the stability and dispersion ability of the chemical nickel plating solution can be effectively improved, and the stress of the nickel plating layer can be reduced, and the brittleness of the chemical nickel plating layer can be reduced, which can solve the problem of easy brittle cracking when chemical nickel-palladium-gold is bound to copper wire or aluminum wire.

[0007] Optionally, the synthesis method of the complexing agent M comprises the following steps:

[0008] Evenly mixing diethylenetriaminepentaacetic acid and anhydrous ethanol to obtain a premixed solution;

[0009] Add allyl chloride to the premixed solution, then heat to 40-50° C., stir and react for 1-3 hours to obtain a reaction product;

[0010] The reaction product is subjected to rotary evaporation, washing and drying to obtain a complexing agent M;

[0011] Wherein, the mass ratio of diethylenetriaminepentaacetic acid, anhydrous ethanol and allyl chloride is 1:(4-6):(0.5-1.5).

[0012] Preferably, the mass ratio of diethylenetriaminepentaacetic acid, anhydrous ethanol and allyl chloride is 1:5:1.

[0013] In the second aspect, the low stress chemical nickel plating solution provided by the present application adopts the following technical solution:

[0014] A low stress chemical nickel plating solution comprises a composite complexing agent, a reducing agent, a water-soluble nickel salt, a water-soluble

[0015] A lead compound, polyethylene glycol, any one of the above low stress additives and deionized water;

[0016] The composite complexing agent includes lactic acid, malic acid and sodium succinate, wherein the volume concentration of the lactic acid in the low stress chemical nickel plating solution is 15-25 mL / L, the mass concentration of the malic acid in the low stress chemical nickel plating solution is 10-15 g / L, and the mass concentration of the sodium succinate in the low stress chemical nickel plating solution is 10-15 g / L;

[0017] The mass concentration of the reducing agent in the low stress chemical nickel plating solution is 20-30 g / L;

[0018] The mass concentration of the water-soluble nickel salt is 20-30 g / L;

[0019] The water-soluble lead compound is Pb 2+ Pb 2+ In the low stress chemical nickel plating solution

[0020] The concentration is 0.05-1.0ppm;

[0021] The volume concentration of the polyethylene glycol in the low stress chemical nickel plating solution is 0.1-1.0 g / L;

[0022] The mass concentration of the sodium m-nitrobenzene sulfonate in the low stress chemical nickel plating solution is 1-5 g / L;

[0023] The mass concentration of the complexing agent M in the low stress chemical nickel plating solution is 5-10 g / L.

[0024] In the present application, the chemical nickel plating solution uses lactic acid, malic acid and sodium succinate as composite chelating agents, which is beneficial to the stable nickel plating of the chemical nickel plating solution, thereby obtaining a chemical nickel plating layer with good uniformity. Secondly, the chemical nickel plating solution of the present application also adds low-stress additives sodium m-nitrobenzene sulfonate and chelating agent M. Through the synergistic effect of sodium m-nitrobenzene sulfonate and chelating agent M at a specific concentration, the stress of the nickel plating layer is reduced, and the brittleness of the chemical nickel plating layer is reduced, which can solve the problem of brittle cracking that is easy to occur when chemical nickel-palladium-gold is bound to copper wire or aluminum wire.

[0025] Preferably, the reducing agent is sodium hypophosphite.

[0026] In the present application, using sodium hypophosphite in the above mass concentration range as a reducing agent for chemical nickel plating solution is beneficial to obtaining a chemical nickel plating layer with a smooth surface, good corrosion resistance and good uniformity.

[0027] Preferably, the water-soluble lead compound is at least one of lead acetate and lead nitrate.

[0028] Preferably, the water-soluble nickel salt is nickel sulfate.

[0029] Preferably, the polyethylene glycol is at least one of polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.

[0030] In a third aspect, the present application provides a chemical nickel-palladium-gold plating process using the following technical solutions:

[0031] A chemical nickel-palladium-gold plating process comprises a chemical nickel deposition step, wherein the chemical nickel deposition step adopts any one of the above-mentioned low-stress chemical nickel plating solutions for chemical nickel deposition.

[0032] In the chemical nickel-palladium-gold plating process of the present application, the chemical nickel deposition step adopts low-stress chemical nickel plating solution for chemical nickel deposition, and the obtained chemical nickel plating layer has good uniformity and low brittleness, which can solve the problem of brittle cracking easily generated when chemical nickel-palladium-gold is bound to copper wire or aluminum wire.

[0033] Preferably, when the low stress chemical nickel plating solution is used for nickel deposition, the temperature of the low stress chemical nickel plating solution is 78-82° C., and the nickel deposition time is 20-30 min.

[0034] In summary, this application includes the following beneficial technical effects:

[0035] (1) In the present application, the complexing agent M is the reaction product of diethylenetriaminepentaacetic acid and allyl chloride and then dehydrochlorination. The synergistic combination of sodium m-nitrobenzenesulfonate and the complexing agent M can effectively improve the stability and dispersion ability of the chemical nickel plating solution, reduce the stress of the nickel plating layer, and reduce the brittleness of the chemical nickel plating layer, thereby solving the problem of brittle cracking when chemical nickel-palladium-gold is bound to copper wire or aluminum wire.

[0036] (2) In the present application, the chemical nickel plating solution uses lactic acid, malic acid and sodium succinate as composite complexing agents, which is conducive to the stable nickel plating of the chemical nickel plating solution, thereby obtaining a chemical nickel plating layer with good uniformity. Secondly, the chemical nickel plating solution of the present application also adds low-stress additives sodium m-nitrobenzene sulfonate and complexing agent M. Through the synergistic effect of sodium m-nitrobenzene sulfonate and complexing agent M at a specific concentration, the stress of the nickel plating layer is reduced, and the brittleness of the chemical nickel plating layer is reduced, which can solve the problem of brittle cracking when chemical nickel-palladium-gold is bound to copper wire or aluminum wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of the effect of chemical nickel-palladium-gold bonding copper wire or aluminum wire without brittle cracking.

[0038] Figure 2 This is a schematic diagram of the brittle cracking effect after chemical nickel-palladium-gold plating binds copper wire or aluminum wire.

[0039] Figure 3 This is a schematic diagram of the brittle cracking effect after chemical nickel-palladium-gold plating binds copper wire or aluminum wire. DETAILED DESCRIPTION

[0040] The present application is further described below in conjunction with specific experiments.

[0041] Preparation Example

[0042] [Preparation Example 1]

[0043] A complexing agent M, the preparation method comprises the following steps:

[0044] 1 kg of diethylenetriaminepentaacetic acid and 4 kg of anhydrous ethanol were uniformly mixed to obtain a premixed solution;

[0045] Add 0.5 kg of allyl chloride to the premixed solution, then heat to 40°C and stir to react for 3 hours to obtain a reaction product;

[0046] The reaction product is subjected to rotary evaporation, washing and drying to obtain the complexing agent M.

[0047] [Preparation Example 2]

[0048] A complexing agent M, the preparation method comprises the following steps:

[0049] 1 kg of diethylenetriaminepentaacetic acid and 6 kg of anhydrous ethanol were uniformly mixed to obtain a premixed solution;

[0050] Add 1 kg of allyl chloride to the premixed solution, then heat to 50 °C and stir for 1 hour to obtain

[0051] Reaction products;

[0052] The reaction product is subjected to rotary evaporation, washing and drying to obtain the complexing agent M.

[0053] Example

[0054] [Example 1]

[0055] A low-stress chemical nickel plating solution comprises a composite complexing agent, sodium hypophosphite, nickel sulfate, lead acetate, polyethylene glycol 1000, a low-stress additive and deionized water; wherein the composite complexing agent comprises lactic acid, malic acid and sodium succinate, and the low-stress additive comprises sodium m-nitrobenzene sulfonate and the complexing agent M prepared in [Preparation Example 1]. In addition, the concentration of each component in the low-stress chemical nickel plating solution is as follows:

[0056] Lactic acid: 15mL / L;

[0057] Malic acid: 15g / L;

[0058] Sodium succinate: 15g / L;

[0059] Sodium hypophosphite: 20g / L;

[0060] Nickel sulfate: 20g / L;

[0061] Lead acetate, Pb 2+ Pb 2+ The mass concentration in low stress chemical nickel plating solution is 0.05ppm;

[0062] Polyethylene glycol 1000: 0.1 g / L;

[0063] Sodium m-nitrobenzenesulfonate: 1g / L;

[0064] Complexing agent M: 10g / L;

[0065] Deionized water, balance.

[0066] [Example 2]

[0067] A low-stress chemical nickel plating solution comprises a composite complexing agent, sodium hypophosphite, nickel sulfate, lead acetate, polyethylene glycol 1000, a low-stress additive and deionized water; wherein the composite complexing agent comprises lactic acid, malic acid and sodium succinate, and the low-stress additive comprises sodium m-nitrobenzene sulfonate and the complexing agent M prepared in [Preparation Example 2]. In addition, the concentration of each component in the low-stress chemical nickel plating solution is as follows:

[0068] Lactic acid: 25 mL / L;

[0069] Malic acid: 10g / L;

[0070] Sodium succinate: 10g / L;

[0071] Sodium hypophosphite: 30g / L;

[0072] Nickel sulfate: 30g / L;

[0073] Lead acetate, Pb 2+ Pb 2+ The mass concentration in low stress chemical nickel plating solution is 1ppm;

[0074] Polyethylene glycol 1000: 1 g / L;

[0075] Sodium m-nitrobenzene sulfonate: 5g / L;

[0076] Complexing agent M: 5g / L;

[0077] Deionized water, balance.

[0078] Comparative Example

[0079] [Comparative Example 1]

[0080] A chemical nickel plating solution, which differs from [Example 1] in that the mass concentration of sodium m-nitrobenzene sulfonate is 11 g / L and no complexing agent M is added.

[0081] [Comparative Example 2]

[0082] A chemical nickel plating solution, which differs from [Example 1] in that the mass concentration of the complexing agent M is 11 g / L, and sodium m-nitrobenzene sulfonate is not added.

[0083] [Comparative Example 3]

[0084] A chemical nickel plating solution, which differs from [Example 1] in that sodium m-nitrobenzene sulfonate and complexing agent M are not added.

[0085] Application Examples

[0086]

Application Example 1

[0087] A chemical nickel-palladium-gold plating process comprises the following steps:

[0088] Step (1) sandblasting: sandblasting the printed circuit board;

[0089] Step (2) Degreasing: Clean the printed circuit board with Smet acid degreasing agent S-31 for 5 minutes, then rinse with water;

[0090] Step (3) micro-etching: immersing the printed circuit board treated in step (2) in a micro-etching solution for 2 minutes, and then washing with water; wherein the concentration of sodium persulfate in the micro-etching solution is 100 g / L, and the concentration of sulfuric acid is 50 g / L;

[0091] Step (4) pickling: immersing the printed circuit board treated in step (3) in a 100 g / L sulfuric acid solution for 3 min, and then washing with water;

[0092] Step (5) pre-acidification: immerse the printed circuit board treated in step (4) in a 50 g / L sulfuric acid solution for 2 min;

[0093] Step (6) activation: immerse the printed circuit board after the immersion in step (5) in a S-32 activator solution for activation for 5 minutes, and then wash with water;

[0094] Step (7) post-immersion: immerse the printed circuit board treated in step (6) in a 20 g / L sulfuric acid solution for 2 min, and then rinse with water;

[0095] Step (8) chemical nickel plating: immerse the printed circuit board treated in step (7) in the low stress chemical nickel plating solution of [Example 1] of the present application, and deposit nickel for 20 minutes at a nickel deposition temperature of 80° C., and then wash with water;

[0096] Step (9) chemical palladium deposition: immerse the printed circuit board treated in step (8) in Smet SPD-38 chemical palladium plating solution to deposit palladium. The palladium deposition time is 10 minutes and the palladium deposition temperature is 50°C.

[0097] Step (10) chemical gold plating: immerse the printed circuit board treated in step (9) in a reduced chemical gold plating solution of Smet SKG-22, with a gold plating time of 20 minutes and a temperature of 80° C. to obtain a printed circuit board with chemical nickel-palladium-gold plating.

[0098]

Application Example 2

[0099] A chemical nickel-palladium-gold plating process, which differs from [Application Example 1] in that: in step (8) chemical nickel deposition, the printed circuit board treated in step (7) is immersed in the low-stress chemical nickel plating solution of [Example 2] of this application, and the nickel deposition is carried out for 20 minutes at a nickel deposition temperature of 80°C, followed by water washing.

[0100] Comparative Application Examples

[0101]

Comparative Application Example 1

[0102] A chemical nickel-palladium-gold plating process, which differs from [Application Example 1] in that: in step (8) chemical nickel deposition, the printed circuit board treated in step (7) is immersed in the chemical nickel plating solution of [Comparative Example 1] of this application, and the nickel deposition is carried out for 20 minutes at a nickel deposition temperature of 80°C, followed by water washing.

[0103]

Comparative Application Example 2

[0104] A chemical nickel-palladium-gold plating process, which differs from [Application Example 1] in that: in step (8) chemical nickel deposition, the printed circuit board treated in step (7) is immersed in the chemical nickel plating solution of [Comparative Example 2] of this application, and the nickel deposition is carried out for 20 minutes at a nickel deposition temperature of 80°C, followed by water washing.

[0105]

Comparative Application Example 3

[0106] A chemical nickel-palladium-gold plating process, which differs from [Application Example 1] in that: in step (8) chemical nickel deposition, the printed circuit board treated in step (7) is immersed in the chemical nickel plating solution of [Comparative Example 3] of this application, and the nickel deposition is carried out for 20 minutes at a nickel deposition temperature of 80°C, followed by water washing.

[0107] Performance testing

[0108] The products obtained from each application example and comparative application example are bound with copper wires or aluminum wires according to regulations. After standing for 48 hours, the copper wires or aluminum wires are removed, and then the coating of the printed circuit board is observed to see if brittle cracks occur.

[0109] Table 1

[0110] sample Binding copper wire Aluminum wire binding Application Example 1 No brittle crack No brittle crack Application Example 2 No brittle crack No brittle crack Comparative application example 1 Brittle Brittle Comparative Application Example 2 Brittle Brittle Comparative Application Example 3 Brittle Brittle

[0111] Combining the above-mentioned comparative application example 1 with application example 1, it can be seen that when the chemical nickel plating solution uses sodium m-nitrobenzene sulfonate alone as a low-stress additive, it cannot solve the problem of easy brittle cracking when chemical nickel-palladium-gold is bound to copper wire or aluminum wire.

[0112] Combining the above comparative application example 2 with application example 1, it can be seen that when the chemical nickel plating solution uses the complexing agent M alone as a low-stress additive, it cannot solve the problem of brittle cracking when the chemical nickel-palladium-gold is bound to the copper wire or aluminum wire.

[0113] Combining the above comparative application example 3 with application example 1, it can be seen that when the chemical nickel plating solution does not add low-stress additives, it is impossible to solve the problem of brittle cracking when the chemical nickel-palladium-gold is bound to the copper wire or aluminum wire.

[0114] Combined with Application Examples 1-2, it can be seen that when sodium m-nitrobenzene sulfonate and complexing agent M within a specific concentration range are added simultaneously as low-stress additives to the chemical nickel plating solution, the problem of brittle cracking that is prone to occur when chemical nickel-palladium-gold is bound to copper wire or aluminum wire can be effectively solved.

[0115] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low stress additive, characterized in that: The invention comprises sodium m-nitrobenzene sulfonate and a complexing agent M, wherein the complexing agent M is a reaction product of diethylenetriaminepentaacetic acid and allyl chloride and then HCl is removed. The synthesis method of the complexing agent M comprises the following steps: Evenly mixing diethylenetriaminepentaacetic acid and anhydrous ethanol to obtain a premixed solution; Add allyl chloride to the premixed solution, then heat to 40-50°C and stir to react for 1-3h. obtaining a reaction product; The reaction product is subjected to rotary evaporation, washing and drying to obtain a complexing agent M; Wherein, the mass ratio of diethylenetriaminepentaacetic acid, anhydrous ethanol and allyl chloride is 1:(4-6):(0.5-1.5).

2. A low stress additive according to claim 1, characterized in that: The mass ratio of the diethylenetriaminepentaacetic acid, anhydrous ethanol and allyl chloride is 1:5:

1.

3. A low stress chemical nickel plating solution, characterized in that: It comprises a composite complexing agent, a reducing agent, a water-soluble nickel salt, a water-soluble lead compound, polyethylene glycol, the low stress additive according to any one of claims 1 to 2, and deionized water; The composite complexing agent includes lactic acid, malic acid and sodium succinate, wherein the volume concentration of the lactic acid in the low stress chemical nickel plating solution is 15-25 mL / L, the mass concentration of the malic acid in the low stress chemical nickel plating solution is 10-15 g / L, and the mass concentration of the sodium succinate in the low stress chemical nickel plating solution is 10-15 g / L; The mass concentration of the reducing agent in the low stress chemical nickel plating solution is 20-30 g / L; The mass concentration of the water-soluble nickel salt is 20-30 g / L; The water-soluble lead compound is Pb 2+ Pb 2+ In the low stress chemical nickel plating solution The concentration is 0.05-1.0ppm; The volume concentration of the polyethylene glycol in the low stress chemical nickel plating solution is 0.1-1.0 g / L; The mass concentration of the sodium m-nitrobenzene sulfonate in the low stress chemical nickel plating solution is 1-5 g / L; The mass concentration of the complexing agent M in the low stress chemical nickel plating solution is 5-10 g / L.

4. A low stress chemical nickel plating solution according to claim 3, characterized in that: The reducing agent is sodium hypophosphite.

5. The low stress chemical nickel plating solution according to claim 3, characterized in that: The water-soluble lead compound is at least one of lead acetate and lead nitrate.

6. The low stress chemical nickel plating solution according to claim 3, characterized in that: The water-soluble nickel salt is nickel sulfate.

7. The low stress chemical nickel plating solution according to claim 3, characterized in that: The polyethylene glycol is at least one of polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.

8. A chemical nickel-palladium-gold plating process, characterized in that: The method comprises a chemical nickel deposition step, wherein the chemical nickel deposition step adopts a low-stress chemical nickel plating solution as described in any one of claims 3 to 7 for chemical nickel deposition.

9. A chemical nickel-palladium-gold plating process according to claim 8, characterized in that: When the low stress chemical nickel plating solution is used for nickel deposition, the temperature of the low stress chemical nickel plating solution is 78-82° C., and the nickel deposition time is 20-30 min.

Citation Information

Patent Citations

  • A chemical nickel plating solution and a chemical nickel plating process

    CN102268658A

  • Substitution type electroless gold plating bath containing purine or pyrimidine-based compound having carbonyl oxygen and method using same

    CN110923680A

  • Double-complexing-system low-stress electroless copper plating solution and preparation method and application thereof

    CN113897600A

  • Lead-free environment-friendly chemical nickel liquid medicine and preparation process thereof

    CN113957422A

  • Process formula of chemical nickel-palladium-gold plating liquid for aluminum substrate of power chip

    CN117758244A