A bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material and preparation method thereof

By constructing C-N-Mn bonds on the surface of porous carbon in bamboo thin-walled cells and anchoring Mn oxides, the problem of insufficient cyclic stability and capacity performance of manganese dioxide and porous carbon material composites in electrochemical energy storage is solved, and a It has high specific capacity and good cycle stability, and is suitable for zinc ion hybrid capacitors.

CN118486551BActive Publication Date: 2024-11-26INT CENT FOR BAMBOO & RATTAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410651875.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-26
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

The insufficient cyclic stability and capacity performance of existing manganese dioxide and porous carbon material composites in electrochemical energy storage leads to their unstable electron transmission paths and lower capacity in electrochemical energy storage applications.

Method used

By constructing C-N-Mn chemical bonds, Mn oxide is anchored on the surface of porous charcoal of bamboo thin-walled cells, forming a bamboo thin-walled cell porous charcoal nitrogen grafted manganese oxide composite electrode material, strengthening the connection of Mn and building stable electron transport channel to improve its electrochemical properties.

Benefits of technology

Achieve high specific capacity and good cycling stability. The zinc ion hybrid capacitor provides a specific capacity of 248.3mAh/g in the voltage range of 0-1.6V, and the capacity retention rate reaches after cycling for 10,000 cycles at 8.8A/g current density. 88.1%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118486551B_ABST
    Figure CN118486551B_ABST
Patent Text Reader

Abstract

The present invention relates to a bamboo thin-walled cell porous carbon nitrogen-grafted manganese oxide composite electrode material, wherein the specific surface area of ​​the bamboo thin-walled cell porous carbon is 1000-1500m 2 / g, with both micropores and mesopores, microporosity of 60-70%, mesoporosity of 20-30%, and tap density of 0.2-0.3g / cm 3 , the flake δ-MnO2 is anchored on the inner surface of the bamboo parenchyma cell porous carbon cavity by C-N-Mn bonds. The present invention uses hydrothermal grafting to anchor MnO2 on the surface of the bamboo parenchyma cell porous carbon by C-N-Mn bonds, optimizes the composite interface and stabilizes the electron transmission structure. The above-mentioned electrochemical energy storage composite material of the present invention has a stable structure, controllable morphology, and a large specific surface area. The microscopic morphology of the composite material is flaky, which is more conducive to the transmission of electrolyte ions, so that the specific capacity of the composite material can reach 248.3mAh / g, and the capacitance retention rate after repeated charge and discharge 10,000 times at a higher current density is still as high as 88.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical energy storage materials, and in particular to a bamboo thin-wall cell porous carbon-nitrogen grafted manganese oxide composite electrode material and a preparation method thereof. Background Art

[0002] The depletion of oil resources and environmental pollution have promoted the development of sustainable energy. As a new type of electrochemical energy storage device, zinc ion hybrid capacitors combine the energy storage advantages of batteries and capacitors, showing the advantages of long cycle life, high capacity performance, and high power density.

[0003] The pores and structures of electrode materials are the main factors affecting the electrochemical performance of energy storage devices. Among them, biomass-derived carbon materials with porous structures are the most commonly used positive electrode materials for zinc ion hybrid capacitors. Bamboo parenchyma cells are biomass raw materials separated from bamboo with multi-walled, porous, and cavity structures. After carbonization and activation, they can become porous carbons with high specific surface area and rich pore structures. Different from traditional petroleum-based and coconut shell porous carbons, the surface of multi-walled bamboo parenchyma cells contains relatively abundant micropores, which is conducive to full contact with the activator to build a more developed pore structure and optimize the contact surface between the electrolyte and the battery material. In addition, its cavity structure provides a larger reaction interface for heterogeneous composites or metal loading.

[0004] The introduction of pseudocapacitors through transition metals is currently the main way to further improve the volume energy density of porous carbon materials. Manganese dioxide (MnO2) is a cheap, environmentally friendly and high theoretical capacity pseudocapacitor electrode material, but MnO2 has low intrinsic conductivity, poor structural stability and insufficient specific surface area, which limits its application in electrochemical energy storage. The composite of manganese dioxide and porous carbon materials can play a synergistic role, especially the porous carbon of bamboo parenchyma cells with a cavity structure has abundant internal and external surface pores, providing sufficient space for manganese dioxide anchoring. In the prior art, the preparation method of such composite materials is to prepare manganese / carbon composite materials by hydrothermal reaction of carbon and manganese source, but the composite relationship between the two is not explained, only that manganese dioxide is coated on the carbon surface. Because the composite relationship between manganese dioxide and the carbon surface is unstable, and manganese will have structural deformation and dissolution problems during the charge and discharge process, it shows insufficient cycle stability and capacity performance. Pseudocapacitance is achieved through redox reactions to transmit and transfer electrons. Its electron transmission path / channel must maintain good stability, which makes the pore structure of porous carbon materials and the anchoring or connection method of manganese dioxide on porous carbon particularly important. Therefore, building a stable electrochemical reaction interface and promoting electron transmission / transfer are the keys to improving the electrochemical performance of porous carbon and manganese dioxide composites. Summary of the invention

[0005] In order to solve the problem that the electrochemical performance of the composite material of manganese dioxide and porous carbon material in the prior art cannot meet the requirements of industrialization, especially the defects of low capacity and poor cycle stability, the present invention provides a bamboo thin-walled cell porous carbon nitrogen grafted manganese oxide composite electrode material. Aiming at the problem of poor cycle stability of manganese-based composite materials, Mn oxide is anchored on the surface of the carbon matrix by constructing CN-Mn chemical bonds, and the connection of Mn is strengthened to improve stability. Thin-walled cells are selected because their large cavities and pores are convenient for loading and ion access. The present invention provides the following technical solutions to solve the above technical problems.

[0006] The present invention first provides a bamboo thin-walled cell porous carbon nitrogen-grafted manganese oxide composite electrode material, wherein the specific surface area of ​​the bamboo thin-walled cell porous carbon is 1000-1500m 2 / g, with both micropores and mesopores, microporosity of 60-70%, mesoporosity of 20-30%, and tap density of 0.2-0.3g / cm 3 , flake-like δ-MnO2 is anchored on the inner surface of the porous carbon cavity of bamboo parenchyma cells through CN-Mn bonds.

[0007] Furthermore, the loading rate of MnO2 is 30-40%, such as 33.4%.

[0008] Furthermore, the composite electrode material has the following characteristic peaks of the XPS C1s spectrum: 284.2±0.1eV, 285.7±0.1eV, and 288.0±0.1eV; the composite electrode material has the following characteristic peaks of the XPS N1s spectrum: 400.5±0.1eV, 399.2±0.1eV, and 398.2±0.1eV.

[0009] In the XPS C1s spectrum, the characteristic peak near 284.2eV is the CC bond, the characteristic peak near 285.7eV is the CN bond, and the characteristic peak near 288eV is the OC=O bond; in the XPS N1s spectrum, the characteristic peak near 400.5eV is the graphite-N bond, the characteristic peak near 399.2eV is the Mn-N bond, and the characteristic peak near 398.2eV is the pyridine-N bond.

[0010] The present invention uses bamboo thin-walled cell porous carbon as a carrier of flaky δ-MnO2. The bamboo thin-walled cell porous carbon has abundant pores and cavities, and a large number of micropores and mesopores can achieve high heterogeneous loading. By comparing the activator impregnation experiment, it is found that the loading amount of bamboo thin-walled cell KHCO3 activator is 2.6 times that of bamboo charcoal fiber, and the specific surface area of ​​bamboo thin-walled cell porous carbon after direct high-temperature activation is 1.7 times that of bamboo fiber porous carbon. This provides a good interface for the composite of manganese oxide, strengthens the connection between porous carbon and manganese oxide, and constructs a stable electron transmission channel, thereby improving its electrochemical performance.

[0011] The second object of the present invention is to provide a method for preparing the above-mentioned bamboo thin-walled cell porous carbon-nitrogen grafted manganese oxide composite electrode material, comprising the following steps:

[0012] (S1) placing the bamboo parenchyma cell raw material in a tubular furnace, heating it to 500-600° C. at a heating rate of 5° C. / min under nitrogen protection, and keeping the temperature for 2-4 hours to obtain a carbonized material;

[0013] (S2) grinding and mixing the carbonized material and KHCO3, placing the mixture in a tube furnace, heating the mixture to 900-1200° C. under nitrogen protection, and keeping the temperature for 2-4 hours to obtain porous bamboo parenchyma cell carbon;

[0014] (S3) placing the bamboo parenchyma cell porous carbon in a mixed solution of sulfuric acid and concentrated nitric acid and stirring to obtain surface-modified bamboo parenchyma cell porous carbon;

[0015] (S4) adding manganese sulfate, potassium permanganate and potassium sulfate into water, ultrasonicating and stirring to mix, subjecting the mixed solution to a hydrothermal reaction, and washing and drying the obtained product to obtain δ-MnO2;

[0016] (S5) placing δ-MnO2 in a tube furnace, under nitrogen protection, heating to 300-400°C, and keeping the temperature for 1-2 hours to obtain a product of oxygen-deficient δ-MnO;

[0017] (S6) The surface-modified bamboo parenchyma cell porous carbon and the oxygen-rich defect δ-MnO2 are placed in a urea solution, uniformly mixed and then subjected to a hydrothermal reaction. The obtained product is washed with water and dried to obtain a bamboo parenchyma cell porous carbon nitrogen-grafted manganese oxide composite electrode material.

[0018] Furthermore, in steps (S1), (S2) and (S5), the heating rate is 5-20°C / min.

[0019] Furthermore, in step (S1), the bamboo parenchyma cell raw material and the polymer resin carbon source are mixed and placed in a tubular furnace, the polymer resin carbon source is selected from at least one of phenolic resin and urea-formaldehyde resin, and the mass ratio of the bamboo parenchyma cell raw material to the polymer resin carbon source is 1-3:1-3.

[0020] Furthermore, in step (S2), the mass ratio of the carbonized material to KHCO3 is 1:3-5.

[0021] Furthermore, in step (S3), the mass ratio of concentrated sulfuric acid to concentrated nitric acid is 3-4:1, and the volume ratio of the mixed acid to the bamboo parenchyma cell porous carbon obtained in step (S2) is 30-40 ml: 1 g.

[0022] Furthermore, in step (S4), the mass ratio of manganese sulfate, potassium permanganate and potassium sulfate is 1-2:1-2:1-2; the hydrothermal reaction conditions are 150-180° C. and the time is 10-20 h.

[0023] Furthermore, in step (S6), the urea concentration is 0.01-0.1 mol / L, such as 0.05 mol / L; the ratio of surface-modified bamboo parenchyma cell porous carbon, oxygen-rich defect δ-MnO2 and urea solution is 1-2 g: 1-2 g: 40-60 mL; the hydrothermal reaction temperature is 120-140°C, and the time is 5-8 hours.

[0024] The present invention prepares a porous carbon matrix by first carbonizing bamboo parenchyma cells and then alkali activating them, and then performs surface oxidation treatment; prepares oxygen-deficient δ-MnO2; then adds the surface-modified porous carbon matrix and the oxygen-deficient δ-MnO2 into a nitrogen-containing solution for hydrothermal reaction, and anchors MnO2 on the surface of the bamboo porous carbon matrix through Mn-NC bonds. The present invention makes full use of the cavities of bamboo parenchyma cells and the porous structure to provide a rich and stable composite interface for the flake δ-MnO2, enriches the electrochemical reaction interface and improves the stability of the electron transmission path.

[0025] The present invention provides a carbon electrode, comprising the following raw materials: the above-mentioned bamboo parenchyma cell porous carbon nitrogen grafted manganese oxide composite electrode material, a conductive carbon material and a binder. Furthermore, the mass ratio of the bamboo parenchyma cell porous carbon nitrogen grafted manganese oxide composite electrode material, the conductive carbon material and the binder is 7-9:1-2:1-2, the conductive carbon material is selected from at least one of carbon black, SuperP, acetylene black, and graphene, and the binder is selected from at least one of polyvinylidene fluoride and styrene-butadiene latex. Furthermore, the raw materials for preparing the carbon electrode also include an appropriate amount of solvent, such as N-methylpyrrolidone solution, which is fully ground into a slurry, coated on a carbon cloth, and vacuum dried to obtain the carbon electrode.

[0026] The present invention also provides a zinc ion hybrid capacitor, comprising a zinc foil negative electrode, a cellulose diaphragm and an electrolyte of 0.1-2 mol / L ZnSO4 impregnated therein, and the above-mentioned carbon electrode positive electrode.

[0027] The present invention adopts bamboo thin-walled cells with multi-walled, hollow and porous structures as carbon sources, and obtains a rich specific surface area (1340m 2 / g) and porous carbon with multi-level pore structure provide rich interfaces for manganese dioxide grafting. Urea is used as nitrogen source to construct CN-Mn bonds, and manganese dioxide is firmly anchored on the surface of porous carbon by bond grafting, which constructs a stable electron transmission channel and promotes redox reaction, thereby improving electrochemical capacity and cycle stability. The aqueous zinc ion hybrid capacitor based on bamboo parenchyma cell porous carbon nitrogen grafted manganese oxide composite electrode material as the positive electrode material can provide 248.3mAh / g (0.2A g -1 ) specific capacity, even at 5A g -1 At a current density of 1.5A / g, the specific capacity is still 70.4mAh / g. After 10,000 cycles at a current density of 8.8A / g, the capacity retention rate is 88.1%.

[0028] The advantages of the present invention compared with the prior art are:

[0029] 1) The present invention uses bamboo parenchyma cells as raw materials, which are cheap, easily available and abundant as woody biomass. The abundant original pores of bamboo parenchyma cells are conducive to the activation and preparation of activated carbon with rich pore structure, and the cavity structure provides a rich interface for the anchoring of metal heteroatoms.

[0030] 2) The present invention stabilizes the connection between manganese dioxide and porous carbon by constructing CN-Mn bonds, providing a stable electron transmission path. It is applied to the positive electrode of zinc ion hybrid capacitors, has high specific capacity and good cycle stability, and is a positive electrode material that is expected to be industrialized. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The SEM images of the bamboo thin-walled cell porous carbon and bamboo fiber porous carbon electrode materials prepared in Example 1 and Comparative Example 1 are as follows:

[0032] Figure 2 The SEM images of the manganese oxide bamboo thin-walled cell porous carbon composite electrode and the manganese oxide bamboo fiber porous carbon composite electrode material prepared in Example 2 and Comparative Example 2 are shown in FIG.

[0033] Figure 3 The SEM spectrum and energy spectrum of the bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material obtained in Example 3

[0034] Figure 4 This is the C1s and N1s spectrum of the bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material prepared in Example 2.

[0035] Figure 5 This is the XRD diffraction pattern of δ-MnO2 obtained in Example 3.

[0036] Figure 6This is a graph showing the specific capacity of the porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells prepared in Example 4 as a zinc ion hybrid capacitor.

[0037] Figure 7 This is the cycle performance curve of the manganese oxide bamboo thin-walled cell porous carbon composite electrode material prepared in Example 3 as a zinc ion hybrid capacitor.

[0038] Figure 8 This is the cycle performance curve of the porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells prepared in Example 4 as a zinc ion hybrid capacitor.

[0039] Fig. 9 This is a scanning electron microscope energy spectrum of the bamboo parenchyma cell / urea-formaldehyde resin composite electrode material and the bamboo fiber / urea-formaldehyde resin composite electrode material obtained in Example 5. DETAILED DESCRIPTION

[0040] To make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be described in detail below. The following examples are convenient for better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified.

[0041] Example 1

[0042] (I) Preparation of porous carbon electrode materials from bamboo parenchyma cells activated by one-step carbonization

[0043] S1: 3g of bamboo parenchyma cells and 3g of bamboo fibers were soaked in 2M KHCO3 solution, super stirred and allowed to stand for 12h, the solution was filtered out and then dried in an oven at 80°C for 12h to obtain activated bamboo parenchyma cells and activated bamboo fibers, respectively.

[0044] S2: The activated bamboo parenchyma cells and activated bamboo fibers were placed in a corundum burning boat and calcined in a tubular furnace. Under the condition of N2 purge flow rate of 0.2mL / min, the temperature was increased to 850℃ at a rate of 5℃ / min and kept for 2h for carbonization. After the reaction, it was naturally cooled to room temperature and taken out. After acid washing, water washing and drying, a porous carbon material was obtained. After testing, it was found that in the impregnation experiment, the weight of bamboo parenchyma cells increased by 0.0744g, and the weight of bamboo fibers increased by 0.0287g. The impregnation amount of KHCO3 activator of bamboo parenchyma cells was 2.6 times that of bamboo fibers. After activation at 850℃, the specific surface area of ​​porous carbon of bamboo parenchyma cells was 827m 2 / g, the specific surface area of ​​bamboo fiber porous carbon is 487m 2 / g, the specific surface area of ​​bamboo parenchyma cell porous carbon is 1.7 times that of bamboo fiber.

[0045] Example 2

[0046] (I) Preparation of porous carbon electrode materials from bamboo parenchyma cells

[0047] S1: Pour 10g of bamboo parenchyma cells into a corundum boat, place the boat in a tube furnace, and heat to 500℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min for 2h for carbonization. After the reaction is completed, cool naturally to room temperature and take out.

[0048] S2: Grind and mix 2g of the carbonized bamboo parenchyma cell charcoal and 6g of activator KHCO3, pour into a corundum boat, place the boat in a tube furnace, heat to 900℃ at a heating rate of 5℃ / min and keep warm for 2h under the condition of N2 purge flow rate of 0.2mL / min, and cool to room temperature naturally after the reaction. After acid washing and drying, the porous bamboo parenchyma cell charcoal is obtained, which is marked as PC-900. After testing, the specific surface area of ​​PC-900 is 1340m 2 / g, microporosity is 68%, mesoporosity is 24%, and tap density is 0.2726g / cm 3 .

[0049] Comparative Example 1

[0050] (I) Preparation of bamboo fiber porous carbon electrode materials

[0051] S1: Pour 10g of bamboo fiber into a corundum boat, place the boat in a tubular furnace, and heat to 500℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min for 2h for carbonization. After the reaction is completed, cool naturally to room temperature and take out.

[0052] S2: 2g of the carbonized bamboo fiber carbon and 6g of activator KHCO3 were ground and mixed, and then poured into a corundum burning boat. The burning boat was placed in a tube furnace, and heated to 900℃ at a heating rate of 5℃ / min for 2h under the condition of N2 purge flow rate of 0.2mL / min for carbonization. After the reaction was completed, it was naturally cooled to room temperature. After acid washing and drying, bamboo fiber porous carbon was obtained, which was marked as CF-900. After testing, the specific surface area of ​​CF-900 was 798m 2 / g, microporosity is 70%, mesoporosity is 23%, and tap density is 0.3126g / cm 3 .

[0053] Figure 1The SEM images of the porous carbon of bamboo thin-walled cells and porous carbon of bamboo fibers prepared in Example 2 and Comparative Example 1 are shown. It can be seen that multiple bamboo fibers are bonded together by lignin. Since the cavity is small, it is difficult for the activator to enter, so the voids are mainly distributed on the outer surface. There are a large number of micrometer-sized pores on the wall of bamboo thin cells. These natural pore structures provide channels for biomass exchange between adjacent cells, promote activator activation and pore formation to construct developed pores, and the larger accessible surface of the thin-walled cells facilitates the anchoring of manganese oxide loading.

[0054] Application Example 1

[0055] The preparation of zinc ion hybrid capacitor includes the following steps:

[0056] 1. The PC-900 prepared above and the electrode material were mixed with acetylene black and polyvinylidene fluoride binder in a mass ratio of 8:1:1, and an appropriate amount of NMP was added dropwise, and the slurry was completely stirred to form a slurry, which was then coated on carbon paper as the positive electrode of the zinc ion hybrid capacitor;

[0057] 2. Prepare 2 mol / L / L zinc sulfate aqueous solution as the electrolyte of zinc ion hybrid capacitor;

[0058] 3. Zinc ion hybrid capacitors were assembled in the order of zinc metal negative electrode, cellulose diaphragm (with zinc sulfate electrolyte added), and porous carbon electrode material positive electrode. Based on the mass calculation of the positive electrode material, the maximum specific capacities of bamboo parenchyma cell porous carbon electrode materials PC-900 and CF-900 at a current density of 0.5A / g were 94.6mAh / g and 73mAh / g, respectively.

[0059] Example 3

[0060] (I) Preparation of manganese oxide bamboo parenchyma cell porous carbon composite electrode material

[0061] S1: Pour 10g of bamboo parenchyma cells into a corundum boat, place the boat in a tube furnace, heat to 500℃ at a heating rate of 5℃ / min and keep warm for 2h under the condition of N2 purge flow rate of 0.2mL / min for carbonization. After the reaction is completed, cool naturally to room temperature and take out the bamboo parenchyma cell charcoal.

[0062] S2: Grind and mix 2g of the carbonized bamboo parenchyma cell charcoal and 6g of activator KHCO3, add a small amount of water and stir for 4h, and place in a 60℃ oven to dry for 12h. Pour the dried mixture into a corundum boat, place the boat in a tube furnace, and heat to 900℃ at a heating rate of 5℃ / min for 2h under the condition of N2 purge flow rate of 0.2mL / min for carbonization. After the reaction is completed, cool naturally to room temperature and take out the porous bamboo parenchyma cell charcoal.

[0063] S3: The carbonized bamboo parenchyma cell porous carbon was added into 80 mL of concentrated acid solution, wherein the ratio of concentrated sulfuric acid to concentrated hydrochloric acid was 3:1; the carbonized bamboo parenchyma cell porous carbon was filtered after magnetic stirring at room temperature for 6 hours, and then washed with deionized water until neutral, and dried in an oven at 105°C to obtain surface-modified bamboo parenchyma cell porous carbon.

[0064] S4: Take 2g, 2g, and 1g of KMnO4, MnSO4, and K2SO4 respectively in a mass ratio of 2:2:1, add them into 40ml water, stir and mix thoroughly, and then put them into a 50ml polytetrafluoroethylene-lined reactor. Place the reactor in a muffle furnace and calcine at 160℃ for 12h. After the reaction is completed, cool it naturally to room temperature, take it out and wash it with water to obtain δ-MnO2. Figure 5 This is the XRD pattern of the obtained δ-MnO2.

[0065] S5: Pour the above-mentioned δ-MnO2 into a crucible, place the crucible in a tubular furnace, heat to 300℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min, and keep warm for 1h. After the reaction is completed, naturally cool to room temperature, take out, and obtain oxygen-deficient δ-MnO2.

[0066] S6: Take 1g of the surface modified bamboo parenchyma cell porous carbon from the above step (S3) and 1g of the oxygen-deficient δ-MnO2 from step (S5), add them into 40ml of water, sonicate and stir thoroughly, put the dispersion sample into a 50ml polytetrafluoroethylene-lined reactor, place the reactor in a muffle furnace and react at 140°C for 6h. After the reaction is completed, naturally cool to room temperature, take out and wash with water to obtain a manganese oxide bamboo parenchyma cell porous carbon composite electrode material, recorded as PC-900-MnO2.

[0067] Comparative Example 2

[0068] (I) Preparation of manganese oxide bamboo fiber porous carbon composite electrode materials

[0069] S1: Pour 10g of bamboo fiber into a corundum boat, place the boat in a tubular furnace, and heat to 500℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min for 2h for carbonization. After the reaction is completed, cool naturally to room temperature and take out the bamboo fiber charcoal.

[0070] S2: Grind and mix 2g of the carbonized bamboo fiber charcoal and 6g of activator KHCO3, add a small amount of water and stir for 4h, and place in a 60℃ oven to dry for 12h. Pour the dried mixture into a corundum boat, place the boat in a tube furnace, and heat to 900℃ at a heating rate of 5℃ / min for 2h under the condition of N2 purge flow rate of 0.2mL / min for carbonization. After the reaction is completed, naturally cool to room temperature and take out the porous bamboo fiber charcoal.

[0071] S3: The carbonized bamboo fiber porous carbon was added into 80 mL of concentrated acid solution, wherein the ratio of concentrated sulfuric acid to concentrated hydrochloric acid was 3:1; the mixture was magnetically stirred at room temperature for 6 h and then filtered, and then washed with deionized water until neutral, and dried in an oven at 105°C to obtain surface-modified bamboo fiber porous carbon.

[0072] S4: Take 2g, 2g, and 1g of KMnO4, MnSO4, and K2SO4 respectively in a mass ratio of 2:2:1, add them into 40ml water, stir and mix thoroughly, and then put them into a 50ml polytetrafluoroethylene-lined reactor. Place the reactor in a muffle furnace and calcine at 160℃ for 12h. After the reaction is completed, cool it naturally to room temperature, take it out and wash it with water to obtain δ-MnO2.

[0073] S5: Pour the above-mentioned δ-MnO2 into a crucible, place the crucible in a tubular furnace, heat to 300℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min, and keep warm for 1h. After the reaction is completed, naturally cool to room temperature, take out, and obtain oxygen-deficient δ-MnO2.

[0074] S6: Take 1g of the surface-modified bamboo fiber porous carbon from the above step (S3) and 1g of the oxygen-deficient δ-MnO2 from step (S5), add them into 40ml of water, sonicate and stir thoroughly, put the dispersion sample into a 50ml polytetrafluoroethylene-lined reactor, place the reactor in a muffle furnace and react at 140°C for 6h. After the reaction is completed, naturally cool to room temperature, take out and wash with water to obtain a bamboo fiber porous carbon composite electrode material, recorded as CF-900-MnO2.

[0075] Figure 2 This is the SEM spectrum of the manganese oxide bamboo thin-walled cell porous carbon composite electrode and the manganese oxide bamboo fiber porous carbon composite electrode material prepared in Example 3 and Comparative Example 2. It can be seen that the bamboo thin-walled cells can anchor more manganese oxide than the fibers.

[0076] Application Example 2

[0077] The preparation of zinc ion hybrid capacitor includes the following steps:

[0078] 1. The PC-900-MnO2 and CF-900-MnO2 electrode materials prepared above were mixed with acetylene black and polyvinylidene fluoride binder in a mass ratio of 8:1:1, and an appropriate amount of NMP was added dropwise, and the slurry was completely stirred to form a slurry, which was then coated on carbon paper as the positive electrode of the zinc ion hybrid capacitor;

[0079] 2. Prepare 2 mol / L / L zinc sulfate aqueous solution as the electrolyte of zinc ion hybrid capacitor;

[0080] 3. Assemble the zinc ion hybrid capacitor in the order of zinc metal negative electrode, cellulose diaphragm (add zinc sulfate electrolyte), and porous carbon electrode material positive electrode. Based on the mass calculation of the positive electrode material, the maximum specific capacity of PC-900-MnO2 and CF-900-MnO2 at a current density of 0.5A / g is 110mAh / g and 86.5mAh / g, respectively. Figure 7 It can be seen that the capacity retention rate of PC-900-MnO2 is 85% after 8000 cycles at a current density of 8.8 A / g.

[0081] Example 4

[0082] (I) Preparation of bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material, comprising the following steps:

[0083] S1: Put 10g of bamboo parenchyma cells into a corundum boat, place the boat in a tube furnace, heat to 500℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min, keep warm for 2h for carbonization treatment, cool naturally to room temperature after the reaction is completed, and take out the bamboo parenchyma cell charcoal.

[0084] S2: Grind and mix 2g of the above-mentioned bamboo parenchyma cell charcoal with 6g of activator KHCO3, put them into a corundum boat, place the boat in a tube furnace, and heat to 900℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min. Keep warm for 2h for activation treatment. After the reaction is completed, cool naturally to room temperature, take out and wash with 2mol / L hydrochloric acid and deionized water in turn until neutral, and then dry the bamboo parenchyma cell porous charcoal.

[0085] S3: Take 2 g of the above-mentioned bamboo parenchyma cell porous carbon and add it into 80 mL of concentrated acid solution, in which the ratio of concentrated sulfuric acid to concentrated hydrochloric acid is 3:1; stir magnetically at room temperature for 6 hours, filter, wash with deionized water until neutral, and dry to obtain surface-modified bamboo parenchyma cell porous carbon.

[0086] S4: Take 2g, 2g, and 1g of KMnO4, MnSO4, and K2SO4, add them into 80ml water, stir and mix thoroughly, then put them into a 100ml polytetrafluoroethylene-lined reactor, place the reactor in a muffle furnace and calcine at 160℃ for 12h. After the reaction is completed, cool it naturally to room temperature, take it out, wash it with water, and dry it to obtain δ-MnO2.

[0087] S5: Pour the above δ-MnO2 into a corundum boat, place the boat in a tubular furnace, heat to 300℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min, and keep warm for 1h. After the reaction is completed, naturally cool to room temperature, take out, and obtain oxygen-deficient δ-MnO2.

[0088] S6: Prepare 0.5mol / L urea solution, take 1g of the surface-modified bamboo parenchyma cell porous carbon in the above step (S3) and 1g of the oxygen-deficient δ-MnO2 in step (S5) and add them to the urea solution, ultrasonicate and stir thoroughly, put the mixed solution into a 50ml polytetrafluoroethylene-lined reactor, place the reactor in a muffle furnace at 140°C for 6h, cool naturally to room temperature after the reaction, take out and wash, and obtain the bamboo parenchyma cell porous carbon nitrogen-grafted manganese oxide composite electrode material, recorded as PC-N-MnO2. After testing, the MnO2 loading is 33.4wt%.

[0089] Figure 3 The SEM spectrum and energy spectrum of the bamboo parenchyma cell porous carbon nitrogen-grafted manganese oxide composite electrode material obtained in Example 4 show that manganese oxide and nitrogen elements are evenly distributed in the composite electrode material and their distribution positions are basically overlapped, and δ-MnO2 is anchored on the surface of the bamboo parenchyma cell porous carbon. Nitrogen doping of the porous carbon can improve the conductivity and electrolyte wettability of the composite material, which has an important improvement effect on the poor intrinsic conductivity of manganese oxide and the unstable electron transmission path.

[0090] Figure 4 The C1s and N1s spectra of the porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells prepared in Example 4. The composite electrode material has the following characteristic peaks of the XPS C1s spectrum: 284.2±0.1ev, 285.7±0.1ev, and 288.0±0.1ev. The characteristic peak near 284.2eV is the CC bond, the characteristic peak near 285.7eV is the CN bond, and the characteristic peak near 288eV is the OC=O bond. The composite material has the following characteristic peaks of the XPS N1s spectrum: 400.5eV, 399.2eV, and 398.2eV. The characteristic peak near 400.5eV is the graphite-N bond, the characteristic peak near 399.2eV is the Mn-N bond, and the characteristic peak near 398.2eV is the pyridine-N bond.

[0091] Comparative Example 3

[0092] (I) Preparation of bamboo fiber porous carbon nitrogen grafted manganese oxide composite electrode material, including the following steps:

[0093] S1: Put 10g of bamboo fiber into a corundum boat, place the boat in a tubular furnace, heat to 500℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min, keep warm for 2h for carbonization treatment, cool naturally to room temperature after the reaction is completed, and take out the bamboo fiber charcoal.

[0094] S2: Grind and mix 2g of the above-mentioned bamboo fiber carbon and 6g of activator KHCO3, then put them into a corundum boat, place the boat in a tubular furnace, and heat to 900℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min. Keep warm for 2h for activation treatment. After the reaction is completed, cool naturally to room temperature, take out and wash with 2mol / L hydrochloric acid and deionized water in turn until neutral, and then dry the bamboo fiber porous carbon.

[0095] S3: Take 2 g of the above-mentioned bamboo fiber porous carbon and add it into 80 mL of concentrated acid solution, in which the ratio of concentrated sulfuric acid to concentrated hydrochloric acid is 3:1; stir magnetically at room temperature for 6 hours, filter, wash with deionized water until neutral, and dry to obtain surface-modified bamboo fiber porous carbon.

[0096] S4: Take 2g, 2g, and 1g of KMnO4, MnSO4, and K2SO4, add them into 80ml water, stir and mix thoroughly, then put them into a 100ml polytetrafluoroethylene-lined reactor, place the reactor in a muffle furnace and calcine at 160℃ for 12h. After the reaction is completed, cool it naturally to room temperature, take it out, wash it with water, and dry it to obtain δ-MnO2.

[0097] S5: Pour the above δ-MnO2 into a corundum boat, place the boat in a tubular furnace, heat to 300℃ at a heating rate of 5℃ / min under a N2 purge flow rate of 0.2mL / min, and keep warm for 1h. After the reaction is completed, naturally cool to room temperature, take out, and obtain oxygen-deficient δ-MnO2.

[0098] S6: Prepare 0.25 mol / L urea solution, take 1g of the surface-modified bamboo fiber porous carbon in the above step (S3) and 1g of the oxygen-deficient δ-MnO2 in step (S5), add them to the urea solution, ultrasonicate and stir thoroughly, put the mixed solution into a 50ml polytetrafluoroethylene-lined reactor, place the reactor in a muffle furnace and react at 140°C for 6h. After the reaction is completed, naturally cool to room temperature, take out and wash, and obtain a bamboo fiber porous carbon nitrogen grafted manganese oxide composite electrode material, recorded as CF-N-MnO2.

[0099] Application Example 3

[0100] The preparation of zinc ion hybrid capacitor includes the following steps:

[0101] 1. The above-mentioned bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material (PC-N-MnO2) / bamboo fiber porous carbon-nitrogen grafted manganese oxide composite electrode material (CF-N-MnO2) were mixed with acetylene black and polyvinylidene fluoride binder in a mass ratio of 8:1:1, and an appropriate amount of NMP solution was added dropwise, and the slurry was completely stirred to form a slurry, which was then coated on a carbon cloth as the positive electrode of a zinc ion hybrid capacitor;

[0102] 2. Prepare 2 mol / L / L zinc sulfate aqueous solution as the electrolyte of zinc ion hybrid capacitor;

[0103] 3. Assemble the zinc ion hybrid capacitor in the order of zinc metal negative electrode, cellulose diaphragm (add zinc sulfate electrolyte), and composite electrode material positive electrode. Based on the mass calculation of the positive electrode material, the maximum specific capacity of PC-N-MnO2 and CF-N-MnO2 at a current density of 0.2A / g is 248.3mAh / g and 168.9mAh / g, respectively. After 10,000 cycles at a current density of 8.8A / g, the capacity retention rate of PC-N-MnO2 is 88.1%.

[0104] Figure 6 This is a graph showing the specific capacity of the porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells prepared in Example 4 as a zinc ion hybrid capacitor. Figure 7 This is the cycle performance curve of the manganese oxide bamboo thin-walled cell porous carbon composite electrode material prepared in Example 2 as a zinc ion hybrid capacitor. Figure 8 This is the cycle performance curve of the porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells prepared in Example 4 as a zinc ion hybrid capacitor.

[0105] Example 5

[0106] (I) Preparation of bamboo parenchyma cell / urea-formaldehyde resin composite electrode materials

[0107] S1: 10 g of bamboo parenchyma cells and 10 g of urea-formaldehyde resin were stirred and mixed in a beaker for 1 h, and the mixed powder was pressed into a round cake shape with a diameter of 2 cm using a mold.

[0108] S2: Place the round cake-shaped mixed raw materials in a tubular furnace, heat to 500°C at a heating rate of 5°C / min and keep warm for 2 hours under the condition of N2 purge flow rate of 0.2mL / min for carbonization. After the reaction is completed, naturally cool to room temperature and take out the nitrogen-doped bamboo parenchyma cell carbonized material.

[0109] S3: Grind and mix 2g of the above carbonized material and 6g of activator KHCO3 and place them in a tubular furnace. Under the condition of N2 purge flow rate of 0.2mL / min, heat to 900℃ at a heating rate of 5℃ / min and keep warm for 2h for activation. After the reaction is completed, naturally cool to room temperature and take out. After acid washing, water washing and drying, nitrogen-doped bamboo parenchyma cell porous carbon is obtained, which is marked as PC-UF-900.

[0110] Comparative Example 4

[0111] (II) Preparation of bamboo fiber / urea-formaldehyde resin composite electrode materials

[0112] S1: 10 g of bamboo fiber and 10 g of urea-formaldehyde resin were stirred and mixed in a beaker for 1 h, and the mixed powder was pressed into a round cake shape with a diameter of 2 cm using a mold.

[0113] S2: Place the round cake-shaped mixed raw materials in a tubular furnace, heat to 500°C at a heating rate of 5°C / min and keep warm for 2 hours under the condition of N2 purge flow rate of 0.2mL / min for carbonization. After the reaction is completed, naturally cool to room temperature and take out the nitrogen-doped bamboo fiber carbonized material.

[0114] S3: Grind and mix 2g of the above carbonized material with 6g of activator KHCO3 and place them in a tubular furnace. Under the condition of N2 purge flow rate of 0.2mL / min, heat to 900℃ at a heating rate of 5℃ / min and keep warm for 2h for activation. After the reaction is completed, naturally cool to room temperature and take out. After acid washing, water washing and drying, nitrogen-doped bamboo fiber porous carbon is obtained, marked as CF-UF-900. After testing, the specific surface area of ​​PC-UF-900 is 1998m2 / g, the microporosity is 71%, the mesoporosity is 22%, and the tap density is 0.285g / cm3. The specific surface area of ​​CF-UF-900 is 1546m2 / g, the microporosity is 67%, the mesoporosity is 25%, and the tap density is 0.361g / cm3. The micropores rich in thin-walled cells facilitate the activator to build a more developed pore structure.

[0115] Fig. 9 The SEM spectra of PC-UF-900 and CF-UF-900 show that the urea-formaldehyde resin evenly covers the surface of the fiber and thin-walled cells after thermal decomposition. The fibers are adhered together, and the urea-formaldehyde resin aggregates on the surface to form large pits, while there are few pits in the wall layer and cavity of the thin-walled cells, showing a more uniform distribution, which shows that the thin-walled cells have unique advantages in heterogeneous bonding.

[0116] Application Example 5

[0117] The preparation of zinc ion hybrid capacitor includes the following steps:

[0118] 1. The PC-UF-900 and CF-UF-900 electrode materials prepared above were mixed with acetylene black and polyvinylidene fluoride binder in a mass ratio of 8:1:1, and an appropriate amount of NMP was added dropwise, and the slurry was completely stirred to form a slurry, which was then coated on carbon paper as the positive electrode of the zinc ion hybrid capacitor;

[0119] 2. Prepare 2 mol / L / L zinc sulfate aqueous solution as the electrolyte of zinc ion hybrid capacitor;

[0120] 3. Zinc ion hybrid capacitors were assembled in the order of zinc metal negative electrode, cellulose diaphragm (with zinc sulfate electrolyte added), and porous carbon electrode material positive electrode. Based on the mass calculation of the positive electrode material, the maximum specific capacities of PC-UF-900 and CF-UF-900 at a current density of 0.5A / g were 290mAh / g and 160mAh / g, respectively.

Claims

1. A bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material, characterized in that: The specific surface area of ​​porous carbon from bamboo parenchyma cells is 1000-1500 m 2 / g, with both micropores and mesopores, microporosity of 60-70%, mesoporosity of 20-30%, and tap density of 0.2-0.3 g / cm 3 , flake-like δ-MnO2 is anchored on the inner surface of the porous carbon cavity of bamboo parenchyma cells through CN-Mn bonds.

2. The porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells according to claim 1, characterized in that: The loading rate of MnO2 is 30-40%.

3. The porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells according to claim 1, characterized in that: The composite electrode material has the following characteristic peaks of the XPS C1s spectrum: 284.2±0.1eV, 285.7±0.1eV, and 288.0±0.1eV; the composite electrode material has the following characteristic peaks of the XPS N1s spectrum: 400.5±0.1eV, 399.2±0.1eV, and 398.2±0.1eV.

4. The method for preparing the porous carbon-nitrogen grafted manganese oxide composite electrode material of bamboo parenchyma cells according to any one of claims 1 to 3, characterized in that: The following steps are involved: (S1) placing the bamboo parenchyma cell raw material in a tubular furnace, heating it to 500-600° C. under nitrogen protection, and keeping it warm for 2-4 hours to obtain a carbonized material; (S2) grinding and mixing the carbonized material and KHCO3, placing the mixture in a tube furnace, heating the mixture to 900-1200° C. under nitrogen protection, and keeping the temperature for 2-4 hours to obtain porous bamboo parenchyma cell carbon; (S3) placing the bamboo parenchyma cell porous carbon in a mixed solution of sulfuric acid and concentrated nitric acid and stirring to obtain surface-modified bamboo parenchyma cell porous carbon; (S4) adding manganese sulfate, potassium permanganate and potassium sulfate into water, performing ultrasonication and stirring to mix, subjecting the mixed solution to a hydrothermal reaction, and washing and drying the obtained product to obtain δ-MnO2; (S5) placing δ-MnO2 in a tube furnace, under nitrogen protection, heating to 300-400°C, and keeping the temperature for 1-2 hours to obtain a product of oxygen-deficient δ-MnO; (S6) The surface-modified bamboo parenchyma cell porous carbon and oxygen-deficient δ-MnO2 are placed in a urea solution, uniformly mixed and then subjected to a hydrothermal reaction. The obtained product is washed with water and dried to obtain a bamboo parenchyma cell porous carbon nitrogen-grafted manganese oxide composite electrode material.

5. The preparation method according to claim 4, characterized in that: In steps (S1), (S2) and (S5), the heating rate is 5-20°C / min.

6. The preparation method according to claim 5, characterized in that: In step (S1), bamboo parenchyma cell raw material and polymer resin carbon source are mixed and placed in a tubular furnace, the polymer resin carbon source is selected from at least one of phenolic resin and urea-formaldehyde resin, and the mass ratio of bamboo parenchyma cell raw material to polymer resin carbon source is 1-3:1-3.

7. The preparation method according to claim 4, characterized in that: In step (S2), the mass ratio of carbonized material to KHCO3 is 1:3-5.

8. The preparation method according to claim 4, characterized in that: In step (S3), the mass ratio of concentrated sulfuric acid to concentrated nitric acid is 3-4:1, and the volume ratio of the mixed acid to the bamboo parenchyma cell porous carbon obtained in step (S2) is 30-40ml:1g.

9. The preparation method according to claim 4, characterized in that: In step (S4), the mass ratio of manganese sulfate, potassium permanganate and potassium sulfate is 1-2:1-2:1-2; the hydrothermal reaction conditions are 150-180° C. and the time is 10-20 h.

10. The preparation method according to claim 4, characterized in that: In step (S6), the urea concentration is 0.01-0.1 mol / L; the ratio of surface-modified bamboo parenchyma cell porous carbon, oxygen-rich defect δ-MnO2 and urea solution is 1-2 g: 1-2 g: 40-60 mL; the hydrothermal reaction temperature is 120-140° C., and the time is 5-8 hours.

11. A carbon electrode comprising the following raw materials: the bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material according to any one of claims 1 to 3, a conductive carbon material and a binder.

12. The carbon electrode according to claim 11, characterized in that The mass ratio of the bamboo parenchyma cell porous carbon-nitrogen grafted manganese oxide composite electrode material, the conductive carbon material and the binder is 7-9:1-2:1-2, the conductive carbon material is selected from at least one of carbon black, SuperP, acetylene black and graphene, and the binder is selected from at least one of polyvinylidene fluoride and styrene-butadiene latex.

13. The carbon electrode according to claim 11, characterized in that The raw materials for preparing the carbon electrode include an appropriate amount of solvent, which is fully ground into slurry, coated on carbon cloth, and vacuum dried to obtain the carbon electrode.

14. The carbon electrode according to claim 13, characterized in that The solvent is N-methylpyrrolidone.