Lithium manganate with core-shell structure and preparation method and use thereof

By designing the core-shell structure of spinel-like lithium manganate as the core and layered lithium cobalt oxide as the shell, the problem of poor rate performance of lithium manganate material is solved, the effect of high capacity and high rate is achieved, and the effect of high capacity and high rate is enhanced. The conductivity and stability of the material.

CN118486816BActive Publication Date: 2024-11-15JIANGMEN KANHOO IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410943428.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-15
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The current lithium manganate materials have poor rate performance, and the traditional surface modification methods are not effective, so they cannot effectively improve their capacity and rate performance.

Method used

Using the core-shell structure design, spinel-like lithium manganese oxide is used as the core and layered lithium cobalt oxide is used as the shell. The layered lithium cobalt oxide is coated to the surface of spinel-like lithium manganese oxide by a specific preparation method to form Composite material.

Benefits of technology

The capacity and rate performance of lithium manganate material are improved, while the conductivity and structural stability of the material are enhanced, the discompatibility with the electrolyte is reduced, and the occurrence of side reactions is reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of new energy technology, and discloses a lithium manganate with a core-shell structure, wherein the lithium manganate with the core-shell structure comprises a core structure of spinel-like lithium manganate and a shell structure of layered lithium cobalt oxide. The lithium manganate with the core-shell structure is obtained by coating the layered lithium cobalt oxide on the surface of the spinel-like lithium manganate. The lithium manganate with the core-shell structure disclosed in the present application has two structures, spinel and layered. The lithium cobalt oxide coated on the outer layer can also provide capacity, thereby improving the rate performance of the material and also improving the capacity of the lithium manganate. In addition, the present application also discloses a preparation method and use of the lithium manganate with the core-shell structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy technology, and in particular to a lithium manganate with a core-shell structure and a preparation method and use thereof. Background Art

[0002] With the continuous advancement of science and technology, the technology of 3C digital batteries is also constantly innovating. For example, fast charging technology has also continuously improved the requirements for the rate performance of lithium-ion positive electrode materials. There are three main types of rate-type commercial lithium-ion positive electrode materials: lithium cobalt oxide, nickel cobalt manganese oxide, and lithium manganese oxide. The performance of the three materials is different. Lithium cobalt oxide has a layered structure, high platform voltage, high volume energy density, good storage performance, and small battery deformation. It is most suitable for mobile phone batteries and tablets; nickel cobalt manganese oxide has a layered ternary structure, high capacity, good storage performance, low platform voltage, and easy gas production to cause battery deformation. The three transition metals in the rate-type nickel cobalt manganese material are mainly cobalt. Lithium manganese oxide material has a spinel structure, low energy density, high platform voltage, good rate, but poor storage performance. Lithium manganese oxide has poor interface properties. After long-term storage, manganese (+3 / +4) at the interface of lithium manganese oxide oxidizes the electrolyte, causing the electrolyte to decompose, producing a large amount of organic byproducts, greatly increasing impedance, and significantly reducing rate performance. In order to reduce the incompatibility between lithium manganese oxide and electrolyte, conventional lithium manganese oxide is surface modified with a large amount of additives to reduce the direct contact between lithium manganese oxide and electrolyte, thereby reducing side reactions. However, the ordinary modification and coating effect is poor and the optimization effect is limited. Moreover, the modified coating layer is mostly an inert layer, which has an inhibitory effect on the performance of lithium manganese oxide itself.

[0003] The rate performance of the material is determined by the speed of lithium ion migration. In the layered structure, lithium cobalt oxide has the best ion conductivity, and lithium insertion and removal is smoother; lithium manganese oxide has poor ion conductivity, but good rate performance. The reason is that the spinel structure is a three-dimensional channel for lithium removal, which greatly improves the speed of lithium insertion and removal compared to the two-dimensional channel of the layered structure.

[0004] Prior art 1: Chinese patent 201710277649.1 discloses a core-shell heterogeneous lithium-ion battery composite positive electrode material composed of a layered lithium-rich manganese base and spinel lithium manganese oxide and a preparation method thereof. The lithium-ion composite positive electrode material has spinel lithium manganese oxide LiMn2O4 as the core, a layered lithium-rich manganese base xLi2MnO3·(1-x)LiMO2(0 <x≤1,M=Mn a Ni b Co 1-a-b, 0

[0005] However, observing the structure of the positive electrode material produced by this scheme, it can be seen that its core is spinel lithium manganese oxide and its shell is a layered lithium-rich manganese-based material.

[0006] Prior art 2: Chinese patent 201811148634.6 discloses a method for preparing a low-cobalt doped spinel-layered structure lithium nickel manganese oxide two-phase composite positive electrode material. This preparation method comprises the following steps: 1) using nickel salt and manganese salt to prepare a spinel structure nickel manganese precursor and a layered structure nickel manganese precursor respectively; 2) mixing the spinel structure nickel manganese precursor, the layered structure nickel manganese precursor, the lithium source and the cobalt source evenly, and then calcining to obtain a composite positive electrode material. This scheme uses the spinel phase to enhance the stability of the layered structure, and in turn the low Li+ migration activation barrier of the layered structure lithium nickel manganese oxide gives the composite material the possibility of high rate performance. The small amount of cobalt incorporated into the composite material can partially enter the transition metal layer, which can inhibit the Ni / Li mixing and enhance the conductivity of the composite material.

[0007] The problem that this solution needs to solve is: how to provide a lithium manganese oxide material with high capacity and high rate. Summary of the invention

[0008] The purpose of the present application is to provide a lithium manganese oxide with a core-shell structure. The present application changes the normal structure of lithium manganese oxide with only spinel, and coats a layered lithium cobalt oxide material on the outer layer to form an inner spinel and outer layered composite lithium manganese oxide material, which has the advantages of high capacity, high rate, etc.

[0009] Unless otherwise specified in this application: nM represents nanomole / liter, μM represents micromole / liter, mM represents millimole / liter, and M represents mole / liter;

[0010] To achieve the above objectives, the present application discloses a lithium manganate with a core-shell structure, wherein the lithium manganate with a core-shell structure comprises a spinel-like lithium manganate core structure and a layered lithium cobaltate shell structure.

[0011] In addition, the present application also discloses a method for preparing the above-mentioned core-shell structured lithium manganese oxide, wherein the method for preparing the core-shell structured lithium manganese oxide is to coat layered lithium cobalt oxide on the surface of spinel-like lithium manganese oxide.

[0012] ​Preferably, the method comprises the following steps:

[0013] Step 1: Mix and disperse the lithium source and the manganese source, burn and crush them once to obtain spinel-like lithium manganate;

[0014] Step 2: Mix and dissolve an alkaline compound containing lithium and a compound containing cobalt to obtain an alkaline mixed solution;

[0015] Step 3: putting the spinel lithium manganate obtained in step 1 into a solution containing ammonium radicals, heating and ammoniation, to obtain aminated spinel lithium manganate;

[0016] Step 4: adding the aminated spinel lithium manganese oxide obtained in step 3 into the alkaline mixed solution obtained in step 2 to react for 3 to 8 hours, followed by centrifugation, secondary calcination, and crushing to obtain lithium manganese oxide with a core-shell structure.

[0017] Preferably, the step 1 is specifically as follows: mixing and dispersing a lithium source and a manganese source according to a molar ratio of lithium element to manganese element of 0.51 to 0.55:1, then calcining at a temperature of 700 to 900° C. for 4 to 12 hours and crushing to obtain spinel-like lithium manganate;

[0018] The median particle size of the spinel lithium manganate is 5 to 7 μm.

[0019] Preferably, step 2 is specifically as follows: mixing and dissolving an alkaline compound containing lithium element and a compound containing cobalt element according to a molar ratio of lithium element to cobalt element of 1.03 to 1.06:1 to obtain an alkaline mixed solution, and the total concentration of the alkaline compound containing lithium element and the compound containing cobalt element in the alkaline mixed solution is 0.5 to 2 mol / L.

[0020] Preferably, the step 3 specifically comprises: adding the spinel lithium manganate obtained in step 1 into a solution containing ammonium radicals and reacting at a temperature of 70 to 150° C. for 3 to 8 hours to obtain aminated spinel lithium manganate;

[0021] The concentration of ammonium in the solution containing ammonium is 0.5 to 5 mol / L.

[0022] Preferably, the step 4 is specifically as follows: adding the aminated spinel lithium manganate obtained in step 3 into the alkaline mixed solution obtained in step 2 to react at a temperature of 70 to 150° C. for 3 to 8 hours, then centrifuging and secondary calcining at a temperature of 700 to 900° C. for 4 to 12 hours, and crushing to obtain lithium manganate with a core-shell structure;

[0023] The median particle size of the core-shell structured lithium manganese oxide is 5 to 7 μm.

[0024] Preferably, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate;

[0025] The manganese source is selected from at least one of manganese tetraoxide, manganese dioxide, manganese trioxide, manganese sulfate, and manganese carbonate;

[0026] The alkaline compound containing lithium is selected from at least one of lithium carbonate and lithium hydroxide;

[0027] The compound containing cobalt is selected from at least one of cobalt sulfate, cobalt nitrate and cobalt carbonate.

[0028] Preferably, the solution containing ammonium radicals is an aqueous ammonia solution and / or an ammonium carbonate solution.

[0029] In addition, the present application also discloses a lithium-ion battery, which contains a positive electrode with the above-mentioned core-shell structured lithium manganese oxide as an active material.

[0030] The beneficial effects of the present application are: the internal structure of the spinel structured lithium manganese oxide is stable, but the interface is unstable. The interface and the electrolyte are not compatible, and various side reactions are likely to occur. The internal structure of the layered structured lithium cobalt oxide is unstable, but the interface can form a positive electrode SEI film, which can effectively protect the direct contact between the positive electrode material and the electrolyte and reduce the erosion effect. At the same time, the interface energy of lithium cobalt oxide is low, and it is not easy to oxidize the electrolyte.

[0031] In addition, the present application changes the traditional single spinel structure of lithium manganese oxide, and prepares a core-shell composite structure with spinel lithium manganese oxide as the core and layered lithium cobalt oxide as the shell. The lithium manganese oxide as the core is a spinel structure with a stable internal structure. The lithium cobalt oxide as the shell is a layered structure, which can form a SEI film of the positive electrode and effectively protect the internal core. Traditional doping and coating are based on the spinel lithium manganese oxide structure, and the main body provides capacity. The solid doping and coating material will not provide any capacity. However, after doping or coating, some metal oxides of the additives replace the Mn position or the Li position, resulting in an increase in the average valence state of Mn and a decrease in capacity. The present application has two structures, spinel and layered. The coated outer layer of lithium cobalt oxide can also provide capacity, which improves the rate performance of the material while also improving the capacity of the lithium manganese oxide. DETAILED DESCRIPTION

[0032] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0033] Example 1

[0034] Step 1: lithium carbonate and manganese tetraoxide are mixed and dispersed according to a molar ratio of lithium element to manganese element of 0.51:1, and then calcined at 700°C for 12 hours and crushed to obtain spinel lithium manganate with a median particle size of 5 μm;

[0035] Step 2: mixing lithium carbonate and cobalt sulfate in water at a molar ratio of lithium to cobalt of 1.03:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and cobalt sulfate in the alkaline mixed solution is 0.5 mol / L;

[0036] Step 3: adding the spinel lithium manganate obtained in step 1 into ammonia water and reacting at 70° C. for 8 hours to obtain aminated spinel lithium manganate;

[0037] The concentration of ammonium in the solution containing ammonium is 1 mol / L;

[0038] Step 4: The aminated spinel lithium manganese oxide obtained in step 3 is added to the alkaline mixed solution obtained in step 2 to react at 150° C. for 8 hours, followed by centrifugation to obtain the precipitate, and then calcined for a second time at 700° C. for 12 hours and crushed to obtain lithium manganese oxide with a core-shell structure having a median particle size of 5 μm.

[0039] Example 2

[0040] Step 1: lithium carbonate and manganese tetraoxide are mixed and dispersed according to a molar ratio of lithium element to manganese element of 0.55:1, and then calcined at 900°C for 4 hours and crushed to obtain spinel lithium manganate with a median particle size of 7 μm;

[0041] Step 2: mixing lithium carbonate and cobalt sulfate in water at a molar ratio of lithium to cobalt of 1.06:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and cobalt sulfate in the alkaline mixed solution is 2 mol / L;

[0042] Step 3: adding the spinel lithium manganese oxide obtained in step 1 into ammonia water and reacting at 150° C. for 3 h to obtain aminated spinel lithium manganese oxide;

[0043] The concentration of ammonium in the solution containing ammonium is 5 mol / L;

[0044] Step 4: The aminated spinel lithium manganese oxide obtained in step 3 is added to the alkaline mixed solution obtained in step 2 to react at 70°C for 3 hours, followed by centrifugation to obtain the precipitate, and then calcined for a second time at 900°C for 4 hours and crushed to obtain lithium manganese oxide with a core-shell structure having a median particle size of 7 μm.

[0045] Example 3

[0046] Step 1: lithium carbonate and manganese tetraoxide are mixed and dispersed according to a molar ratio of lithium element to manganese element of 0.53:1, and then calcined at 800°C for 8 hours and crushed to obtain spinel lithium manganate with a median particle size of 6 μm;

[0047] Step 2: mixing lithium carbonate and cobalt sulfate in water at a molar ratio of lithium to cobalt of 1.05:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and cobalt sulfate in the alkaline mixed solution is 1 mol / L;

[0048] Step 3: adding the spinel lithium manganate obtained in step 1 into ammonia water and reacting at 100° C. for 5 hours to obtain aminated spinel lithium manganate;

[0049] The concentration of ammonium in the solution containing ammonium is 2.5 mol / L;

[0050] Step 4: The aminated spinel lithium manganese oxide obtained in step 3 is added to the alkaline mixed solution obtained in step 2 to react at 100° C. for 5 hours, followed by centrifugation to obtain the precipitate, and secondary calcination at 800° C. for 8 hours and crushing to obtain lithium manganese oxide with a core-shell structure having a median particle size of 6 μm.

[0051] Example 4

[0052] Step 1: lithium carbonate and manganese tetraoxide are mixed and dispersed according to a molar ratio of lithium element to manganese element of 0.51:1, and then calcined at 700°C for 12 hours and crushed to obtain spinel lithium manganate with a median particle size of 5 μm;

[0053] Step 2: mixing lithium carbonate and cobalt sulfate in water at a molar ratio of lithium to cobalt of 1.03:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and cobalt sulfate in the alkaline mixed solution is 0.5 mol / L;

[0054] Step 3: adding the spinel lithium manganate obtained in step 1 into ammonia water and reacting at 70° C. for 8 hours to obtain aminated spinel lithium manganate;

[0055] The concentration of ammonium in the solution containing ammonium is 1 mol / L;

[0056] Step 4: The aminated spinel lithium manganese oxide obtained in step 3 is added to the alkaline mixed solution obtained in step 2 to react at 70°C for 3 hours, followed by centrifugation to obtain the precipitate, and then calcined for a second time at 700°C for 12 hours and crushed to obtain lithium manganese oxide with a core-shell structure having a median particle size of 5 μm.

[0057] Example 5

[0058] Step 1: lithium carbonate and manganese tetraoxide are mixed and dispersed according to a molar ratio of lithium element to manganese element of 0.51:1, and then calcined at 700°C for 12 hours and crushed to obtain spinel lithium manganate with a median particle size of 7 μm;

[0059] Step 2: mixing lithium carbonate and cobalt sulfate in water at a molar ratio of lithium to cobalt of 1.03:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and cobalt sulfate in the alkaline mixed solution is 0.5 mol / L;

[0060] Step 3: adding the spinel lithium manganate obtained in step 1 into ammonia water and reacting at 70° C. for 8 hours to obtain aminated spinel lithium manganate;

[0061] The concentration of ammonium in the solution containing ammonium is 1 mol / L;

[0062] Step 4: The aminated spinel lithium manganese oxide obtained in step 3 is added to the alkaline mixed solution obtained in step 2 to react at 150° C. for 8 hours, followed by centrifugation to obtain the precipitate, and then calcined for a second time at 700° C. for 12 hours and crushed to obtain lithium manganese oxide with a core-shell structure having a median particle size of 5 μm.

[0063] Example 6

[0064] The method is basically the same as Example 1, except that ammonium carbonate solution is used instead of ammonia water in step 3, and the concentration of ammonium ion in the ammonium carbonate solution is 1 mol / L.

[0065] Example 7

[0066] The method is basically the same as Example 1, except that step 3 specifically comprises: adding the spinel lithium manganate obtained in step 1 into a mixed solution of ammonia water and ammonium carbonate and reacting at 70° C. for 8 hours to obtain aminated spinel lithium manganate;

[0067] The concentration of ammonium ion in the mixed solution of ammonia water and ammonium carbonate is 1 mol / L, and the molar ratio of ammonia water to ammonium carbonate is 1:1.

[0068] Example 8

[0069] Step 1: lithium carbonate and manganese tetraoxide are mixed and dispersed according to a molar ratio of lithium element to manganese element of 0.51:1, and then calcined at 700°C for 12 hours and crushed to obtain spinel lithium manganate with a median particle size of 5 μm;

[0070] Step 2: mixing lithium carbonate and cobalt sulfate in water at a molar ratio of lithium to cobalt of 1.03:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and cobalt sulfate in the alkaline mixed solution is 0.5 mol / L;

[0071] Step 3: The aminated spinel lithium manganese oxide obtained in step 1 is added to the alkaline mixed solution obtained in step 2 to react at 150° C. for 8 hours, followed by centrifugation to obtain the precipitate, and then calcined for a second time at 700° C. for 12 hours and crushed to obtain lithium manganese oxide with a core-shell structure having a median particle size of 5 μm.

[0072] Example 9

[0073] The method is basically the same as Example 1, except that in step 3, the concentration of ammonium ion in the ammonia water is 0.1 mol / L.

[0074] Example 10

[0075] The method is basically the same as Example 1, except that in step 3, the concentration of ammonium ions in the ammonia water is 5.5 mol / L.

[0076] Embodiment 11

[0077] Step 1: lithium carbonate and manganese tetraoxide are mixed according to a molar ratio of lithium element to manganese element of 0.51:1, ground, and calcined at 400° C. for 3 hours to synthesize lithium manganate;

[0078] Step 2: lithium carbonate and cobalt sulfate are mixed according to a molar ratio of lithium element to cobalt element of 1.03:1, and then ground together with the lithium manganese oxide prepared in step 1 according to a mass ratio of 0.2:1, and calcined in a muffle furnace at 800° C. for 8 hours to obtain a lithium manganese oxide material having a core-shell material;

[0079] It should be noted that this mass ratio is obtained by referring to the coating mass of the spinel-like lithium manganese oxide obtained in step 1 and the lithium cobalt oxide in step 4 in Example 1;

[0080] The coating mass of lithium cobalt oxide is obtained by the following method: the difference between the mass of the lithium manganese oxide with a core-shell structure obtained in step 4 and the mass of the ammoniated spinel lithium manganese oxide obtained in step 3 is calculated to obtain the coating mass of lithium cobalt oxide, that is, the coating mass of lithium cobalt oxide = the mass of the lithium manganese oxide with a core-shell structure - the mass of the ammoniated lithium cobalt oxide (of course, the error generated by this calculation method is relatively large, but it can still reflect the coating amount of lithium cobalt oxide to a certain extent)

[0081] After calculation, the coating mass ratio of the spinel-like lithium manganese oxide obtained in step 1 of Example 1 to the lithium cobalt oxide in step 4 is about 1:0.2.

[0082] Comparative Example 1

[0083] The method is basically the same as Example 1, except that step 2 is specifically as follows: lithium carbonate and manganese sulfate are mixed and dissolved in water according to a molar ratio of lithium element to manganese element of 1.03:1 to obtain an alkaline mixed solution, and the total concentration of lithium carbonate and manganese sulfate in the alkaline mixed solution is 0.5 mol / L.

[0084] Comparative Example 2

[0085] Step 1: lithium carbonate and cobalt sulfate are mixed and dispersed according to a molar ratio of lithium element to cobalt element of 1.03:1, and then calcined at 700°C for 12 hours and crushed to obtain lithium cobalt oxide with a median particle size of 5 μm;

[0086] Step 2: mixing lithium carbonate and manganese sulfate in water at a molar ratio of lithium to manganese of 0.51:1 to obtain an alkaline mixed solution, wherein the total concentration of lithium carbonate and manganese sulfate in the alkaline mixed solution is 0.5 mol / L;

[0087] Step 3: adding the lithium cobalt oxide obtained in step 1 into ammonia water and reacting at 70° C. for 8 hours to obtain aminated lithium cobalt oxide;

[0088] The concentration of ammonium in the solution containing ammonium is 1 mol / L;

[0089] Step 4: The aminated lithium cobalt oxide obtained in step 3 is added to the alkaline mixed solution obtained in step 2 to react at 150°C for 8 hours, followed by centrifugation to obtain the precipitate, and secondary calcination at 700°C for 12 hours and crushing to obtain lithium cobalt oxide with a core-shell structure having a median particle size of 5 μm.

[0090] Comparative Example 3

[0091] Step 1: lithium carbonate and manganese tetraoxide are mixed according to a molar ratio of lithium element to manganese element of 0.51:1, ground, and calcined at 400° C. for 3 hours to synthesize lithium manganate;

[0092] Step 2: lithium carbonate and cobalt sulfate are mixed according to a molar ratio of lithium to cobalt of 1.03:1, ground, and calcined in a muffle furnace at 800° C. for 8 hours to obtain lithium cobalt oxide;

[0093] Step 3: mixing the lithium manganese oxide obtained in step 1 and the lithium cobalt oxide obtained in step 2 in a mass ratio of 1:0.2, and grinding to obtain a composite material of lithium manganese oxide and lithium cobalt oxide;

[0094] It should be noted that this mass ratio is obtained by referring to the coating mass of the spinel-like lithium manganese oxide obtained in step 1 and the lithium cobalt oxide in step 4 in Example 1;

[0095] The coating mass of lithium cobalt oxide is obtained by the following method: the difference between the mass of the lithium manganese oxide with a core-shell structure obtained in step 4 and the mass of the ammoniated spinel lithium manganese oxide obtained in step 3 is calculated to obtain the coating mass of lithium cobalt oxide, that is, the coating mass of lithium cobalt oxide = the mass of the lithium manganese oxide with a core-shell structure - the mass of the ammoniated lithium cobalt oxide (of course, the error generated by this calculation method is relatively large, but it can still reflect the coating amount of lithium cobalt oxide to a certain extent)

[0096] After calculation, the coating mass ratio of the spinel-like lithium manganese oxide obtained in step 1 of Example 1 to the lithium cobalt oxide in step 4 is about 1:0.2.

[0097] Comparative Example 4

[0098] The method is basically the same as Example 1, except that a nickel-cobalt-manganese ternary precursor is used to replace the manganese tetraoxide in step 1, and the molar ratio of the lithium element to the sum of the nickel-cobalt-manganese elements is 1.03:1.

[0099] Comparative Example 5

[0100] Lithium carbonate and manganese tetraoxide were mixed and dispersed in a molar ratio of lithium to manganese of 0.51:1, and then calcined at 700°C for 12 hours and crushed to obtain spinel lithium manganate with a median particle size of 5 μm.

[0101] Comparative Example 6

[0102] Lithium carbonate and nickel-cobalt-manganese precursor were mixed and dispersed at a molar ratio of lithium to manganese of 1.03:1, and then calcined at 700°C for 12 hours and crushed to obtain lithium nickel-cobalt-manganese oxide with a median particle size of 5 μm.

[0103] Comparative Example 7

[0104] Lithium carbonate and cobalt oxide were mixed and dispersed in a molar ratio of lithium element to cobalt element of 1.03:1, and then calcined at 700°C for 12 hours and crushed to obtain lithium cobalt oxide with a median particle size of 5 μm.

[0105] Performance Test:

[0106] The positive electrode materials prepared in the examples and comparative examples were used to prepare the buckle test capacity and rate performance. The preparation process of the buckle is pulping, coating, drying, cutting, rolling, punching, and assembling the buckle. According to the formula of positive electrode material, conductive carbon, PVNF, and NMP solution of 14.1g, 0.45g, 0.45g, and 15mL, pulping was carried out, and then after coating, drying, cutting, rolling, punching, and assembling the buckle, the capacity and rate of 1C, 8C, and 15C were evaluated.

[0107] The capacity test results are shown in Table 1:

[0108] Table 1

[0109] Group 1C (mAh / g) 8C (mAh / g) 15C (mAh / g) Example 1 135.5 130.4 125.3 Example 2 120.9 115.3 109.6 Example 3 132.6 129.8 125.5 Example 4 136.4 133.6 130.8 Example 5 135.5 132.0 127.9 Example 6 135.1 130.7 124.8 Example 7 136.0 131.8 127.8 Example 8 120.3 112.9 105.5 Example 9 124.8 117.4 111.1 Example 10 128.6 129.0 125.7 Embodiment 11 133.9 127.5 123.0 Comparative Example 1 135.3 130.2 125.0 Comparative Example 2 154.9 145.8 135.3 Comparative Example 3 134.6 128.5 123.9 Comparative Example 4 155.2 139.0 123.6 Comparative Example 5 122.6 113.0 103.7 Comparative Example 6 160.3 148.0 135.7 Comparative Example 7 155.6 146.9 136.1

[0110] The magnification test results are shown in Table 2:

[0111] Table 2

[0112] Group 1C / 1C ratio (%) 8C / 1C ratio (%) 15C / 1C rate (%) Example 1 100.00 96.24 92.47 Example 2 100.00 95.37 90.65 Example 3 100.00 97.89 94.65 Example 4 100.00 97.95 95.87 Example 5 100.00 97.42 94.39 Example 6 100.00 96.13 92.16 Example 7 100.00 96.91 93.97 Example 8 100.00 93.85 87.70 Example 9 100.00 94.51 89.09 Example 10 100.00 93.97 88.15 Embodiment 11 100.00 93.82 87.56 Comparative Example 1 100.00 94.10 87.28 Comparative Example 2 100.00 94.13 87.35 Comparative Example 3 100.00 93.58 87.09 Comparative Example 4 100.00 89.56 79.64 Comparative Example 5 100.00 92.17 84.58 Comparative Example 6 100.00 92.33 84.65 Comparative Example 7 100.00 94.52 86.97

[0113] Results Analysis

[0114] Referring to Table 1-2, it can be seen from Examples 1-3 that although only small changes are made to the relevant parameters in the preparation process between Examples 1-3, it can be seen from Table 1 that there is still a certain degree of difference in capacity between Examples 1-3. We believe that the reason for this phenomenon may be the difference in particle size of lithium manganese oxide in the core structure between Examples 1-3.

[0115] Further observation of Table 2 shows that the rate performance is less affected by the particle size of lithium manganate, but the rate performance of Example 13 still fluctuates to a certain extent, which may be affected by the reaction temperature and time of adding the aminated spinel lithium manganate into the alkaline mixed solution obtained in step 2 during the coating process;

[0116] Further observation of Examples 1-2 and 4-5 shows that when the lithium manganate particle sizes of Example 1 and Example 4 are the same, and the lithium manganate particle sizes of Example 2 and Example 5 are the same, the capacity and rate performance of Examples 4 and 5 are improved relative to those of Examples 1 and 2. It is speculated that the reason for this phenomenon may be that Example 1 increases the temperature and time of the coating process in step 4 on the basis of small-particle lithium manganate, making the coating layer too thick, while Example 2 is the opposite, making the coating layer too thin, and the coating layers of Examples 4 and 5 are relatively more moderate, so the electrochemical performance is more excellent;

[0117] It can be seen from Example 1 and Examples 6-7 that when Example 7 uses a mixed solution of ammonia water and ammonium carbonate, the capacity and rate performance of the positive electrode material are better. It is speculated that the reason for this phenomenon may be that the mixed solution of Example 7 has a better amination effect on lithium manganate, thereby improving the binding force between the coating layer and lithium manganate, thereby improving the electrochemical performance of the positive electrode material;

[0118] It can be seen from Examples 1 and 8 that when lithium manganate is not subjected to ammoniation treatment, its capacity and rate performance are both reduced. The reason may be that the coating layer of lithium cobalt oxide has too weak binding force, resulting in the shedding of the coating layer. In Examples 9 and 10, when the concentration of ammonium radicals in water fluctuates greatly, the ammoniation effect of lithium manganate also fluctuates, thereby affecting the binding force of the coating layer and causing the electrochemical performance of Examples 9 and 10 to fluctuate.

[0119] It can be seen from Example 11 that when the preparation method of Example 11 is used, the ratio of the lithium manganese oxide of the core-shell structure is also significantly reduced relative to that of Example 1. It can be seen that the electrochemical performance of the lithium manganese oxide of the core-shell material prepared by this preparation method is poor.

[0120] It can be seen from Example 1 and Comparative Example 1 that when the coating layer of lithium cobalt oxide is replaced with lithium manganate, the rate performance of Comparative Example 1 has a significant decrease. It can be seen that the effect of lithium manganate coating lithium manganate is far less than that of lithium cobalt oxide coating lithium manganate.

[0121] It can be seen from the observation of Example 1 and Comparative Example 2 that the capacity of Comparative Example 2 has a significant advantage over that of Example 1. It is speculated that this is determined by the core material of Comparative Example 2, lithium cobalt oxide. Therefore, further observation of Comparative Example 7 shows that the lithium cobalt oxide without coating treatment does have good capacity performance, but after coating, Comparative Example 2 does not show a significant improvement;

[0122] By observing Example 1 and Comparative Examples 4-6 at the same time, it can be seen that only when lithium cobalt oxide is used to coat lithium manganese oxide, a significant improvement effect on the capacity and rate is produced.

[0123] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing lithium manganese oxide with a core-shell structure, characterized in that: The following steps are involved: Step 1: Mix and disperse the lithium source and the manganese source, burn and crush them once to obtain spinel-like lithium manganate; Step 2: Mix and dissolve an alkaline compound containing lithium and a compound containing cobalt to obtain an alkaline mixed solution; Step 3: adding the aminated spinel lithium manganate obtained in step 3 to the alkaline mixed solution obtained in step 2 to react at a temperature of 70 to 150° C. for 3 to 8 hours, then centrifuging and secondary calcining at a temperature of 700 to 900° C. for 4 to 12 hours, and crushing to obtain lithium manganate with a core-shell structure; Step 4: adding the aminated spinel lithium manganese oxide obtained in step 3 into the alkaline mixed solution obtained in step 2 to react for 3 to 8 hours, followed by centrifugation, secondary calcination, and crushing to obtain lithium manganese oxide with a core-shell structure; The concentration of ammonium in the solution containing ammonium is 0.5-5 mol / L; The median particle size of the core-shell structured lithium manganese oxide is 5 to 7 μm.

2. The method for preparing the core-shell lithium manganate according to claim 1, characterized in that: The step 1 specifically comprises: mixing and dispersing a lithium source and a manganese source according to a molar ratio of lithium element to manganese element of 0.51 to 0.55:1, and then calcining at a temperature of 700 to 900° C. for 4 to 12 hours and crushing to obtain spinel-like lithium manganate; The median particle size of the spinel lithium manganate is 5 to 7 μm.

3. The method for preparing the core-shell lithium manganate according to claim 1, characterized in that: The step 2 is specifically as follows: mixing and dissolving an alkaline compound containing lithium and a compound containing cobalt at a molar ratio of lithium to cobalt of 1.03 to 1.06:1 to obtain an alkaline mixed solution, wherein the total concentration of the alkaline compound containing lithium and the compound containing cobalt in the alkaline mixed solution is 0.5 to 2 mol / L.

4. The method for preparing the core-shell lithium manganate according to claim 1, characterized in that: The step 3 specifically comprises: putting the spinel lithium manganate obtained in step 1 into a solution containing ammonium radicals and reacting at a temperature of 70 to 150° C. for 3 to 8 hours to obtain aminated spinel lithium manganate; The concentration of ammonium in the solution containing ammonium is 0.5 to 5 mol / L.

5. The method for preparing the core-shell lithium manganate according to claim 1, characterized in that: The lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate; The manganese source is selected from at least one of manganese tetraoxide, manganese dioxide, manganese trioxide, manganese sulfate, and manganese carbonate; The alkaline compound containing lithium is selected from at least one of lithium carbonate and lithium hydroxide; The compound containing cobalt is selected from at least one of cobalt sulfate, cobalt nitrate and cobalt carbonate.

6. The method for preparing the core-shell lithium manganate according to claim 1, characterized in that: The solution containing ammonium ions is an ammonia solution and an ammonium carbonate solution, the concentration of ammonium ions in the mixed solution of ammonia water and ammonium carbonate is 1 mol / L, and the molar ratio of ammonia water to ammonium carbonate is 1:

1.

7. A lithium ion battery, characterized in that: A positive electrode containing lithium manganese oxide with a core-shell structure prepared by the method for preparing lithium manganese oxide with a core-shell structure according to any one of claims 1 to 6, and containing the lithium manganese oxide with a core-shell structure as an active material.