A lithium battery positive electrode material, preparation method and application thereof

By preparing lithium battery positive electrode material with core-shell structure and doped elements, the problem of ternary positive electrode material prone to internal cracks during circulation is solved, the crack resistance strength and cycle stability are improved, and the service life of the material is extended.

CN118486821BActive Publication Date: 2024-11-08GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410910299.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-08
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing ternary positive electrode materials are prone to internal cracks during the circulation process, resulting in a decrease in battery capacity and failure. The dense arrangement of secondary particles increases the difficulty of synthesis and internal stress, affecting the circulation stability and life of the material.

Method used

The general formula of lithium battery positive electrode material is LixNiaCobMcM'1-a-b-cAyO2-y, and the precursor core and shell with core-shell structure are prepared through co-precipitation reaction. Combined with doping elements, the strength of unit cells and grain boundaries is controlled, and the resistance is improved. crack strength and introduce crack resistance through specific calcining conditions and reinforcement additives.

Benefits of technology

It improves the crack resistance strength and cycle stability of the material, inhibits the spread of internal cracks to the interface, extends the service life of the material, and reduces the difficulty of synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118486821B_ABST
    Figure CN118486821B_ABST
Patent Text Reader

Abstract

The present invention discloses a lithium battery positive electrode material, a preparation method and application thereof, and relates to the technical field of lithium batteries. The ability of a polycrystalline positive electrode material to resist the generation of internal cracks during a cycle is evaluated by crack resistance, and a lithium battery positive electrode material is provided, wherein the crack resistance of the lithium battery positive electrode material meets a specific range, has high-strength crystals and grain boundaries, can improve the structural stability of the material, effectively inhibit the diffusion of internal cracks to the interface, and thus improve the cycle stability and life of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a lithium battery positive electrode material, a preparation method and application thereof. Background Art

[0002] The rapid development of lithium-ion batteries has led to the rapid development of ternary cathode materials, which have the advantages of high specific capacity, moderate price, low toxicity and relatively abundant resources. However, ternary materials also have many problems, especially nickel-rich ternary materials, which have poor battery cycle performance, multi-level phase transitions during charge and discharge, and large volume changes during charge and discharge, which easily cause residual stress and lead to mechanical fracture.

[0003] In order to increase the tap density of ternary materials and suppress the occurrence of surface side reactions, the ternary materials are prepared into secondary particles composed of densely packed primary particles, which greatly reduces the contact between the primary particles and the electrolyte, thereby reducing the occurrence of interface side reactions. However, secondary particles still bring new problems: first, secondary particles require a very dense arrangement of primary particles, especially a dense interface, which can effectively block the contact between the internal primary particles and the electrolyte. This dense secondary particle greatly increases the difficulty of synthesis; in addition, the expansion and contraction of the volume of secondary particles during the charge and discharge process will cause an increase in internal stress, and long-term cycles will cause these stresses to gradually accumulate, gradually leading to microcracks inside and on the surface of the secondary particles, and eventually causing the entire secondary particle to rupture.

[0004] The mechanical fracture of ternary cathode materials goes through the following development process: During the charging process, as Li + The interlayer spacing of the ternary material will gradually increase due to the release of Li + After the release, the electrostatic repulsion between the layers increases. When the high-delithiation state is reached, the interlayer spacing will shrink. The reason for the shrinkage may be the transition of Li + Structural slip caused by O escaping from the interlayer; it may also be that O participates in the redox reaction, resulting in a decrease in interlayer electrostatic repulsion and a decrease in interlayer spacing. During the discharge process, the change in interlayer spacing is completely opposite to that during the charging process. During a charge and discharge process, the layered material undergoes four expansions and contractions, and residual stress is inevitably generated in the volume change. The accumulation of residual stress causes microcracks in the grain boundaries between the particles, thereby increasing the contact with the electrolyte, aggravating the interface side reaction, and further aggravating the expansion of microcracks, and ultimately leading to the rupture of the particles, resulting in a decrease in battery capacity or even failure. It can be seen that the final rupture of the polycrystalline ternary positive electrode material particles is related to the unit cell deformation and grain boundary failure of the ternary positive electrode material. Unit cells and grain boundaries jointly affect whether the positive electrode material is prone to cracks during use. It is of great significance to provide positive electrode materials with both high-strength crystals and grain boundaries.

[0005] Therefore, there is an urgent need to provide positive electrode materials that have both high-strength crystals and grain boundaries, so as to improve the material's ability to resist internal cracks during the cycle process, thereby improving the material's cycle stability and life.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The purpose of the present invention is to provide a lithium battery positive electrode material, a preparation method and application thereof, aiming to improve the material's ability to resist the generation of internal cracks during the cycle process, thereby improving the material's cycle stability and life.

[0008] The present invention is achieved in that:

[0009] In a first aspect, the present invention provides a lithium battery positive electrode material, wherein the cracking strength of the lithium battery positive electrode material is 4-15 MPa;

[0010] in, ;

[0011] Where, St represents the crushing strength, which is obtained through the indentation test and the unit is MPa; It represents the average crushing strength in MPa. = , n is the sample size, n≥10;

[0012] It refers to the maximum change of shear strain during the first charging process;

[0013] = - ;

[0014] It refers to the change in shear strain after 10 charge-discharge cycles, t=10;

[0015] = - , It refers to the shear strain measured in static state after 10 charge-discharge cycles. It refers to the shear strain measured in static state before the first charge;

[0016] a and c represent unit cell parameters.

[0017] In an optional embodiment, the crack strength of the lithium battery positive electrode material is 6-15 MPa;

[0018] St = 2.8 × P / (πd 2 );

[0019] P represents the maximum pressure value before the pressure drop point, in mN;

[0020] d represents the particle diameter of lithium battery positive electrode material, in μm;

[0021] The value of is 0.2-0.3, The value of is 0.01-0.20, The value is 90-140MPa;

[0022] c and a were obtained by X-ray diffractometer XRD test;

[0023] The general formula of lithium battery positive electrode material is Li x Ni a Co b M c M' 1-a-b-c A y O 2-y ;

[0024] In the general formula, M is selected from at least one of Al and Mn;

[0025] M' is at least one selected from Zr, Sr, Mo, Ba, W, B, Ti, Mg, Li, C, Si, Ca, Cu, La, Ce, Bi, In, Al, Nb and Y;

[0026] A is selected from at least one of P and F;

[0027] 0.95≤x<1.1, a>0, b>0, c>0, 0.95≤(a+b+c)≤1, 0≤y≤0.01.

[0028] In a second aspect, the present invention further provides a method for preparing a lithium battery positive electrode material, comprising: preparing a lithium battery positive electrode material that meets the requirements of crack resistance.

[0029] In an optional embodiment, the method comprises: using nickel salt, cobalt salt and M salt to perform a coprecipitation reaction to prepare a precursor core;

[0030] The precursor core is mixed with a reinforcement solution for reaction, and a reinforcement aid is introduced after calcination to obtain a reinforced precursor core; wherein the reinforcement aid is selected from at least one of LiAlO2, LiMn2O4 and LiCoPO4;

[0031] A coprecipitation reaction is carried out using nickel salt, cobalt salt, M salt and a first doping element compound, and a shell is continuously grown on the basis of a reinforced precursor core to obtain a ternary precursor having a core-shell structure; wherein the doping element contained in the first doping element compound is selected from at least one of Ti, Al, Zr and Mg;

[0032] The ternary precursor is mixed with a lithium source and calcined.

[0033] In an optional embodiment, the primary particles of the precursor core are radially arranged and have a porosity of 4%-12%;

[0034] The process for preparing the precursor core includes: preparing a base liquid in a reaction kettle, and passing a first mixed metal salt solution, a first precipitant solution, and a first complexing agent solution into the base liquid for a coprecipitation reaction. The process for preparing the precursor core satisfies at least one of the characteristics A1 to K1:

[0035] Feature A1: The reaction temperature of the coprecipitation reaction is controlled to be 75°C-95°C;

[0036] Feature B1: The reaction pH value of the coprecipitation reaction is controlled to be 10.5-11.5;

[0037] Characteristic C1: The first complexing agent solution is an ammonia solution with a mass fraction of 18%-22%, and the ammonia concentration in the reactor is controlled to be 3g / L-7g / L during the precipitation process;

[0038] Feature D1: The total metal ion molar concentration of the first mixed metal salt solution is 1.8M-2.2M, and the flow rate of the first mixed metal salt solution is 400L / h-500L / h;

[0039] Characteristic E1: After the reaction reaches a particle size D50 of 2-17 μm, the feeding is stopped;

[0040] Feature F1: After the coprecipitation reaction is completed, aging is performed, followed by alkali solution washing, water washing, and drying;

[0041] Feature G1: The molar ratio of nickel, cobalt and M in the first mixed metal salt solution is (35-98): (1-35): (1-35);

[0042] Feature H1: The first mixed metal salt solution is selected from any one of nitrate, chloride and sulfate;

[0043] Characteristic I1: The first precipitant solution is a sodium hydroxide solution with a mass fraction of 30%-34%;

[0044] Feature J1: The concentration of ammonia in the base solution is 4.5g / L-5.5g / L, and the pH value is 11.8-12.2;

[0045] Feature K1: The coprecipitation reaction is carried out under the protection of an inert atmosphere, and the rotation speed during the reaction is 400rpm-800rpm.

[0046] In an optional embodiment, the preparation process of the reinforced precursor core includes: mixing the precursor core with the reinforcement solution by ultrasonication, reacting for 10 min to 60 min at a temperature of 100° C. to 150° C. and a pressure of 10 MPa to 20 MPa, then separating the solid and the liquid, and calcining the obtained solid material;

[0047] The raw materials in the reinforcement solution are calcined to obtain reinforcement additives;

[0048] The preparation process of the reinforced precursor core satisfies at least one of features A2 to F2:

[0049] Feature A2: The strengthening solution further contains a thickener, and the viscosity of the strengthening solution is adjusted to 5 mPa·s-8 mPa·s by adjusting the amount of the thickener;

[0050] Feature B2: When feature A2 is met, the thickener is selected from at least one of carbomer, xanthan gum, gelatin and starch;

[0051] Characteristic C2: The amount of strengthening solution corresponding to 1g of precursor core is 90mL-110mL;

[0052] Feature D2: Control the ultrasonic time to 10min-60min;

[0053] Feature E2: The calcination temperature is controlled to be 600°C-700°C and the calcination time is 3h-8h;

[0054] Feature F2: The solid material is first dried at 80°C-120°C for 5h-10h and then calcined.

[0055] In an optional embodiment, the preparation process of the ternary precursor having a core-shell structure includes: adding the reinforced precursor core to the bottom liquid in the reaction kettle, passing the second mixed metal salt solution, the second precipitant solution and the second complexing agent solution into the reaction kettle for coprecipitation reaction;

[0056] The second mixed metal salt solution contains nickel salt, cobalt salt, M salt and the first doping element compound, and the addition rate of the second mixed metal salt solution is regulated so that the addition rate of nickel, cobalt and M element during the reaction is controlled to be lower than the addition rate when preparing the precursor core;

[0057] The preparation process of the ternary precursor having a core-shell structure satisfies at least one of the characteristics A3 to I3:

[0058] Feature A3: The total concentration of nickel, cobalt and M element in the second mixed metal salt solution is 1.8M-2.2M, the flow rate of the second mixed metal salt solution is 100L / h-200L / h, and the pH value of the second mixed metal salt solution is regulated to be 2-5;

[0059] Feature B3: The total molar amount of metal is calculated based on the total molar amount of nickel, cobalt and M element, and the ratio of the total molar amount of metal in the reinforcement precursor core to the total molar amount of metal in the second mixed metal salt solution is (4-12): 1;

[0060] Characteristic C3: In the second mixed metal salt solution, the molar ratio of nickel, cobalt and M element is (30-60): (20-35): (20-35);

[0061] Feature D3: The reaction temperature of the coprecipitation reaction is 75°C-95°C, and the reaction pH is 10.8-11.2;

[0062] Feature E3: The second complexing agent solution is an ammonia solution with a mass fraction of 18%-22%, and the ammonia concentration in the reactor is controlled to be 3g / L-7g / L during the precipitation process;

[0063] Feature F3: The first doping element compound is selected from at least one of titanium disulfate, sodium aluminate, zirconium nitrate, zirconium acetate, zirconium sulfate, magnesium sulfate and magnesium nitrate;

[0064] Feature G3: The bottom liquid in the reactor is water, and the second precipitant solution is a sodium hydroxide solution with a mass fraction of 30%-40%;

[0065] Characteristic H3: The coprecipitation reaction is carried out under the protection of an inert atmosphere, and the rotation speed during the reaction is 300rpm-500rpm;

[0066] Feature I3: After the second mixed metal salt solution is added, the reaction is continued for 0.5h-2.0h, and then solid-liquid separation is performed, and the obtained solid material is washed with water and dried.

[0067] In an optional embodiment, the ternary precursor, the second doping element compound and the lithium source are mixed and calcined; wherein the doping element contained in the second doping element compound is selected from at least one of Zr, Sr, Mo, Ba, W, B, Ti, Mg, Li, C, F, Si, Ca, Cu, La, P, Ce, Bi, In, Nb and Y;

[0068] The process of mixing and calcining the ternary precursor, the second doping element compound and the lithium source satisfies at least one of the features A4 to F4:

[0069] Feature A4: The molar ratio of the total amount of nickel, cobalt and M elements in the ternary precursor to the lithium content in the lithium source is 1:(1.05-1.1);

[0070] Feature B4: The lithium source is selected from lithium hydroxide;

[0071] Feature C4: The second doping element compound is selected from at least one of oxides, fluorides, carbonates, hydroxides, nitrides, borides and nitrates;

[0072] Feature D4: During the calcination process, the steel is first calcined at 400°C-500°C for 2h-6h, and then calcined at 750°C-850°C for 10h-15h.

[0073] Feature E4: calcining in an oxygen-containing atmosphere;

[0074] Feature F4: The ternary precursor, the second doping element compound and the lithium source are first mixed and ground, and then calcined.

[0075] In a third aspect, the present invention further provides a positive electrode plate, comprising the lithium battery positive electrode material in any of the above embodiments or the lithium battery positive electrode material prepared by the preparation method in any of the above embodiments.

[0076] In a fourth aspect, the present invention further provides a lithium battery, comprising the positive electrode plate in the above embodiment.

[0077] The present invention has the following beneficial effects: by constructing a calculation formula for crack resistance, the ability of a polycrystalline positive electrode material to resist the generation of internal cracks during a cycle is evaluated, and the influence of unit cells and grain boundaries is comprehensively considered so that the crack resistance meets a specific value range, the positive electrode material can have high-strength crystals and grain boundaries, the structural stability of the material can be improved, and the diffusion of internal cracks to the interface can be effectively inhibited, thereby improving the cycle stability and life of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0079] Figure 1 This is an ion cross-sectional view of the positive electrode material prepared in Example 1;

[0080] Figure 2 This is an ion cross-sectional view of the positive electrode material prepared in Comparative Example 1;

[0081] Figure 3 This is a cross-sectional view of the positive electrode material prepared in Example 1;

[0082] Figure 4 This is a cross-sectional view of the positive electrode material prepared in Comparative Example 2;

[0083] Figure 5 is the XRD pattern of the precursor core and the precursor material in Example 1;

[0084] Figure 6 TEM and EDS images of the positive electrode material prepared in Example 1; (a) represents the TEM image, and (b) represents the EDS image;

[0085] Figure 7 TEM and EDS images of the positive electrode material prepared in Example 4; (a) represents the TEM image, and (b) represents the EDS image. DETAILED DESCRIPTION

[0086] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0087] The embodiment of the present invention provides a lithium battery positive electrode material, which is a secondary particle formed by agglomeration of primary particles and belongs to a polycrystalline material. The general formula of the lithium battery positive electrode material is Li x Ni a Co b M c M' 1-a-b-c A y O 2-y .

[0088] The description of each parameter in the general formula is as follows:

[0089] M is selected from at least one of Al and Mn, and M may be any one or two of the above.

[0090] M' is selected from at least one of Zr, Sr, Mo, Ba, W, B, Ti, Mg, Li, C, Si, Ca, Cu, La, Ce, Bi, In, Al, Nb and Y, and M' can be any one or more of the above.

[0091] A is selected from at least one of P and F, and can be any one or two of the above.

[0092] x, y, a, b and c are expressed in mol, 0.95≤x<1.1, and x can specifically be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.03, 1.05, 1.08, 1.10, etc.

[0093] a>0, b>0, c>0, and 0.95≤(a+b+c)≤1, a+b+c can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, etc. When a+b+c=1, there is no M' element.

[0094] 0≤y≤0.01, the value of y can be 0.000, 0.003, 0.005, 0.008, 0.010, etc. When the value of y is 0, the positive electrode material does not contain element A.

[0095] The inventors found that the crystal strength and grain boundary strength simultaneously determine the ability of the positive electrode material to resist internal cracks during the cycle, and the relationship between them can be expressed in accordance with the following formula:

[0096] ;

[0097] Where St represents the crushing strength, which is obtained through the indentation test and is measured in MPa. The pressure calculated from the maximum pressure value corresponding to the pressure drop point during the test is used as the crushing strength of the material, St = 2.8 × P / (πd 2 ), P represents the maximum pressure value corresponding to the pressure drop point, in mN; d represents the particle diameter of the lithium battery positive electrode material, in μm;

[0098] represents the average crushing strength, = , n is the sample size, n≥10;

[0099] It refers to the maximum change in shear strain during the first charging process, reflecting the degree of immediate deformation of the material; that is:

[0100] = - ;

[0101] It refers to the change in shear strain after 10 charge-discharge cycles (i.e. t=10), reflecting the irreversible strain accumulated during the material cycle. = - , It refers to the shear strain measured in static state after 10 charge-discharge cycles. It refers to the shear strain measured in static state before the first charge;

[0102] c represents the unit cell parameter; a represents the unit cell parameter. c and a are obtained by X-ray diffractometer XRD test.

[0103] The crack strength of the lithium battery positive electrode material provided in an embodiment of the present invention is 4-15 MPa, preferably 6-15 MPa, such as 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa, 15 MPa, etc., or any value among the above adjacent values.

[0104] The value of is 0.2-0.3, such as 0.20, 0.22, 0.25, 0.28, 0.30;

[0105] The value of is 0.01-0.20, such as 0.01, 0.03, 0.05, 0.08, 0.10, 0.12, 0.15, 0.18, 0.20;

[0106] The value is 90-140 MPa, such as 90 MPa, 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa, etc.

[0107] It should be noted that the present invention provides crack resistance strength parameter indicators, which can comprehensively evaluate various factors that cause internal cracks in positive electrode materials, including the crystal structure itself and grain boundary strength. It reflects the crystal's ability to resist deformation during charging; It reflects the permanent deformation of the crystal during the cycle and reflects the irreversible phase change of the crystal. The above two factors both reflect the influence of the crystal structure itself on the generation of internal cracks. The crushing strength can reflect the strength of the grain boundary. The first crack in the polycrystalline material is the dissociation of the grain boundary (the contact surface between the primary particles) because the grain boundary has a lower bonding strength than the crystal. It has been verified through experiments that the greater the crack resistance, the smaller the rate of change of the specific surface area of ​​the material after the charge and discharge test with the same number of cycles. The specific surface area can reflect the degree of microcracks in the material. The more microcracks the material produces, the worse the cyclic stability of the material. In summary, the greater the crack resistance, the higher the cyclic stability of the material.

[0108] Unit cell deformation is an inherent property of the material, and this problem is usually improved by doping elements to improve the strength of chemical bonds; for the problem of grain boundary failure, it is usually improved by controlling the grain shape of the primary particles and the morphology after agglomeration, doping elements, etc. The inventor also provides a method for preparing a lithium battery positive electrode material, which combines the core and the shell by doping elements to make the product's crack resistance meet the requirements. The specific preparation process is as follows:

[0109] The present invention provides a method for preparing a positive electrode material for a lithium battery, comprising the following steps:

[0110] S1. Preparation of precursor core

[0111] The precursor core is prepared by coprecipitation reaction of nickel salt, cobalt salt and M salt (ie, salt containing element M in the general formula), and the M salt can be a manganese salt or an aluminum salt.

[0112] In some embodiments, the primary particles in the precursor core are radially arranged and have a porosity of 4%-12% (such as 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, etc.). The radial arrangement of the primary particles and maintaining a certain porosity are beneficial to the dissipation of stress, which is beneficial to inhibiting the formation of intercrystalline cracks during the cycle of the positive electrode material and delaying the irreversible phase transition from the layered phase to the rock salt phase, thereby improving the structural stability of the ternary positive electrode material.

[0113] In some embodiments, the preparation process of the precursor core includes: configuring a bottom liquid in a reactor, passing a first mixed metal salt solution, a first precipitant solution, and a first complexing agent solution into the bottom liquid, and performing a coprecipitation reaction under the protection of an inert atmosphere, controlling the reaction temperature of the coprecipitation reaction to be 75°C-95°C, the reaction pH value to be 10.5-11.5, the rotation speed to be 400rpm-800rpm, the particles gradually grow, and after the reaction to a particle size D50 of 2-17μm, the feeding is stopped. After the coprecipitation reaction is completed, aging is performed, followed by alkali washing, water washing, and drying in sequence, the sodium sulfur residue is washed away by alkali washing, the alkali solution residual on the surface is removed by water washing, the moisture can be removed after drying, and after drying, it can also be sieved to obtain a precursor core with a particle size that meets the requirements.

[0114] Specifically, the reaction temperature of the coprecipitation reaction can be 75°C, 80°C, 85°C, 90°C, 95°C, etc., the pH value can be 10.5, 10.8, 11.0, 11.2, 11.5, etc., and the rotation speed can be 400rpm, 500rpm, 600rpm, 700rpm, 800rpm, etc. The particle size of the product is detected during the reaction, and the particle size D50 is controlled to be 2μm, 5μm, 8μm, 10μm, 12μm, 15μm, 17μm, etc. at the end of the reaction. The inert atmosphere can be nitrogen, but is not limited thereto. Alkali washing can be washing with a hot dilute alkaline solution to effectively wash away the sodium sulfur residue.

[0115] In some embodiments, the first complexing agent solution is an ammonia solution with a mass fraction of 18%-22%, and the ammonia concentration in the reactor is controlled to be 3g / L-7g / L during the precipitation process by adjusting the addition rate of the first complexing agent solution; the first precipitant solution is a sodium hydroxide solution with a mass fraction of 30%-34%, and the pH value of the system is controlled to meet the requirements by adjusting the addition rate of the first precipitant solution. Specifically, the mass fraction of the ammonia solution can be 18%, 20%, 22%, etc., and the ammonia concentration in the reactor can be controlled to be 3g / L, 4g / L, 5g / L, 6g / L, 7g / L, etc. during the precipitation process; the mass fraction of the sodium hydroxide solution can be 30%, 31%, 32%, 33%, 34%, etc.

[0116] In some embodiments, the molar ratio of nickel, cobalt and M in the first mixed metal salt solution is (35-98): (1-35): (1-35), the total metal ion molar concentration of the first mixed metal salt solution is 1.8M-2.2M, and the flow rate of the first mixed metal salt solution is 400L / h-500L / h. By further regulating the composition, concentration and addition rate of the first mixed metal salt solution, the deposition rate can be controlled so that the precursor core presents a porous morphology.

[0117] Specifically, in the first mixed metal salt solution, the molar ratio of nickel, cobalt and M element can be 35:30:35, 40:30:30, 50:20:30, 60:20:20, 70:10:20, 80:10:10, 90:5:5, 98:1:1, etc. The total metal ion molar concentration of the first mixed metal salt solution refers to the total concentration of nickel, cobalt and M element, which can be 1.8M, 1.9M, 2.0M, 2.1M, 2.2M, etc. The flow rate of the first mixed metal salt solution can be 400L / h, 420L / h, 450L / h, 480L / h, 500L / h, etc.

[0118] Furthermore, the first mixed metal salt solution is selected from any one of nitrates, chlorides and sulfates, and can be any of the above salts, such as all nitrates, using nickel nitrate, cobalt nitrate and manganese nitrate (or aluminum nitrate) as raw materials.

[0119] In some embodiments, the bottom liquid can be prepared by using an ammonia solution and a sodium hydroxide solution, and the ammonia concentration in the bottom liquid is 4.5g / L-5.5g / L, and the pH value is 11.8-12.2 to meet the reaction conditions of coprecipitation. Specifically, the ammonia concentration in the bottom liquid can be 4.5g / L, 5.0g / L, 5.5g / L, etc., the pH value can be 11.8, 11.9, 12.0, 12.1, 12.2, etc., and the volume of the bottom liquid can account for 60%-80% of the volume of the reactor.

[0120] S2. Preparation of reinforced precursor core

[0121] The precursor core is mixed with a reinforcement solution for reaction, and a reinforcement aid is introduced after calcination to obtain a reinforced precursor core. The introduced reinforcement aid is selected from at least one of LiAlO2, LiMn2O4 and LiCoPO4, and the introduced reinforcement aid can be any one or more of the above. The grain boundaries of the primary particles of the precursor core are reinforced by a sol-gel method to strengthen the grain boundary strength of the primary particles.

[0122] In some embodiments, the preparation process of the reinforced precursor core includes: mixing the precursor core with the reinforcement solution by ultrasonication for 10-60 minutes, reacting at a temperature of 100°C-150°C and a pressure of 10MPa-20MPa for 10-60 minutes, separating the solid and the liquid after the reaction is completed, and calcining the obtained solid material. The reaction is carried out under high temperature and high pressure conditions, and the reaction liquid is pressurized by heating to vaporize the solvent to ensure that the precursor core is completely infiltrated.

[0123] Specifically, the time for ultrasonic mixing of the precursor core and the reinforcement solution can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, etc. The high temperature and high pressure reaction can be carried out in a general high pressure reactor, the reaction temperature can be controlled to be 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., the reaction pressure can be controlled to be 10 MPa, 13 MPa, 15 MPa, 18 MPa, 20 MPa, etc., and the pressure holding reaction time can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, etc.

[0124] Among them, the raw materials in the reinforcement solution can obtain the above-mentioned reinforcement aid after calcination. If the reinforcement aid is LiMn2O4, the raw materials can be manganese acetate and lithium hydroxide.

[0125] In some embodiments, the reinforcement solution also contains a thickener, and the viscosity of the reinforcement solution is 5mPa·s-8mPa·s by adjusting the amount of the thickener. A high viscosity is conducive to the reinforcement solution being retained in the pores of the precursor core and further crystallizing during the calcination process, that is, the viscosity is too low and the doping amount is also low; if the viscosity is too high, it is not easy to enter the pores, resulting in a low doping amount. The thickener is selected from at least one of carbomer, xanthan gum, gelatin and starch, and the thickener can be any one or more of the above. The amount of reinforcement solution corresponding to 1g of the precursor core is 90mL-110mL, such as 90mL, 95mL, 100mL, 105mL, 110mL.

[0126] In some embodiments, the calcination temperature is controlled to be 600°C-700°C, and the calcination time is 3h-8h. After calcination, a reinforcing agent can be introduced into the precursor core to strengthen the grain boundary strength of the primary particles. Specifically, the calcination temperature can be 600°C, 620°C, 650°C, 680°C, 700°C, etc., and the calcination time can be 3h, 4h, 5h, 6h, 7h, 8h, etc.

[0127] In some embodiments, the solid material may be dried at 80°C-120°C for 5h-10h before calcining to fully remove surface moisture before calcining. Specifically, the drying temperature may be 80°C, 90°C, 100°C, 110°C, 120°C, etc.; the drying time may be 5h, 6h, 7h, 8h, 9h, 10h, etc.

[0128] S3. Preparation of ternary precursor with core-shell structure

[0129] A coprecipitation reaction is carried out using nickel salt, cobalt salt, M salt and a first doping element compound, and an outer shell is continuously grown on the basis of a reinforced precursor core, so as to obtain a ternary precursor with a core-shell structure.

[0130] In some embodiments, the preparation process of a ternary precursor with a core-shell structure includes: adding a reinforced precursor core to the bottom liquid in a reactor, and passing a second mixed metal salt solution, a second precipitant solution, and a second complexing agent solution into the reactor for a co-precipitation reaction; wherein the second mixed metal salt solution contains nickel salt, cobalt salt, M salt, and a first doping element compound, and by regulating the addition rate of the second mixed metal salt solution, the addition rate of nickel, cobalt, and M elements during the reaction is controlled to be less than the addition rate when preparing the precursor core, and by reducing the addition rate of the second mixed metal salt solution to control the co-precipitation reaction rate, it is beneficial to obtain a denser shell.

[0131] Furthermore, in the second mixed metal salt solution, the molar ratio of nickel, cobalt and M element is (30-60): (20-35): (20-35), and a dense, low Ni content, element-doped shell is prepared, which is beneficial to reduce the contact with the electrolyte, and the element doping and the low Ni content are beneficial to improve the strength and stability of the crystal structure, improve its strain resistance, and inhibit the internal cracks from spreading to the interface. In the second mixed metal salt solution, the total concentration of nickel, cobalt and M element is 1.8M-2.2M. Before adding to the reactor, the pH value of the second mixed metal salt solution is adjusted to 2-5 by adding acid to prevent precipitation. During the precipitation process, the second mixed metal salt solution can be slowly dripped into the reactor using a peristaltic pump, and the flow rate of the second mixed metal salt solution is controlled to be 100L / h-200L / h.

[0132] Specifically, in the second mixed metal salt solution, the molar ratio of nickel, cobalt and M element can be 30:35:35, 40:30:30, 50:25:25, 60:20:20, etc. In the second mixed metal salt solution, the total concentration of nickel, cobalt and M element can be 1.8M, 1.9M, 2.0M, 2.1M, 2.2M, etc. Before adding to the reactor, the pH value of the second mixed metal salt solution can be adjusted to 3.5, 3.8, 4.0, 4.2, 4.5, etc. The flow rate of the second mixed metal salt solution can be 100L / h, 120L / h, 150L / h, 180L / h, 200L / h, etc.

[0133] Furthermore, the total molar amount of metal is calculated based on the total molar amount of nickel, cobalt and M element, and the ratio of the total molar amount of metal in the core of the reinforcement precursor to the total molar amount of metal in the second mixed metal salt solution is (4-12): 1. By regulating the amount of the core and the shell, the ratio of the core and the shell is better regulated to improve the electrochemical performance of the material. Specifically, the ratio of the total molar amount of metal in the core of the reinforcement precursor to the total molar amount of metal in the second mixed metal salt solution can be 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, etc.

[0134] Wherein, the doping element contained in the first doping element compound is selected from at least one of Ti, Al, Zr and Mg, and the doping element contained in the first doping element compound can be any one or more of the above. The first doping element compound is selected from at least one of titanium disulfate, sodium aluminate, zirconium nitrate, zirconium acetate, zirconium sulfate, magnesium sulfate and magnesium nitrate, and the first doping element compound can be any one or more of the above, and the dosage is regulated according to the doping amount of the doping element.

[0135] In some embodiments, the bottom liquid in the reactor is water, and the volume of water added to the reactor can be 15%-25% of the volume of the reactor. The second precipitant solution is a sodium hydroxide solution with a mass fraction of 30%-40%, and the pH value during the reaction is 10.8-11.2 by adjusting the addition rate of the second precipitant solution. The second complexing agent solution is an ammonia solution with a mass fraction of 18%-22%, and the ammonia concentration in the reactor is controlled to be 3g / L-7g / L during the precipitation process. Specifically, the mass fraction of the sodium hydroxide solution can be 30%, 32%, 34%, 36%, 38%, 40%, etc., and the pH value during the reaction can be 10.8, 10.9, 11.0, 11.1, 11.2, etc.; the mass fraction of the ammonia solution can be 18%, 19%, 20%, 21%, 22%, etc., and the ammonia concentration in the reactor can be controlled to be 3g / L, 4g / L, 5g / L, 6g / L, 7g / L, etc. during the precipitation process.

[0136] In some embodiments, the precipitation process can be carried out in an inert atmosphere (such as nitrogen), the reaction temperature of the coprecipitation reaction is 75°C-95°C, and the rotation speed during the reaction is 300rpm-500rpm, so that the reaction proceeds at a uniform speed. Specifically, the reaction temperature can be 75°C, 80°C, 85°C, 90°C, 95°C, etc., and the rotation speed during the reaction can be 300rpm, 400rpm, 500rpm, etc.

[0137] Furthermore, after the second mixed metal salt solution is added, the reaction is continued for 0.5h-2.0h (such as 0.5h, 1.0h, 1.5h, 2.0h, etc.), and then solid-liquid separation is performed, and the obtained solid material is washed and dried to obtain a precursor with a dense shell.

[0138] S4. Preparation of ternary positive electrode materials

[0139] The ternary precursor, the second doping element compound and the lithium source are mixed and calcined to obtain a ternary positive electrode material.

[0140] Wherein, the doping element contained in the second doping element compound is selected from at least one of Zr, Sr, Mo, Ba, W, B, Ti, Mg, Li, C, F, Si, Ca, Cu, La, P, Ce, Bi, In, Nb and Y, and the doping element contained in the second doping element compound can be any one or more of the above. The second doping element compound is selected from at least one of oxides, fluorides, carbonates, hydroxides, nitrides, borides and nitrates, and the second doping element compound can be any one or more of the above. By adjusting the amount of the second doping element compound, the doping amount of the doping element meets the requirements.

[0141] In some embodiments, the lithium source may be lithium hydroxide, but is not limited thereto. The molar ratio of the total amount of nickel, cobalt and M elements in the ternary precursor to the lithium content in the lithium source is 1:(1.05-1.1), which may be 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1.10, etc.

[0142] In some embodiments, calcination is carried out in an oxygen-containing atmosphere. During the calcination process, a primary calcination is first carried out at 400°C-500°C for 2h-6h, and then a secondary calcination is carried out at 750°C-850°C for 10h-15h. Through a two-stage calcination process, low-temperature calcination is first carried out and then high-temperature calcination is carried out to obtain a uniform lithium battery positive electrode material. Specifically, the oxygen-containing atmosphere can be an oxygen atmosphere, but is not limited thereto. The temperature of the primary calcination can be 400°C, 420°C, 450°C, 480°C, 500°C, etc., and the primary calcination time can be 2h, 3h, 4h, 5h, 6h, etc.; the temperature of the secondary calcination can be 750°C, 780°C, 800°C, 820°C, 850°C, etc., and the secondary calcination time can be 10h, 11h, 12h, 13h, 14h, 15h, etc.

[0143] In some embodiments, the ternary precursor, the second doping element compound and the lithium source are first mixed and ground, and then calcined. Grinding allows the raw materials to be better mixed and evenly mixed, which is beneficial to improving the uniformity of the positive electrode material.

[0144] It should be noted that the lithium battery positive electrode material prepared in the embodiment of the present invention has high crack strength and a core-shell structure. The primary particles in the core are radially arranged and have a certain porosity. The shell is relatively dense and has doping elements and a lower Ni content.

[0145] The embodiment of the present invention further provides a positive electrode plate, including the above-mentioned lithium battery positive electrode material, and may also include a positive electrode plate, the positive electrode plate is provided with a positive electrode active coating, and the lithium battery positive electrode material exists in the positive electrode active coating.

[0146] An embodiment of the present invention further provides a lithium battery, including the above-mentioned positive electrode plate, and may also include a negative electrode plate, an electrolyte, a separator, etc., to form a complete battery structure with good cycle performance.

[0147] Specifically, the specific types of the negative electrode sheet, electrolyte, and separator are not limited. During the charge and discharge process of the secondary battery, active ions are intercalated and removed back and forth between the positive electrode sheet and the negative electrode sheet, and the electrolyte plays a role in conducting ions between the positive electrode sheet and the negative electrode sheet.

[0148] In other embodiments, the battery may not be in the form of a secondary battery, but may be in the form of a battery module, a battery pack, etc.

[0149] The embodiment of the present invention provides a device, including the above-mentioned secondary battery, battery module or battery pack, which can be used as a power source of the device or as an energy storage unit of the device. The device can be, but is not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0150] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0151] The present invention provides positive electrode materials as shown in Table 1 and Table 2, and the cracking strength of the positive electrode materials is evaluated; further, the cycle performance and electrochemical performance are tested, and the results are listed in Table 3. The method for characterizing and testing the performance of the positive electrode materials prepared in the embodiments and comparative examples is as follows:

[0152] (1) The overall and cross-sectional microstructures of the material were observed using a JEOL JSM-6490LV scanning electron microscope. In order to obtain the complete cross-sectional morphology of the sample, the sample was cut using a focused ion beam method. The porosity analysis of the ion-cut profile was performed as follows: NanoMeasurer software was used to measure the porosity of the ion-cut profile.

[0153] (2) The active material was coated on an ultra-thin aluminum foil and assembled into a mold battery with a beryllium window. An in-situ XRD test was then performed on an EMPYREAN XRD diffractometer. During the test, the battery was charged and discharged at a current density of 0.1C. The 2θ range of the X-ray scan was 10-60°, and each scanning cycle was 600 s. The values ​​of the cell parameters c and a during the charging process at a voltage of 3-4.5 V and after 10 cycles were recorded, and the values ​​of the cell parameters c and a were calculated. and .

[0154] (3) Particle size: tested using MS3000 laser particle size analyzer.

[0155] (4) Tap density TD: measured in accordance with GB / T 21354-2008 method for measuring tap density of powder products.

[0156] (5) BET specific surface area: The data of nitrogen adsorption and desorption curves at medium and low pressure stages are analyzed using the BET formula to obtain the specific surface area of ​​the material. The test is performed on the Autosorb IQ2 fully automatic specific surface area pore size analyzer produced by Anton Paar Instruments of Austria. The BET of the positive electrode material during the first charge (denoted as BET0 ) and the BET of the positive electrode material after 100 cycles of charge and discharge (denoted as BET t ), the sampling method after the cycle is as follows: after the cycle, the battery is flexibly disassembled, the electrode piece is taken out, the electrode piece is immersed in DMSO, and stirred until the electrode powder is completely detached. The electrode powder is rinsed with ethanol for 5 times, and then dried at 60°C to constant weight. The carbon material and the positive electrode material in the electrode powder are separated by a magnetic separator, and the separated positive electrode material is the sample to be tested.

[0157] (6) Chemical composition analysis was performed using PE Avio200 inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0158] (7) The samples were characterized using a FEI Titan Cubed G2 60-300 transmission electron microscope. The local diffraction pattern of the material was first obtained by selected area electron diffraction (SAED) to determine the crystal structure, and then a high-resolution atomic arrangement image was obtained by high-angle annular dark field imaging (HAADF-STEM) mode, and the element distribution of the material was qualitatively and quantitatively analyzed in combination with the EDS detector.

[0159] (8) Determination of crushing strength: The prepared powder is dispersed in NMP by ultrasonic treatment, and the obtained dispersion is dropped on a 2cm*2cm smooth silicon wafer and dried under a heating lamp to obtain a well-dispersed sample. The sample is observed under an optical microscope, and particles on the silicon wafer that are more than 100μm apart are selected. Using a flat indentation head with a diameter of 100μm, an indentation test of the marked particles is carried out on a CSM UNHT nanoindenter to obtain a pressure-displacement relationship curve. In the real-time monitoring of the indentation experiment, the sudden drop in pressure is used to determine whether the particle has been crushed; the maximum pressure P before the sudden drop in pressure is used to calculate the crushing strength of the particle according to formula (1) ( St ), take n particles from each sample for testing, and calculate the average crushing strength according to formula (2) ( ).

[0160] St = 2.8 × P / (πd 2 ) formula (1)

[0161] = Formula (2)

[0162] Wherein, St represents the crushing strength, in MPa; P represents the maximum pressure value corresponding to the pressure drop point, in mN; d represents the particle diameter of the lithium battery positive electrode material, in μm; represents the average crushing strength, n is the sample size, and n=10 in the test of the specific embodiment of the present invention.

[0163] (9) Electrochemical performance: The rate performance test was carried out using the LANHE CT2001A battery testing system.

[0164] Electrode preparation method: The ternary cathode material, conductive carbon black and PVDF were weighed in a mass ratio of 8:1:1, ground thoroughly and put into a bottle, and an appropriate amount of NMP solvent was added. The mixture was stirred on a stirrer for 24 h to form a uniform slurry. The prepared slurry was evenly coated on a clean aluminum foil using a wet film preparation device, and the loading amount was controlled to be 2.5±0.05 mg / cm 2 Then, place it in a vacuum drying oven at 100°C for 24 hours to dry until there is no material attached. Then, place the electrode sheet on an oil press and roll it at a pressure of 6MPa.

[0165] Button battery assembly: The positive electrode sheet is further punched into a circular electrode sheet with a diameter of 12 mm, and then a CR2032 button battery is assembled using a metal lithium disc as the negative electrode, Celgard2300 as the separator, and 1M LiPF6 solution (the solvent is a mixed solution of EMC, DC, and DMC in a volume ratio of 1:1:1) as the electrolyte.

[0166] The parameters such as particle size D50, TD, BET, and crack strength obtained in the examples and comparative examples are shown in Tables 1 and 2, and the crack strength is calculated as shown in Tables 1 and 2.

[0167] Table 1 Chemical formula of cathode materials, D50 and TD test results

[0168]

[0169] Table 2 Positive electrode materials provided in various embodiments and comparative examples

[0170]

[0171] Table 3 Cyclic performance and electrochemical performance test results of various embodiments and comparative examples

[0172]

[0173] From the data in Table 1 and Table 2, it can be seen that the greater the crack strength of the positive electrode material, the greater the change rate of the specific surface area (BET t / BET 0 ) is smaller, indicating that the material has a greater crack resistance, a stronger ability to resist microcracks during the charge and discharge cycle, and a better cycle stability. The crack resistance of the comparative example exceeds the range specified in this application, resulting in a significant decrease in cycle performance.

[0174] Example 1

[0175] This embodiment provides a lithium battery positive electrode material (LiN i0.761 Co0.11 Mn 0.123 Ti 0.006 The preparation method of O2) corresponds to the product of Example 1 above, comprising the following steps:

[0176] (1) Preparation of precursor core

[0177] According to the molar ratio of nickel, cobalt and manganese of 8:1:1, the metal sulfate was weighed and dissolved in deionized water to form a metal salt solution with a total metal ion concentration of 2M. 70% volume of coprecipitation bottom liquid was added to the reactor, the ammonia concentration of the bottom liquid was 5g / L, the pH was 12±0.2, nitrogen was introduced, the metal salt solution, the precipitant sodium hydroxide solution (30wet%) and the complexing agent ammonia solution (20wt%) were added to the reactor at the same time through the feed pump, the temperature was raised to 85°C and the coprecipitation reaction was carried out at a stirring speed of 600rpm. During the reaction, the flow rate of ammonia water was adjusted to stabilize the ammonia concentration at 4g / L, the flow rate of sodium hydroxide solution was adjusted to stabilize the reaction pH at 11, the flow rate of the metal salt solution was adjusted to 450L / h, the reaction conditions were maintained until the D50 particle size was 8μm, the feeding was stopped and the aging was carried out for 12h. After aging, the slurry was washed with 60 g / L NaOH solution at 80 °C to remove the sodium sulfur residue, then rinsed with 80 °C pure water, dried at 120 °C for 12 h, and sieved to obtain the ternary precursor core (porosity of 8.44%).

[0178] (2) Preparation of reinforcement precursor

[0179] A reinforcement solution was prepared. The reinforcement solution was an aqueous solution containing 2 wt % manganese acetate, 0.15 wt % lithium hydroxide, and 1.5 wt % starch. The viscosity of the reinforcement solution was 6.5 mPa.s.

[0180] The precursor core obtained in step (1) is added to the reinforcement solution, the solid-liquid ratio of the precursor core to the reinforcement solution is 1g:100mL, and the reaction solution is obtained after ultrasonication for 30 minutes. The reaction solution is placed in a high-pressure reactor, and the reaction solution is pressurized by heating to vaporize the solvent. The heating temperature is controlled to be 100-110°C, and the pressure is controlled to be 15MPa to ensure that the precursor core is completely infiltrated. After maintaining the pressure for 30 minutes, the reaction solution is filtered. The filtered solid material is dried at 100°C for 8 hours, and then calcined at 650°C for 6 hours. After cooling, the reinforcement precursor core is obtained.

[0181] (3) Preparation of ternary precursor with core-shell structure

[0182] The sulfate of nickel, cobalt and manganese and titanium disulfate are dissolved in deionized water and an acid is added to adjust the pH to 4 to form a metal salt solution, wherein the molar ratio of nickel, cobalt and manganese in the nickel salt, cobalt salt and manganese salt in the metal salt solution is 50:30:20, the concentration of the first doping element compound is 0.11 M, and the total concentration of nickel, cobalt and manganese ions in the metal salt solution is 2 M. The ratio of the molar amount of nickel, cobalt and manganese in the reinforcement precursor core prepared in step (2) to the molar amount of nickel, cobalt and manganese in the metal salt solution is 8:1.

[0183] Add 20% volume of deionized water into the reactor, and introduce nitrogen. Add the reinforced precursor core obtained in step (2), and slowly drip the metal salt solution into the reactor at 150 L / h using a peristaltic pump while stirring. Adjust the pH of the reaction solution to 11±0.2 and the ammonia concentration to 5 g / L using sodium hydroxide solution and ammonia water. After the addition is completed, react for 1 hour, filter and rinse with 80°C pure water, and dry at 120°C for 12 hours to obtain a ternary precursor with a core-shell structure.

[0184] (4) Preparation of ternary cathode materials

[0185] The ternary precursor obtained in step (3) is mixed and ground with lithium hydroxide, and then calcined to obtain a ternary positive electrode material having a chemical formula of LiN i0.761 Co 0.11 Mn 0.123 Ti 0.006 O2. The ternary precursor and lithium source were added at a Li / (Ni+Co+Mn) ratio of 1.05. Calcination conditions: in an oxygen environment, the temperature was raised to 450°C at 1°C / min and kept for 4h, then raised to 800°C at 2°C / min and kept for 12h.

[0186] Example 2

[0187] The difference from Example 1 is that step (1) is as follows:

[0188] According to the molar ratio of nickel, cobalt and manganese of 8:1:1, the metal sulfate was weighed and dissolved in deionized water to form a metal salt solution with a metal ion concentration of 2M. 60% volume of coprecipitation bottom liquid was added to the reactor, the ammonia concentration of the bottom liquid was 5.5g / L, the pH was 12±0.2, nitrogen was introduced, the metal salt solution, the precipitant sodium hydroxide solution (30wet%) and the complexing agent ammonia solution (20wt%) were added to the reactor through the feed pump at the same time, the temperature was raised to 75°C and the coprecipitation reaction was carried out at a stirring speed of 800rpm. During the reaction, the flow rate of ammonia water was adjusted to stabilize the ammonia concentration at 7g / L, the flow rate of sodium hydroxide solution was adjusted to stabilize the reaction pH at 11, the flow rate of the metal salt solution was adjusted to 450L / h, the reaction conditions were maintained until the D50 particle size was 8μm, the feeding was stopped and the aging was carried out for 12h. After aging, the slurry was washed with 60 g / L NaOH solution at 80 °C to remove the sodium sulfur residue, then rinsed with 80 °C pure water, dried at 120 °C for 12 h, and sieved to obtain the ternary precursor core (porosity of 4.13%).

[0189] Example 3

[0190] The difference from Example 1 is that step (1) is as follows:

[0191] According to the molar ratio of nickel, cobalt and manganese of 8:1:1, the metal sulfate was weighed and dissolved in deionized water to form a metal salt solution with a metal ion concentration of 2M. 80% volume of the coprecipitation bottom liquid was added to the reactor, the ammonia concentration of the bottom liquid was 4.5g / L, the pH was 12±0.2, nitrogen was introduced, the metal salt solution, the precipitant sodium hydroxide solution (30wet%) and the complexing agent ammonia solution (20wt%) were added to the reactor through the feed pump at the same time, the temperature was raised to 95°C and the coprecipitation reaction was carried out at a stirring speed of 800rpm. During the reaction, the flow rate of ammonia water was adjusted to stabilize the ammonia concentration at 3g / L, the flow rate of sodium hydroxide solution was adjusted to stabilize the reaction pH at 11, the flow rate of the metal salt solution was adjusted to 450L / h, the reaction conditions were maintained until the D50 particle size was 8μm, the feeding was stopped and the aging was carried out for 12h. After aging, the slurry was washed with 60 g / L NaOH solution at 80 °C to remove the sodium sulfur residue, then rinsed with 80 °C pure water, dried at 120 °C for 12 h, and sieved to obtain the ternary precursor core (porosity of 11.85%).

[0192] Example 4

[0193] The only difference from Example 1 is that some conditions in steps (2) to (4) are different, as follows:

[0194] In step (2): the reinforcement solution is an aqueous solution containing 2 wt% aluminum isopropoxide and 0.24 wt% lithium hydroxide, and the viscosity of the reinforcement solution is 5.8 mPa.s. The solid-liquid ratio of the precursor core to the reinforcement solution is 1 g:100 mL. The drying is performed at 100°C for 8 h, and the calcination is performed at 600°C for 5 h.

[0195] In step (3): dissolve the sulfate of nickel, cobalt and manganese and magnesium sulfate in deionized water and add acid to adjust the pH to 4 to form a metal salt solution. The molar ratio of nickel, cobalt and manganese in the nickel salt, cobalt salt and manganese salt in the metal salt solution is 60:20:20; the concentration of magnesium sulfate is 0.018M, and the total concentration of nickel, cobalt and manganese ions in the metal salt solution is 2M. The ratio of the molar amount of nickel, cobalt and manganese in the ternary precursor core to the molar amount of nickel, cobalt and manganese in the metal salt solution is 8:1. Add 20% volume of deionized water to the reactor, and pass nitrogen gas into it. Add the reinforced precursor core obtained in step (2), and slowly drip the metal salt solution into the reactor at 100L / h with a peristaltic pump under stirring. Adjust the pH of the reaction solution to 11±0.2 with sodium hydroxide solution and ammonia water, and the ammonia concentration to 3g / L. After the dripping is completed, react for 1h, filter and rinse with 80℃ pure water, and dry at 120℃ for 12h to obtain a ternary precursor with a core-shell structure.

[0196] In step (4): the ternary precursor and the lithium source are added at a Li / (Ni+Co+Mn) ratio of 1.05. Calcination conditions: in an oxygen environment, the temperature is raised to 500°C at 1°C / min and kept for 4 hours, then raised to 750°C at 2°C / min and kept for 12 hours.

[0197] Example 5

[0198] The only difference from Example 1 is that some conditions in steps (2) to (4) are different, as follows:

[0199] In step (2): the reinforcement solution is an aqueous solution containing 2wt% cobalt acetate, 0.75wt% lithium acetate, 1.1wt% phosphoric acid, and 1.8wt% Carbomer 940, and the viscosity of the reinforcement solution is 7.4mPa.s. The solid-liquid ratio of the precursor core to the reinforcement solution is 1g:100mL. Drying is performed at 100°C for 8h, and calcination is performed at 700°C for 10h.

[0200] In step (3): dissolve the sulfate of nickel, cobalt and manganese and zirconium acetate in deionized water and add acid to adjust the pH to 5 to form a metal salt solution. The molar ratio of nickel, cobalt and manganese in the nickel salt, cobalt salt and manganese salt in the metal salt solution is 60:20:20; the concentration of zirconium acetate is 0.04M, and the total concentration of nickel, cobalt and manganese ions in the metal salt solution is 2M. The ratio of the molar amount of nickel, cobalt and manganese in the ternary precursor core to the molar amount of nickel, cobalt and manganese in the metal salt solution is 4:1. Add 20% volume of deionized water to the reactor, pass nitrogen, add the reinforced precursor core obtained in step (2), and slowly drip the metal salt solution into the reactor at 150L / h with a peristaltic pump under stirring. Adjust the pH of the reaction solution to 11±0.2 with sodium hydroxide solution and ammonia water, and the ammonia concentration to 5g / L. After the addition is completed, react for 1h, filter and rinse with 80℃ pure water, and dry at 120℃ for 12h to obtain a ternary precursor with a core-shell structure.

[0201] In step (4): the ternary precursor and the lithium source are added at a Li / (Ni+Co+Mn) ratio of 1.05. Calcination conditions: in an oxygen environment, the temperature is raised to 500°C at 1°C / min and kept for 4 hours, then raised to 850°C at 2°C / min and kept for 12 hours.

[0202] Example 6

[0203] The only difference from Example 1 is that some conditions in steps (2) to (4) are different, as follows:

[0204] In step (2): the reinforcement solution is an aqueous solution containing 2 wt% aluminum isopropoxide and 0.24 wt% lithium hydroxide, and the viscosity of the reinforcement solution is 5.8 mPa.s. The solid-liquid ratio of the precursor core to the reinforcement solution is 1 g:100 mL. The drying is performed at 100°C for 8 h, and the calcination is performed at 700°C for 10 h.

[0205] In step (3): dissolve the sulfate of nickel, cobalt and manganese and titanium disulfate in deionized water and add acid to adjust the pH to 4 to form a metal salt solution. The molar ratio of nickel, cobalt and manganese in the nickel salt, cobalt salt and manganese salt in the metal salt solution is 33:33:34; the concentration of titanium disulfate is 0.1M, and the total concentration of nickel, cobalt and manganese ions in the metal salt solution is 2M. The ratio of the molar amount of nickel, cobalt and manganese in the ternary precursor core to the molar amount of nickel, cobalt and manganese in the metal salt solution is 12:1. Add 20% volume of deionized water to the reactor, and pass nitrogen into it. Add the reinforced precursor core obtained in step (2), and slowly drip the metal salt solution into the reactor at 200L / h with a peristaltic pump under stirring. Adjust the pH of the reaction solution to 11±0.2 with sodium hydroxide solution and ammonia water, and the ammonia concentration to 7g / L. After the addition is completed, react for 1h, filter and rinse with 80℃ pure water, and dry at 120℃ for 12h to obtain a ternary precursor with a core-shell structure.

[0206] (4) The ternary precursor and lithium source were added at a Li / (Ni+Co+Mn) ratio of 1.05, and the doping amount of B element in boron oxide was 0.2%. Calcination conditions: in an oxygen environment, the temperature was increased to 500°C at 1°C / min and kept for 4 hours, and then increased to 850°C at 2°C / min and kept for 12 hours.

[0207] Example 7

[0208] The only difference from Example 1 is that in step (2): the reinforcement solution is an aqueous solution containing 2 wt% aluminum isopropoxide, 0.24 wt% lithium hydroxide, and 0.62 wt% starch, and the viscosity of the reinforcement solution is 6.5 mPa.s.

[0209] Example 8

[0210] The only difference from Example 1 is that in step (2): the reinforcement solution is a solution containing 2 wt% cobalt acetate, 0.75 wt% lithium acetate, 1.1 wt% phosphoric acid, and 0.79 wt% starch in water, and the viscosity of the reinforcement solution is 6.5 mPa.s.

[0211] Example 9

[0212] The only difference from Example 1 is that in step (2): the reinforcement solution is an aqueous solution containing 2 wt % manganese acetate and 0.15 wt % lithium hydroxide, and the viscosity of the reinforcement solution is 1.62 mPa.s.

[0213] Example 10

[0214] The only difference from Example 1 is that in step (2): the reinforcement solution is an aqueous solution containing 2 wt% manganese acetate, 0.15 wt% lithium hydroxide, and 2.12 wt% starch, and the viscosity of the reinforcement solution is 7.92 mPa.s.

[0215] Comparative Example 1 (porosity less than 4%)

[0216] The difference from Example 1 is that step (1) is as follows:

[0217] According to the molar ratio of nickel, cobalt and manganese of 8:1:1, the metal sulfate was weighed and dissolved in deionized water to form a metal salt solution with a metal ion concentration of 2M. 50% volume of coprecipitation bottom liquid was added to the reactor, the ammonia concentration of the bottom liquid was 4g / L, the pH was 11.5±0.2, nitrogen was introduced, the metal salt solution, the precipitant sodium hydroxide solution (30wet%) and the complexing agent ammonia solution (20wt%) were added to the reactor through the feed pump at the same time, the temperature was raised to 85°C and the coprecipitation reaction was carried out at a stirring speed of 600rpm. During the reaction, the flow rate of ammonia water was adjusted to stabilize the ammonia concentration at 3g / L, the flow rate of sodium hydroxide solution was adjusted to stabilize the reaction pH at 10, the flow rate of the metal salt solution was adjusted to 450 L / h, the reaction conditions were maintained until the D50 particle size was 8μm, the feeding was stopped and the aging was carried out for 12h. After aging, the slurry was washed with 60 g / L NaOH solution at 80 °C to remove the sodium sulfur residue, then rinsed with 80 °C pure water, dried at 120 °C for 12 h, and sieved to obtain the ternary precursor core (porosity of 2.2%).

[0218] Comparative Example 2 (primary particles are granular)

[0219] The difference from Example 1 is that step (1) is as follows:

[0220] According to the molar ratio of nickel, cobalt and manganese of 8:1:1, the metal sulfate was weighed and dissolved in deionized water to form a metal salt solution with a metal ion concentration of 2M. 50% volume of coprecipitation bottom liquid was added to the reactor, the ammonia concentration of the bottom liquid was 5g / L, the pH was 12±0.2, nitrogen was introduced, the metal salt solution, the precipitant sodium hydroxide solution (30wet%) and the complexing agent ammonia solution (20wt%) were added to the reactor at the same time through the feed pump, the temperature was raised to 50°C and the coprecipitation reaction was carried out at a stirring speed of 300rpm. During the reaction, the flow rate of ammonia water was adjusted to stabilize the ammonia concentration at 6g / L, the flow rate of sodium hydroxide solution was adjusted to stabilize the reaction pH at 11, the flow rate of the metal salt solution was adjusted to 500 L / h, the reaction conditions were maintained until the D50 particle size was 8μm, the feeding was stopped and the aging was carried out for 12h. After aging, the slurry was washed with 60 g / L NaOH solution at 80 °C to remove the sodium sulfur residue, then rinsed with 80 °C pure water, dried at 120 °C for 12 h, and sieved to obtain the ternary precursor core (porosity of 6.7%).

[0221] Comparative Example 3 (precursor shell not formed)

[0222] The difference from Example 1 is that step (3) is not performed, and step (4) is as follows:

[0223] The ternary precursor is mixed with lithium hydroxide and titanium oxide and ground, and then calcined to obtain the ternary positive electrode material. The ternary precursor and lithium source are added according to the Li / (Ni+Co+Mn) ratio of 1.05, and the doping amount of Ti element in titanium oxide is 0.2%. Calcination conditions: oxygen environment, heating to 450℃ at 1℃ / min for 4h, and then heating to 800℃ at 2℃ / min for 12h.

[0224] Comparative Example 4 (without grain boundary reinforcement)

[0225] The only difference from Example 1 is that step (2) is not performed.

[0226] Result analysis:

[0227] The ion cross-sectional diagrams of the positive electrode materials prepared in Example 1 and Comparative Example 1 are as follows: Figure 1 and Figure 2 As shown, a core-shell structure can be seen, and the porosity of Example 1 is higher.

[0228] The cross-sectional views of Example 1 and Comparative Example 2 are as follows: Figure 3 and Figure 4 As shown, it can be seen that the primary particles of Example 1 are radially radiated, while the primary particles of Comparative Example 2 are granular.

[0229] The XRD patterns of the precursor core and the precursor material prepared in Example 1 are as follows: Figure 5 As shown, it can be seen that: consistent with the card, there is no impurity phase on the surface, and the (006) peak, (012) peak, (018) peak and (110) peak of all samples have obvious splitting, and the surface samples have a good layered structure.

[0230] The TEM and EDS images of the positive electrode materials prepared in Example 1 and Example 4 are as follows: Figure 6 and Figure 7 As shown, it can be seen that: the enrichment of Mn element or Al element appears at the grain boundary of the primary particles, indicating that the reinforcing agent is successfully distributed near the grain boundary to reinforce the primary particles.

[0231] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A lithium battery positive electrode material, characterized in that: The cracking strength of the lithium battery positive electrode material is 4-15 MPa; in, ; Where, St represents the crushing strength, which is obtained through the indentation test and the unit is MPa; It represents the average crushing strength in MPa. = , n is the sample size, n≥10; It refers to the maximum change of shear strain during the first charging process; = - ; It refers to the change in shear strain after 10 charge-discharge cycles, t=10; = - , It refers to the shear strain measured in static state after 10 charge-discharge cycles. It refers to the shear strain measured in static state before the first charge; a and c represent unit cell parameters; St=2.8×P / (πd 2 ); P represents the maximum pressure value corresponding to the pressure drop point in the indentation test, in mN; d represents the particle diameter of lithium battery positive electrode material, in μm; The value of is 0.2-0.3, The value of is 0.01-0.20, The value is 90-140 MPa; c and a were obtained by X-ray diffractometer XRD test; The general formula of the lithium battery positive electrode material is Li x Ni a Co b M c M' 1-a-b-c A y O 2-y ; In the general formula, M is selected from at least one of Al and Mn; M' is at least one selected from Zr, Sr, Mo, Ba, W, B, Ti, Mg, Li, Si, Ca, Cu, La, Ce, Bi, In, Al, Nb and Y; A is selected from at least one of P and F; 0.95≤x<1.1, a>0, b>0, c>0, 0.95≤(a+b+c)≤1, 0≤y≤0.

01.

2. The lithium battery positive electrode material according to claim 1, characterized in that The cracking strength of the lithium battery positive electrode material is 6-15 MPa.

3. A method for preparing a lithium battery positive electrode material according to any one of claims 1 to 2, characterized in that: include: A precursor core is prepared by coprecipitation reaction of nickel salt, cobalt salt and M salt; The precursor core is mixed with a reinforcement solution for reaction, and the reinforcement precursor core is obtained after calcination; wherein the raw materials in the reinforcement solution are calcined to obtain a reinforcement aid; the reinforcement aid is selected from at least one of LiAlO2, LiMn2O4 and LiCoPO4; A coprecipitation reaction is carried out using nickel salt, cobalt salt, M salt and a first doping element compound, and a shell is continuously grown on the basis of the core of the reinforced precursor to obtain a ternary precursor with a core-shell structure; wherein the doping element contained in the first doping element compound is selected from at least one of Ti, Al, Zr and Mg; The ternary precursor is mixed with a lithium source and calcined; or, the ternary precursor, a second doping element compound and a lithium source are mixed and calcined; the doping element contained in the second doping element compound is selected from at least one of Zr, Sr, Mo, Ba, W, B, Ti, Mg, Li, F, Si, Ca, Cu, La, P, Ce, Bi, In, Nb and Y.

4. The preparation method according to claim 3, characterized in that: The primary particles of the precursor core are radially arranged, and the porosity is 4%-12%; The preparation process of the precursor core includes: preparing a base liquid in a reaction kettle, and passing a first mixed metal salt solution, a first precipitant solution, and a first complexing agent solution into the base liquid for a coprecipitation reaction. The process of preparing the precursor core satisfies at least one of the characteristics A1 to K1: Feature A1: The reaction temperature of the coprecipitation reaction is controlled to be 75°C-95°C; Feature B1: The reaction pH value of the coprecipitation reaction is controlled to be 10.5-11.5; Characteristic C1: The first complexing agent solution is an ammonia solution with a mass fraction of 18%-22%, and the ammonia concentration in the reactor is controlled to be 3g / L-7g / L during the precipitation process; Feature D1: The total metal ion molar concentration of the first mixed metal salt solution is 1.8M-2.2M, and the flow rate of the first mixed metal salt solution is 400L / h-500L / h; Characteristic E1: After the reaction reaches a particle size D50 of 2-17 μm, the feeding is stopped; Feature F1: After the coprecipitation reaction is completed, aging is performed, followed by alkali solution washing, water washing, and drying; Feature G1: The molar ratio of nickel, cobalt and M in the first mixed metal salt solution is (35-98): (1-35): (1-35); Feature H1: The first mixed metal salt solution is selected from any one of nitrate, chloride and sulfate; Feature I1: The first precipitant solution is a sodium hydroxide solution with a mass fraction of 30%-34%; Feature J1: The concentration of ammonia in the base solution is 4.5 g / L-5.5 g / L, and the pH value is 11.8-12.2; Feature K1: The coprecipitation reaction is carried out under the protection of an inert atmosphere, and the rotation speed during the reaction is 400rpm-800rpm.

5. The preparation method according to claim 3, characterized in that: The preparation process of the reinforced precursor core includes: mixing the precursor core with the reinforcement solution by ultrasonication, reacting for 10 min to 60 min at a temperature of 100° C. to 150° C. and a pressure of 10 MPa to 20 MPa, then separating the solid from the liquid, and calcining the obtained solid material; The preparation process of the reinforced precursor core satisfies at least one of features A2 to F2: Feature A2: The strengthening solution further contains a thickener, and the viscosity of the strengthening solution is adjusted to be 5 mPa·s-8 mPa·s by adjusting the amount of the thickener; Feature B2: When feature A2 is met, the thickener is selected from at least one of carbomer, xanthan gum, gelatin and starch; Characteristic C2: The amount of the reinforcement solution corresponding to 1g of the precursor core is 90mL-110mL; Feature D2: Control the ultrasonic time to 10min-60min; Feature E2: The calcination temperature is controlled to be 600°C-700°C and the calcination time is 3h-8h; Feature F2: The solid material is first dried at 80° C.-120° C. for 5 h-10 h, and then calcined.

6. The preparation method according to claim 3, characterized in that: The preparation process of the ternary precursor with a core-shell structure comprises: adding the reinforced precursor core to the bottom liquid in the reaction kettle, and passing the second mixed metal salt solution, the second precipitant solution and the second complexing agent solution into the reaction kettle for coprecipitation reaction; The second mixed metal salt solution contains nickel salt, cobalt salt, M salt and a first doping element compound, and the addition rate of the second mixed metal salt solution is regulated so that the addition rate of nickel, cobalt and M element during the reaction is controlled to be lower than the addition rate during the preparation of the precursor core; The preparation process of the ternary precursor having a core-shell structure satisfies at least one of the characteristics A3 to I3: Feature A3: The total concentration of nickel, cobalt and M element in the second mixed metal salt solution is 1.8M-2.2M, the flow rate of the second mixed metal salt solution is 100L / h-200L / h, and the pH value of the second mixed metal salt solution is regulated to be 2-5; Feature B3: The total molar amount of metal is calculated based on the total molar amount of nickel, cobalt and M element, and the ratio of the total molar amount of metal in the reinforcement precursor core to the total molar amount of metal in the second mixed metal salt solution is (4-12): 1; Characteristic C3: In the second mixed metal salt solution, the molar ratio of nickel, cobalt and M element is (30-60): (20-35): (20-35); Characteristic D3: The reaction temperature of the coprecipitation reaction is 75°C-95°C, and the reaction pH is 10.8-11.2; Feature E3: The second complexing agent solution is an ammonia solution with a mass fraction of 18%-22%, and the ammonia concentration in the reactor is controlled to be 3g / L-7g / L during the precipitation process; Feature F3: The first doping element compound is selected from at least one of titanium disulfate, sodium aluminate, zirconium nitrate, zirconium acetate, zirconium sulfate, magnesium sulfate and magnesium nitrate; Feature G3: The bottom liquid in the reactor is water, and the second precipitant solution is a sodium hydroxide solution with a mass fraction of 30%-40%; Characteristic H3: The coprecipitation reaction is carried out under the protection of an inert atmosphere, and the rotation speed during the reaction is 300rpm-500rpm; Feature I3: After the second mixed metal salt solution is added, the reaction is continued for 0.5h-2.0h, and then solid-liquid separation is performed, and the obtained solid material is washed with water and dried.

7. The preparation method according to claim 3, characterized in that: The process of mixing and calcining the ternary precursor, the second doping element compound and the lithium source satisfies at least one of Features A4 to F4: Feature A4: The molar ratio of the total amount of nickel, cobalt and M elements in the ternary precursor to the lithium content in the lithium source is 1:(1.05-1.1); Feature B4: The lithium source is selected from lithium hydroxide; Feature C4: The second doping element compound is selected from at least one of oxides, fluorides, carbonates, hydroxides, nitrides, borides and nitrates; Feature D4: During the calcination process, the calcination is first performed at 400°C-500°C for 2h-6h, and then a secondary calcination is performed at 750°C-850°C for 10h-15h; Feature E4: calcining in an oxygen-containing atmosphere; Feature F4: The ternary precursor, the second doping element compound and the lithium source are first mixed and ground, and then calcined.

8. A positive electrode sheet, characterized in that: The invention comprises the lithium battery positive electrode material as described in any one of claims 1 to 2 or the lithium battery positive electrode material prepared by the preparation method as described in any one of claims 3 to 7.

9. A lithium battery, characterized in that: Including the positive electrode sheet as described in claim 8.