A method for preparing carbon-free phosphate positive electrode material

By mixing phosphate cathode materials in the liquid phase, the preparation method solves the problem of grain size and impurity phases caused by uneven mixing of raw materials in the existing technology, and achieves smaller and more uniform particle generation and higher electric current. performance, low process energy consumption, environmental protection and safety.

CN118495499BActive Publication Date: 2024-10-01四川优源新能源有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964494.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to achieve uniform mixing of raw materials during the mixing and grinding process of lithium iron manganese phosphate and lithium manganese phosphate cathode materials, resulting in large grain size and easy generation of impurity phases, which affects the performance of the materials.

Method used

By mixing phosphate solution, lithium salt solution and salt solution in the liquid phase, the reaction conditions are controlled to be carried out under mild conditions, including stirring, heating and filtration, to ensure uniform mixing of the raw materials at the molecular level and avoid the generation of impurities.

Benefits of technology

It achieves the generation of cathode materials with smaller particle size and more uniformity, reduces energy consumption, improves the purity and electrical performance of the material, and the process is more environmentally friendly and safer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495499B_ABST
    Figure CN118495499B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a carbon-free phosphate positive electrode material, which belongs to the technical field of positive electrode material preparation; the method comprises the following steps: S1. preparing a phosphate solution, a lithium salt solution and a salt solution A respectively; S2. mixing the phosphate solution, the lithium salt solution and the salt solution A in step S1 to obtain an acidic mixed solution C; S3. stirring the mixed solution C in step S2 at room temperature, and adding alkali during the stirring process to obtain a weakly acidic mixed solution D; S4. heating and keeping the mixed solution D in step S3 to obtain a solid-liquid mixture, and then filtering and drying the solid-liquid mixture in sequence to obtain a carbon-free phosphate positive electrode material; the salt solution A is a manganese salt solution or a mixed solution of iron salt and manganese salt. The invention can make the particle size of the generated product smaller and more uniform, and thus make the element distribution in the product more uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery positive electrode material preparation, and specifically relates to a method for preparing a carbon-free phosphate positive electrode material. Background Art

[0002] LiFePO4 (LFP) is considered to be an ideal cathode material for lithium-ion batteries due to its excellent charge and discharge cycle performance, low price, excellent high-temperature performance, and environmental friendliness and pollution-free. However, in recent years, the energy density of LFP batteries has increased rapidly and is close to its limit. With the continuous iteration of battery technology, according to the recommended vehicle model catalog for the promotion and application of new energy released by the Ministry of Industry and Information Technology, the maximum energy density of LFP battery systems in 2022 is 161.27Wh / kg, and this maximum value has hardly changed in the past two years. Since then, lithium iron manganese phosphate and lithium manganese phosphate materials have come into being.

[0003] In the prior art, lithium iron manganese phosphate and lithium manganese phosphate positive electrode materials are mostly prepared by solid phase method, that is, lithium precursor, iron precursor, manganese precursor, phosphorus precursor and carbon source are mixed, ground and calcined in a certain ratio to form lithium manganese (iron) phosphate positive electrode material.

[0004] However, according to the above method, it is difficult to mix the raw materials evenly during the mixing and grinding process, resulting in large grain size and easy generation of impurities in the final product, which in turn affects the performance of the material. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a carbon-free phosphate-based positive electrode material; this method can achieve uniform mixing of raw materials at the molecular level, and realize and control the reaction under relatively mild conditions.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] A method for preparing a carbon-free phosphate-based positive electrode material comprises the following steps:

[0008] S1. preparing a phosphate solution, a lithium salt solution and a salt solution A respectively;

[0009] S2. The phosphate solution, the lithium salt solution and the salt solution A in step S1 are mixed to obtain an acidic mixed solution C;

[0010] S3. The mixed solution C in step S2 is stirred at room temperature, and a base is added during the stirring process to obtain a weakly acidic mixed solution D;

[0011] S4. The mixed solution D in step S3 is heated and kept warm to obtain a solid-liquid mixture, and then the solid-liquid mixture is filtered in sequence to obtain a solid and a mother liquor, and then the solid is dried to obtain a carbon-free phosphate cathode material;

[0012] The salt solution A is a manganese salt solution or a mixed solution of iron salt and manganese salt;

[0013] The chemical formula of the carbon-free phosphate positive electrode material is LiMn x Fe 1-x PO4(0<x≤1).

[0014] The present invention can make the raw materials mixed more evenly by mixing the phosphate solution, the lithium salt solution and the salt solution A in the liquid phase, so that the particle size of the generated particles is smaller and more even, and no impurity phase is detected. This can effectively overcome the technical defects of the prior art of preparing positive electrode materials by the solid phase method, that is, the final product has a large grain size and is prone to the generation of impurities due to the uneven mixing of the raw materials.

[0015] In addition, in the prior art, in addition to the solid phase method for preparing positive electrode materials, the coprecipitation method, sol-gel method and hydrothermal method are also used. The present invention uses the above raw materials in one step to synthesize carbon-free phosphate positive electrode materials. The process path is extremely short. Compared with the above several prior arts, it has the characteristics of low energy consumption, smaller and more uniform particle size of the prepared product, and more uniform element distribution in the product. In addition, organic solvents are generally added to the reaction medium of the hydrothermal method. The reaction medium of the present invention is pure water, and no toxic organic solvents are added during the whole process. Compared with the hydrothermal method, it is more environmentally friendly and safer.

[0016] As an embodiment of the present application, the salt solution A is a salt solution to which a strong acid is added. The salt solution A is a manganese salt solution or a mixed solution of an iron salt and a manganese salt; wherein a strong acid is added to each solution to inhibit the hydrolysis of iron ions or manganese ions.

[0017] As an implementation mode of the present application, in step S2, before the phosphate solution, the lithium salt solution and the salt solution A are mixed, a strong acid is added during the mixing process to obtain an acidic mixed solution B, and then the mixed solution B is mixed with the salt solution A to obtain a mixed solution C. In this solution, the mixed solution is made weakly acidic in order to fully dissolve the lithium salt and the phosphate.

[0018] In addition, the order of adding the phosphate solution, the lithium salt solution and the salt solution A in the present invention is extremely important. The inventors have proved through a large number of experiments that if the order of adding the materials in the present invention is not followed (such as first mixing the salt solution A and the lithium salt solution, and then mixing with the phosphate solution), impurities will be generated in the prepared positive electrode material, which will seriously affect the purity and electrical properties of the product.

[0019] As an embodiment of the present application, the pH of the mixed solution D is 4.5-6.5. In the present invention, by limiting the pH value, it is possible to prevent the generation of impurities in the prepared positive electrode material and maximize the yield of the positive electrode material. If the pH is too high, such as 6.5-7 (excluding 6.5), the (Fe+Mn) / P in the product is 0.6-0.9, which will cause a deviation in the composition and seriously affect the performance of the electrical properties; if it is lower than 4.5, the acidity in the mixed solution reacted in step S4 is too strong, and part of the solid (the positive electrode material is alkaline) will dissolve in the mother liquor, resulting in a low solid weight after drying, which in turn leads to a low yield of the positive electrode material.

[0020] As an embodiment of the present application, the strong acid is one or more of sulfuric acid, hydrochloric acid, and nitric acid.

[0021] As an embodiment of the present application, the alkali added in step S3 is one or both of sodium hydroxide and ammonia water.

[0022] As an embodiment of the present application, the phosphate is one or more of monoammonium phosphate, sodium phosphate, lithium phosphate, and lithium dihydrogen phosphate;

[0023] The lithium salt is one or more of lithium sulfate, lithium chloride, lithium hydroxide, lithium nitrate, lithium carbonate, lithium phosphate, and lithium dihydrogen phosphate;

[0024] The iron salt is one or more of ferrous sulfate, ferrous chloride, and ferrous nitrate;

[0025] The manganese salt is one or more of manganese sulfate, manganese chloride and manganese nitrate.

[0026] As an embodiment of the present application, in step S4, the heating temperature is ≤120 °C, the holding time is 6h, and the pressure is ≤0.1 MPa. In the prior art, the reaction temperature in the reaction medium of the hydrothermal method is usually 180 °C, and the reaction pressure is 2-3MPa. The reaction temperature of the present invention is ≤120 °C, and the reaction pressure is ≤0.1 MPa. Therefore, the temperature and pressure used are lower, and the reaction conditions are milder and more energy-saving than those of the hydrothermal method; in addition, the reaction temperature in the present invention is lower, which is conducive to inhibiting the oxidation of manganese (because manganese has many valence states and is easily oxidized at high temperatures).

[0027] Furthermore, in actual synthesis, the lower the synthesis temperature and the lower the pressure, the easier it is for the obtained positive electrode material to generate impurities. The present invention optimizes various parameters in the production process, such as limiting the order of adding materials, adjusting the pH of the solution, limiting the amount of components, etc., and can synthesize positive electrode materials without impurities and with uniform grain size distribution at low temperature (≤120 °C) and low pressure (≤0.1 MPa), thereby greatly reducing energy consumption and solving the technical defects of low-temperature synthesis with many impurities that have long been difficult to overcome in the industry, which is a very significant improvement.

[0028] Preferably, in step S4, the heating temperature is 90-120° C. The synthesis temperature in the present invention is extremely important. The inventors have proved through a large number of experiments that if the reaction temperature is lower than 90° C., it is difficult to synthesize the positive electrode material in the present invention.

[0029] As an embodiment of the present application, in the mixed solution D, the molar ratio of lithium ions, total metal ions in the salt solution A, and phosphate ions is (1-3): 1: 1.

[0030] As an embodiment of the present application, after step S4, step S5 is further included, namely, adding phosphate or phosphoric acid to the mother liquor obtained by filtration in step S4, and then adjusting the pH to alkaline, precipitating and filtering to obtain lithium phosphate.

[0031] The present invention can convert lithium in the mother liquor into lithium phosphate by processing the mother liquor, thereby realizing the recovery of the lithium phosphate and recycling the lithium phosphate as a raw material, thus saving costs to a great extent.

[0032] As an embodiment of the present application, in S5, the molar ratio of phosphorus ions to lithium ions is not less than 1:3.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The present invention can make the raw material ratio more accurate and the raw material mixing more uniform by mixing the phosphate solution, the lithium salt solution and the salt solution A in the liquid phase, so that the particle size of the generated particles is smaller and more uniform, no impurities are detected, and the element distribution in the product is more uniform; in addition, the present invention can synthesize the carbon-free phosphate-based positive electrode material in one step using the above raw materials, which has the characteristics of short process path and low energy consumption.

[0035] The reaction medium of the invention is pure water, and no toxic organic solvent is added during the whole process, so the preparation method is more environmentally friendly and safe. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is the XRD detection diagram of the product in Example 1;

[0037] Figure 2This is the SEM image of the product in Example 1;

[0038] Figure 3 This is the XRD detection diagram of the product in Example 2;

[0039] Figure 4 This is the SEM image of the product in Example 2;

[0040] Figure 5 This is the XRD detection diagram of the product in Example 3;

[0041] Figure 6 This is the SEM detection image of the product in Example 3;

[0042] Figure 7 It is the XRD detection diagram of the product in Example 4;

[0043] Figure 8 This is the SEM detection image of the product in Example 4;

[0044] Fig. 9 This is the XRD detection diagram of the product in Example 5;

[0045] Fig.10 This is the SEM detection image of the product in Example 5;

[0046] Fig.11 This is the XRD detection diagram of the product in Example 6;

[0047] Fig.12 This is the SEM detection image of the product in Example 6;

[0048] Fig.13 This is the XRD detection diagram of the product in Example 7;

[0049] Fig.14 This is the SEM detection image of the product in Example 7. DETAILED DESCRIPTION

[0050] The technical solutions in the embodiments of the present application are described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0051] Example 1

[0052] In this embodiment, a carbon-free lithium manganese phosphate (LiMnPO4) precursor is prepared using lithium phosphate and manganese sulfate as raw materials and sulfuric acid and sodium hydroxide as acid and base for adjusting the pH value. The preparation method is as follows:

[0053] S1) Use sulfuric acid to fully dissolve lithium phosphate, and use deionized water to prepare 750 mL of a lithium salt solution with a lithium ion concentration of 0.9 mol / L, and adjust the pH to less than 4 with sulfuric acid; use deionized water to prepare 750 mL of a manganese sulfate solution with a manganese ion concentration of 0.3 mol / L, and adjust its pH to less than 4 with sulfuric acid.

[0054] S2) In a 2 L reactor, lithium salt solution and manganese sulfate solution were added in sequence, and the mixture was stirred and mixed to obtain a mixed solution.

[0055] S3) Slowly add sodium hydroxide solution to the reactor until the pH value of the mixed solution reaches 6.5, heat the reactor to 120 °C, maintain the pressure in the reactor at 0.1 MPa, and after keeping the temperature for 6 h, the reaction is completed.

[0056] S4) The mixture in the reactor is filtered, and the filtered solid is washed with deionized water for at least 3 times, and then dried to obtain the product LiMnPO4 (XRD and SEM are shown in Figures 2 and 3, respectively). Figure 1 and Figure 2 as shown).

[0057] S5) collecting the filtered liquid and the washing water obtained by washing the product in a stirring tank, adding phosphoric acid, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding sodium hydroxide solution until the pH value is greater than 10, performing solid-liquid separation, and the obtained solid is lithium phosphate.

[0058] Example 2

[0059] In this embodiment, lithium chloride, ferrous chloride, manganese chloride and sodium phosphate are used as raw materials, and hydrochloric acid and ammonia water are used as acid and base to adjust the pH value to prepare carbon-free lithium manganese iron phosphate (LiMn 0.8 Fe 0.2 PO4) precursor, the preparation method thereof is as follows:

[0060] S1) Prepare 200 mL of lithium chloride solution with a lithium ion concentration of 0.9 mol / L with deionized water, and adjust its pH to less than 4 with hydrochloric acid; prepare 200 mL of manganese chloride solution with a manganese ion concentration of 0.24 mol / L with deionized water, and adjust its pH to less than 4 with hydrochloric acid; prepare 200 mL of ferrous chloride solution with a ferrous ion concentration of 0.06 mol / L with deionized water, and adjust its pH to less than 4 with hydrochloric acid; prepare 200 mL of sodium phosphate solution with a phosphate ion concentration of 0.3 mol / L with deionized water, and adjust its pH to less than 4 with hydrochloric acid.

[0061] S2) In a 2 L reactor, add a manganese salt solution and a ferrous salt solution in sequence, stir evenly, then add a lithium salt solution and a phosphate solution, stir and mix evenly to obtain a mixed solution.

[0062] S3) Slowly add ammonia water to the reactor until the pH value of the mixed solution reaches 5.8, heat the reactor to 110 °C, maintain the pressure in the reactor at 0.05 MPa, and after keeping the temperature for 6 h, the reaction is completed.

[0063] S4) Filter the mixture in the reactor, wash the filtered solid with deionized water for at least 3 times, and dry it to obtain the product LiMn 0.8 Fe 0.2 PO4 (XRD and SEM are shown in Figure 3 and Figure 4 as shown).

[0064] S5) collecting the filtered liquid and the washing water obtained by washing the product in a stirring tank, adding sodium phosphate, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding sodium hydroxide solution until the pH value is greater than 10, performing solid-liquid separation, and the obtained solid is lithium phosphate.

[0065] Example 3

[0066] In this embodiment, lithium nitrate, ferrous nitrate, manganese nitrate and monoammonium phosphate are used as raw materials, and nitric acid and sodium hydroxide are used as acid and base to adjust the pH value to prepare carbon-free lithium manganese iron phosphate (LiMn 0.8 Fe 0.2 PO4) precursor, the preparation method thereof is as follows:

[0067] S1) Prepare 30 L of lithium nitrate solution with a lithium ion concentration of 0.9 mol / L with deionized water, and adjust its pH to less than 4 with nitric acid; prepare 30 L of manganese nitrate solution with a manganese ion concentration of 0.72 mol / L with deionized water, and adjust its pH to less than 4 with nitric acid; prepare 30 L of ferrous nitrate solution with a ferrous ion concentration of 0.18 mol / L with deionized water, and adjust its pH to less than 4 with nitric acid; prepare 30 L of monoammonium phosphate solution with a phosphate ion concentration of 0.9 mol / L with deionized water, and adjust its pH to less than 4 with nitric acid.

[0068] S2) In a 125 L reactor, add a manganese salt solution and a ferrous salt solution in sequence, stir evenly, then add a lithium salt solution and a phosphate solution, stir and mix evenly to obtain a mixed solution.

[0069] S3) Slowly add sodium hydroxide solution to the reactor until the pH value of the mixed solution reaches 6, heat the reactor to 100 °C, keep the pressure in the reactor at normal pressure, and after keeping the temperature for 6 hours, the reaction is completed.

[0070] S4) Filter the mixture in the reactor, wash the filtered solid with deionized water for at least 3 times, and dry it to obtain the product LiMn 0.8 Fe0.2 PO4 (XRD and SEM are shown in Figure 5 and Figure 6 as shown).

[0071] S5) collecting the filtered liquid and the washing water obtained by washing the product in a stirring tank, adding phosphoric acid, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding sodium hydroxide solution until the pH value is greater than 10, performing solid-liquid separation, and the obtained solid is lithium phosphate.

[0072] Example 4

[0073] In this embodiment, lithium sulfate, ferrous sulfate, manganese sulfate and lithium dihydrogen phosphate are used as raw materials, and sulfuric acid and ammonia water are used as acid and base to adjust the pH value to prepare carbon-free lithium manganese iron phosphate (LiMn 0.6 Fe 0.4 PO4) precursor, the preparation method thereof is as follows:

[0074] S1) Prepare 400 mL of lithium sulfate solution with a lithium ion concentration of 0.6 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 400 mL of manganese sulfate solution with a manganese ion concentration of 0.18 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 400 mL of ferrous sulfate solution with a ferrous ion concentration of 0.12 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 400 mL of lithium dihydrogen phosphate solution with a phosphate ion concentration of 0.3 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid.

[0075] S2) In a 2 L reactor, add a manganese salt solution and a ferrous salt solution in sequence, stir evenly, then add a lithium salt solution and a phosphate solution, stir and mix evenly to obtain a mixed solution.

[0076] S3) Slowly add ammonia water to the reactor until the pH value of the mixed solution reaches 4.5, heat the reactor to 100 °C, keep the pressure in the reactor at normal pressure, and after keeping the temperature for 6 hours, the reaction is completed.

[0077] S4) Filter the mixture in the reactor, wash the filtered solid with deionized water for at least 3 times, and dry it to obtain the product LiMn 0.6 Fe 0.4 PO4 (XRD and SEM are shown in Figure 7 and Figure 8 as shown).

[0078] S5) collecting the filtered liquid and the washing water obtained from the washing product in a stirring tank, adding phosphoric acid, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding ammonia water until the pH value is greater than 10, and performing solid-liquid separation to obtain a solid lithium phosphate.

[0079] Example 5

[0080] In this embodiment, lithium carbonate, ferrous sulfate, manganese sulfate and sodium phosphate are used as raw materials, and sulfuric acid and sodium hydroxide are used as acid and base to adjust the pH value to prepare carbon-free lithium manganese iron phosphate (LiMn 0.6 Fe 0.4 PO4) precursor, the preparation method thereof is as follows:

[0081] S1) Use sulfuric acid to fully dissolve lithium carbonate, and use deionized water to prepare 200 L of lithium solution with a lithium ion concentration of 0.9 mol / L, and adjust its pH to less than 4 with sulfuric acid; use deionized water to prepare 200 L of manganese sulfate solution with a manganese ion concentration of 0.54 mol / L, and adjust its pH to less than 4 with sulfuric acid; use deionized water to prepare 200 L of ferrous sulfate solution with a ferrous ion concentration of 0.36 mol / L, and adjust its pH to less than 4 with sulfuric acid; use deionized water to prepare 200 L of sodium phosphate solution with a phosphate ion concentration of 0.9 mol / L, and adjust its pH to less than 4 with sulfuric acid.

[0082] S2) In a 1000 L reactor, a manganese salt solution and a ferrous salt solution are added in sequence, and after stirring evenly, a lithium salt solution and a phosphate solution are added, and after stirring and mixing evenly, a mixed solution is obtained.

[0083] S3) Slowly add sodium hydroxide solution to the reactor until the pH value of the mixed solution is 5.5, heat the reactor to 100 °C, keep the pressure in the reactor at normal pressure, and after keeping the temperature for 6 hours, the reaction is completed.

[0084] S4) Filter the mixture in the reactor, wash the filtered solid with deionized water for at least 3 times, and dry it to obtain the product LiMn 0.6 Fe 0.4 PO4 (XRD and SEM are shown in Fig. 9 and Fig.10 as shown).

[0085] S5) collecting the filtered liquid and the washing water obtained by washing the product in a stirring tank, adding phosphoric acid, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding sodium hydroxide solution until the pH value is greater than 10, performing solid-liquid separation, and the obtained solid is lithium phosphate.

[0086] Example 6

[0087] In this embodiment, lithium dihydrogen phosphate, ferrous sulfate and manganese sulfate are used as raw materials, and sulfuric acid and sodium hydroxide are used as acid and base to adjust the pH value to prepare carbon-free lithium iron manganese phosphate (LiMn 0.6 Fe 0.4 PO4) precursor, the preparation method thereof is as follows:

[0088] S1) Prepare 300 L of lithium dihydrogen phosphate solution with a lithium ion concentration of 0.8 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 300 L of manganese sulfate solution with a manganese ion concentration of 0.24 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 300 L of ferrous sulfate solution with a ferrous ion concentration of 0.16 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid.

[0089] S2) In a 1000 L reactor, add a manganese salt solution and a ferrous salt solution in sequence, stir them evenly, then add a lithium salt solution, stir and mix evenly to obtain a mixed solution.

[0090] S3) slowly add sodium hydroxide solution to the reactor until the pH value of the mixed solution reaches 6, heat the reactor to 95°C, keep the pressure in the reactor at normal pressure, and after keeping the temperature for 6 hours, the reaction is completed.

[0091] S4) Filter the mixture in the reactor, wash the filtered solid with deionized water for at least 3 times, and dry it to obtain the product LiMn 0.6 Fe 0.4 PO4 (XRD and SEM are shown in Fig.11 and Fig.12 as shown).

[0092] S5) collecting the filtered liquid and the washing water obtained by washing the product in a stirring tank, adding phosphoric acid, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding sodium hydroxide solution until the pH value is greater than 10, performing solid-liquid separation, and the obtained solid is lithium phosphate.

[0093] Example 7

[0094] In this embodiment, lithium phosphate, ferrous sulfate and manganese sulfate are used as raw materials, and sulfuric acid and sodium hydroxide are used as acid and base to adjust the pH value to prepare carbon-free lithium manganese iron phosphate (LiMn 0.6 Fe 0.4 PO4) precursor, the preparation method thereof is as follows:

[0095] S1) Prepare 300 L of lithium phosphate solution with a lithium ion concentration of 0.9 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 300 L of manganese sulfate solution with a manganese ion concentration of 0.18 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid; prepare 300 L of ferrous sulfate solution with a ferrous ion concentration of 0.12 mol / L with deionized water, and adjust its pH to less than 4 with sulfuric acid.

[0096] S2) In a 1000 L reactor, add a manganese salt solution and a ferrous salt solution in sequence, stir them evenly, then add a lithium salt solution, stir and mix evenly to obtain a mixed solution.

[0097] S3) Slowly add sodium hydroxide solution to the reactor until the pH value of the mixed solution reaches 6.2, heat the reactor to 90 °C, keep the pressure in the reactor at normal pressure, and after keeping the temperature for 6 hours, the reaction is completed.

[0098] S4) Filter the mixture in the reactor, wash the filtered solid with deionized water for at least 3 times, and dry it to obtain the product LiMn 0.6 Fe 0.4 PO4 (XRD and SEM are shown in Fig.13 and Fig.14 as shown).

[0099] S5) collecting the filtered liquid and the washing water obtained by washing the product in a stirring tank, adding phosphoric acid, and stirring until the molar ratio of lithium to phosphorus in the tank is slightly less than 3, and then adding sodium hydroxide solution until the pH value is greater than 10, performing solid-liquid separation, and the obtained solid is lithium phosphate.

[0100] Through XRD and SEM analysis of the products of Examples 1 to 7, it can be seen that the products all meet the characteristics of lithium manganese (iron) phosphate, no impurity phase is detected, and the crystal size is relatively uniform.

[0101] In addition, the products prepared in Examples 1-7 were numbered AG, and then AG was added to a carbon source, and subjected to conventional process steps such as sand milling, spray drying, sintering, and crushing to obtain a carbon-coated manganese (iron) lithium phosphate composite material, which was used as a positive electrode material to prepare a button battery, and its first charge specific capacity, first discharge specific capacity and first efficiency at 0.1 C were measured. The test temperature was 25±2 ° C. The test results are shown in Table 1:

[0102] Table 1

[0103] serial number First charge specific capacity (mAh / g) First discharge specific capacity (mAh / g) First effect (%) A 121.6 105.4 86.7 B 158.3 147.2 93.0 C 158.6 146.7 92.5 D 160.3 151.2 94.3 E 163.2 152.1 93.2 F 161.7 151.8 93.9 G 160.9 150.9 93.8

[0104] It can be seen from Table 1 that the lithium iron phosphate battery prepared using the lithium manganese (iron) phosphate positive electrode material (referring to lithium manganese phosphate positive electrode material or lithium manganese iron phosphate positive electrode material) prepared by the present invention has excellent electrical properties.

[0105] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a carbon-free phosphate positive electrode material, characterized in that: The following steps are involved: S1. preparing a phosphate solution, a lithium salt solution and a salt solution A respectively; S2. The phosphate solution, the lithium salt solution and the salt solution A in step S1 are mixed to obtain an acidic mixed solution C; S3. The mixed solution C in step S2 is stirred at room temperature, and a base is added during the stirring process to obtain a weakly acidic mixed solution D; S4. The mixed solution D in step S3 is heated and kept warm to obtain a solid-liquid mixture, the heating temperature being 90-120 ° C; thereafter the solid-liquid mixture is filtered and dried sequentially to obtain a carbon-free phosphate cathode material; The salt solution A is a manganese salt solution or a mixed solution of iron salt and manganese salt; In step S2, before mixing the phosphate solution, the lithium salt solution and the salt solution A, the lithium salt solution and the phosphate solution are first mixed, and a strong acid is added during the mixing process to obtain an acidic mixed solution B, and then the mixed solution B is mixed with the salt solution A to obtain a mixed solution C; The pH of the mixed solution D is 4.5-6.

5.

2. The method for preparing a carbon-free phosphate positive electrode material according to claim 1, characterized in that: The salt solution A is a salt solution to which a strong acid is added.

3. The method for preparing a carbon-free phosphate-based positive electrode material according to claim 2, characterized in that: The strong acid is one or more of sulfuric acid, hydrochloric acid and nitric acid.

4. The method for preparing a carbon-free phosphate positive electrode material according to claim 2, characterized in that: The alkali added in step S3 is one or both of sodium hydroxide and ammonia water.

5. The method for preparing a carbon-free phosphate-based positive electrode material according to claim 1, characterized in that: The phosphate is one or more of monoammonium phosphate, sodium phosphate, lithium phosphate, and lithium dihydrogen phosphate; The lithium salt is one or more of lithium sulfate, lithium chloride, lithium hydroxide, lithium nitrate, lithium carbonate, lithium phosphate, and lithium dihydrogen phosphate; The iron salt is one or more of ferrous sulfate, ferrous chloride, and ferrous nitrate; The manganese salt is one or more of manganese sulfate, manganese chloride and manganese nitrate.

6. The method for preparing a carbon-free phosphate positive electrode material according to claim 1, characterized in that: In the mixed solution D, the molar ratio of lithium ions, total metal ions in the salt solution A, and phosphate ions is (1-3):1:

1.

7. The method for preparing a carbon-free phosphate-based positive electrode material according to claim 1, characterized in that: After step S4, step S5 is also included, namely, adding phosphate or phosphoric acid to the mother liquor obtained by filtration in step S4, and then adjusting the pH to alkaline, precipitating and filtering to obtain lithium phosphate.