Preparation method of ammonium rhenate with controllable sulfur content and double particle size and rhenium powder

The dual-particle size ammonium rhenate with controllable sulfur content is prepared through a hierarchical freezing method, which solves the problems of rhenium powder particle size and sulfur content in the existing process, achieves efficient preparation of high-purity rhenium powder, simplifies the process and reduces costs.

CN118495593BActive Publication Date: 2024-10-18BEIJING MINING & METALLURGICAL TECH GRP CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410955747.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-18
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

In the existing preparation process of ammonium rhenate, the particle size is large and the sulfur content is high, resulting in low production efficiency of high-purity rhenium powder, high process complexity and cost, and the inability to meet the particle size requirements of rhenium powder according to different needs.

Method used

A graded freezing method is used to prepare dual-particle size ammonium rhenate with controllable sulfur content. The particle size and sulfur content of the ammonium rhenate crystals are controlled through the first freeze crystallization and liquid nitrogen freeze crystallization separation, and then reduction roasting is performed to prepare rhenium powder.

Benefits of technology

The preparation of high-purity ammonium rhenate powder with different particle size distributions is realized. The sulfur content in the rhenium powder is extremely low, which simplifies the process, reduces the production cost, and meets the particle size requirements of rhenium powder according to different needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495593B_ABST
    Figure CN118495593B_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing ammonium rhenate with controllable sulfur content and dual-particle size and rhenium powder, and relates to the field of rhenium powder preparation. The method comprises: first mixing ammonium rhenate and water to obtain a first ammonium rhenate solution; performing a first freezing crystallization on the first ammonium rhenate solution, and performing a first solid-liquid separation to obtain a first ammonium rhenate crystal and a second ammonium rhenate solution; performing a second freezing crystallization on the second ammonium rhenate solution and liquid nitrogen, and performing a second solid-liquid separation to obtain a second ammonium rhenate crystal. The present application obtains ammonium rhenate grains with different particle size distributions by graded freezing, and removes sulfur impurities in the ammonium rhenate during the freezing process. According to the subsequent industrial demand for rhenium particle size, an appropriate ammonium rhenate crystallization process can be selected to prepare high-purity ammonium rhenate powders with different particle sizes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of rhenium powder preparation, and in particular to a preparation method of ammonium rhenate with controllable sulfur content and double particle size and rhenium powder. Background Art

[0002] Rhenium is a rare refractory metal with excellent physical and chemical properties. It has very good mechanical stability at high temperature (3180℃) and no brittle critical transition temperature. It is suitable for ultra-high temperature and strong thermal shock working environment. Rhenium and its compounds also have excellent catalytic activity. Rhenium is mainly used in high-temperature turbine engine component alloys and petroleum reforming catalysts, accounting for 80% and 15% of its uses respectively. Bimetallic platinum-rhenium catalysts are used in petroleum reforming to produce high-octane hydrocarbons, and play a very important role in the production of unleaded gasoline. In addition, rhenium alloys are often used in electronic components, heating elements, mass spectrometers, metal plating, semiconductors, thermocouples and other fields.

[0003] The purity and particle size of rhenium in the application process have attracted attention. It is necessary to prepare high-purity rhenium powder and strictly control the particle size of rhenium powder. The purity and particle size of rhenium powder are directly affected by the performance of the raw material ammonium rhenate. The ammonium rhenate currently used has problems such as large particle size and high sulfur content, which leads to low mass transfer and thermal efficiency in the production process of high-purity rhenium powder and cannot meet the demand for rhenium powder. It is necessary to add multiple means in the reduction process, which not only increases the complexity of the process, but also increases the process cost. Therefore, it is necessary to improve the existing process to prepare high-purity ammonium rhenate crystals with controllable particle size and low sulfur content to meet the preparation needs of rhenium powder with different requirements.

[0004] Patent 202211226560.X discloses a method for purifying ammonium rhenate, which takes low-purity crude ammonium rhenate as a raw material, adds distilled water, stirs and heats to dissolve, and filters to obtain a supersaturated ammonium rhenate solution; the supersaturated ammonium rhenate solution is passed into a cooling crystallization reactor, and a disc turbine agitator is used for high-speed mechanical stirring, and the stirring intensity and cooling rate are controlled to cool to -10-0°C, maintain this temperature range, and continue to stir mechanically at high speed to obtain a solid-liquid mixture; the obtained solid-liquid mixture is filtered and naturally air-dried to obtain high-purity ammonium rhenate crystals with fine particles, but the preparation process of this method requires multiple recrystallizations, the process is cumbersome, and the steps are long.

[0005] Therefore, in view of this, the present invention is proposed to solve at least one of the above technical problems. Summary of the invention

[0006] The purpose of the present application is to provide a method for preparing ammonium rhenate with controllable sulfur content and double particle size and rhenium powder to solve the above problems.

[0007] To achieve the above objectives, the present application provides a first aspect of a method for preparing ammonium rhenate with controllable sulfur content and double particle size, comprising:

[0008] first mixing ammonium rhenate and water to obtain a first ammonium rhenate solution;

[0009] The first ammonium rhenate solution is subjected to a first freezing crystallization and a first solid-liquid separation to obtain first ammonium rhenate crystals and a second ammonium rhenate solution;

[0010] The second ammonium rhenate solution and liquid nitrogen are mixed for a second time to perform a second freezing crystallization, and a second solid-liquid separation is performed to obtain second ammonium rhenate crystals.

[0011] Optionally, the concentration of the first ammonium rhenate solution is 30 g / L-50 g / L.

[0012] Optionally, the method for preparing the ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0013] A. the temperature of the first ammonium rhenate solution is 20°C-40°C;

[0014] B. The temperature of the first freezing crystallization is -10°C to -4°C.

[0015] Optionally, the method for preparing the ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0016] A. stirring during the first freezing crystallization process, the stirring speed is 200 rpm / min-400 rpm / min, and the time is 0.5h-1h;

[0017] B. The first freezing crystallization is carried out in a double-layer freezing kettle, and the volume ratio of the double-layer freezing kettle and the first ammonium rhenate solution in the double-layer freezing kettle is (3-5):1.

[0018] Optionally, the method for preparing the ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0019] A. the particle size of the first ammonium rhenate crystal is 50 μm-80 μm;

[0020] B. The sulfur content of the first ammonium rhenate crystals is 2ppm-5ppm.

[0021] Optionally, the method for preparing the ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0022] A. the concentration of ammonium rhenate in the second ammonium rhenate solution is 5 g / L-20 g / L;

[0023] B. The temperature of the second ammonium rhenate solution is 5°C-10°C.

[0024] Optionally, the method for preparing the ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0025] A. The second mixing time is 5min-20min;

[0026] B. The temperature of the mixture obtained by the second mixing is -5°C to 0°C.

[0027] Optionally, the method for preparing the ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0028] A. the particle size of the second ammonium rhenate crystal is 10 μm-30 μm;

[0029] B. The sulfur content of the second ammonium rhenate crystals is less than 2 ppm.

[0030] A second aspect of the present application provides a rhenium powder, which is prepared by reduction roasting of the first ammonium rhenate crystals and the second ammonium rhenate crystals prepared by the method for preparing ammonium rhenate with controllable sulfur content and dual particle size.

[0031] Optionally, the reduction roasting is carried out at a temperature of 300°C-750°C and for a time of 2h-6h.

[0032] Compared with the prior art, the beneficial effects of this application include:

[0033] The present application provides a method for preparing ammonium rhenate with controllable sulfur content and dual-size particles, in which ammonium rhenate crystals with different particle size distributions are obtained by graded freezing, and sulfur impurities in the ammonium rhenate are removed during the freezing process. According to the subsequent industrial demand for rhenium particle size, an appropriate ammonium rhenate crystallization process can be selected to prepare high-purity ammonium rhenate powders with different particle sizes.

[0034] The rhenium powder provided in the present application can obtain ammonium rhenate crystals with different particle size distributions by graded freezing, and rhenium powder with different particle size distributions can be obtained, and the sulfur content in the rhenium powder is extremely low. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0036] Figure 1 is a scanning electron microscope image of the first ammonium rhenate crystal in Example 1;

[0037] Figure 2 is a scanning electron microscope image of the second ammonium rhenate crystal in Example 1;

[0038] Figure 3is a scanning electron microscope image of the first rhenium powder in Example 1;

[0039] Figure 4 is a scanning electron microscope image of the second rhenium powder in Example 1;

[0040] Figure 5 is a scanning electron microscope image of the ammonium rhenate crystal in Comparative Example 1;

[0041] Figure 6 This is a scanning electron microscope image of ammonium rhenate. DETAILED DESCRIPTION

[0042] As used herein:

[0043] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0044] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0045] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0046] In these examples, parts and percentages are by mass unless otherwise indicated.

[0047] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.

[0048] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0049] The first aspect of the present application provides a method for preparing ammonium rhenate with controllable sulfur content and double particle size, comprising:

[0050] first mixing ammonium rhenate and water to obtain a first ammonium rhenate solution;

[0051] The first ammonium rhenate solution is subjected to a first freezing crystallization and a first solid-liquid separation to obtain first ammonium rhenate crystals and a second ammonium rhenate solution;

[0052] The second ammonium rhenate solution and liquid nitrogen are mixed for a second time to perform a second freezing crystallization, and a second solid-liquid separation is performed to obtain second ammonium rhenate crystals.

[0053] In some embodiments, the concentration of the first ammonium rhenate solution is 30 g / L-50 g / L.

[0054] Optionally, the concentration of the first ammonium rhenate solution may be 30 g / L, 35 g / L, 40 g / L, 45 g / L, 50 g / L or any value between 30 g / L and 50 g / L.

[0055] It should be noted that when the concentration of the ammonium rhenate solution is too low, it will be difficult to remove the sulfur. Too low a concentration will make it difficult for ammonium rhenate to crystallize, and the solubility cannot reach supersaturation. The existence time of ammonium rhenate ions in the solution will increase, and the freezing time must be increased or the freezing temperature must be lowered for ammonium rhenate to precipitate. This situation will lead to an increase in the amount of sulfur attached to the ammonium rhenate crystals. When the concentration of the ammonium rhenate solution is too high, the ammonium rhenate content increases, and crystallization is likely to occur when stirring is incomplete during the freezing process, and the sulfur content attached to the large particles increases.

[0056] In some embodiments, the method for preparing ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0057] A. the temperature of the first ammonium rhenate solution is 20°C-40°C;

[0058] Optionally, the temperature of the first ammonium rhenate solution may be 20°C, 25°C, 30°C, 35°C, 40°C, or any value between 20°C and 40°C;

[0059] It should be noted that when the initial temperature of the first ammonium rhenate solution is too high, the overall time of the ammonium rhenate freezing and crystallization process is prolonged, resulting in coarse particles in the ammonium rhenate crystals; when the initial temperature of the first ammonium rhenate solution is too low, coarse particles of ammonium rhenate crystals appear before stirring and freezing are fully mixed.

[0060] B. The temperature of the first freezing crystallization is -10°C to -4°C.

[0061] Optionally, the temperature of the first freezing crystallization can be minus 10°C, minus 9°C, minus 8°C, minus 7°C, minus 6°C, minus 5°C, minus 4°C, or any value between minus 10°C and minus 4°C.

[0062] It should be noted that sulfur mostly exists in the form of sulfate in the ammonium rhenate solution. There is a large solubility gap between sulfate and rhenate. A supersaturated solution can be formed by adjusting the temperature, and the ammonium rhenate can be precipitated by using the solubility gap, while the sulfate remains in the liquid. However, during the crystallization process of ammonium rhenate, there is a certain surface adsorption on the crystal surface, and some sulfate will be adsorbed and still exist in the ammonium rhenate crystal. Therefore, when directly frozen, the crystals continue to grow into large ammonium rhenate particles, and a certain amount of sulfate is adsorbed on the crystal surface. During the precipitation process, some sulfate adsorbed on the surface of the ammonium rhenate crystals are not replaced in time, and are covered by the ammonium rhenate ions deposited later. Therefore, some sulfur impurities are trapped inside the ammonium rhenate precipitate, resulting in an excessively high sulfur concentration in the ammonium rhenate, far greater than 5ppm.

[0063] In some embodiments, the method for preparing ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0064] A. stirring during the first freezing crystallization process, the stirring speed is 200 rpm / min-400 rpm / min, and the time is 0.5h-1h;

[0065] Optionally, the stirring speed may be 200rpm / min, 250rpm / min, 300rpm / min, 350rpm / min, 400rpm / min or any value between 200rpm / min-400rpm / min, and the time may be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h or any value between 0.5h-1h;

[0066] It should be noted that the ammonium rhenate prepared by freezing and stirring has a more uniform morphology, showing a typical hexagonal cubic bipyramidal crystal morphology of ammonium rhenate, which proves that the ammonium rhenate crystals grow gradually during rotary freezing, and stirring makes the growth process less affected by the crystallized ammonium rhenate, resulting in a finer particle size.

[0067] B. The first freezing crystallization is carried out in a double-layer freezing kettle, and the volume ratio of the double-layer freezing kettle and the first ammonium rhenate solution in the double-layer freezing kettle is (3-5):1.

[0068] Optionally, the volume ratio of the internal accommodating volume of the double-layer freezing kettle to the first ammonium rhenate solution in the double-layer freezing kettle can be 3:1, 3.5:1, 4:1, 4.5:1, 5:1 or any value between (3-5):1.

[0069] It should be noted that when the volume ratio of the double-layer freezing kettle to the first ammonium rhenate solution is (3-5):1, and the rotation speed is controlled within the range of 200rpm / min-400rpm / min, during the rotary freezing process, the ammonium rhenate solution can fully exchange heat in the freezing kettle, thereby achieving uniform crystal growth and small particle size, and the adsorbed sulfate ions are quickly desorbed under the action of stirring.

[0070] In some embodiments, the method for preparing ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0071] A. the particle size of the first ammonium rhenate crystal is 50 μm-80 μm;

[0072] Optionally, the particle size of the first ammonium rhenate crystals may be 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, or any value between 50 μm and 80 μm;

[0073] B. The sulfur content of the first ammonium rhenate crystals is 2ppm-5ppm.

[0074] Optionally, the sulfur content of the first ammonium rhenate crystals may be 2 ppm, 2.5 ppm, 3 ppm, 3.5 ppm, 4 ppm, 4.5 ppm, 5 ppm or any value between 2 ppm and 5 ppm.

[0075] In some embodiments, the method for preparing ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0076] A. the concentration of ammonium rhenate in the second ammonium rhenate solution is 5 g / L-20 g / L;

[0077] Optionally, the concentration of ammonium rhenate in the second ammonium rhenate solution may be 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, 20 g / L or any value between 5 g / L and 20 g / L;

[0078] It should be noted that when the concentration of the second ammonium rhenate is too high, the ammonium rhenate molecules contact each other and grow continuously, and the ammonium rhenate particles are larger in size; when the concentration of the second ammonium rhenate is too low, the liquid nitrogen is added slowly during rapid cooling, and it is not easy to form a supersaturated solution for precipitation, and the liquid nitrogen supercooled solution will freeze. It is necessary to wait for the solution to change from a frozen state to a solid-liquid mixed state before filtering, prolonging the freezing time and making the grains larger;

[0079] B. The temperature of the second ammonium rhenate solution is 5°C-10°C.

[0080] Optionally, the temperature of the second ammonium rhenate solution may be 5°C, 6°C, 7°C, 8°C, 9°C, 10°C or any value between 5°C and 10°C.

[0081] It should be noted that when the temperature of the second ammonium rhenate solution is too high, the quenching time is prolonged and the size of the ammonium rhenate grains increases; when the temperature of the second ammonium rhenate solution is too low, ammonium rhenate crystals will precipitate without quenching.

[0082] In some embodiments, the method for preparing ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0083] A. The second mixing time is 5min-20min;

[0084] Optionally, the second mixing time can be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min or any value between 5 min and 20 min;

[0085] B. The temperature of the mixture obtained by the second mixing is -5°C to 0°C.

[0086] Optionally, the temperature of the mixture obtained by the second mixing may be minus 5°C, minus 4°C, minus 3°C, minus 2°C, minus 1°C, 0°C or any value between minus 5°C and 0°C.

[0087] In some embodiments, the method for preparing ammonium rhenate with controllable sulfur content and dual particle size meets at least one of the following conditions:

[0088] A. the particle size of the second ammonium rhenate crystal is 10 μm-30 μm;

[0089] Optionally, the particle size of the second ammonium rhenate crystals may be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, or any value between 10 μm and 30 μm;

[0090] It should be noted that the ammonium rhenate prepared by rapid freezing with liquid nitrogen in the present application shows a dispersed small block morphology, no ammonium rhenate agglomeration morphology exists, and the particle size is relatively fine. This is because the ammonium rhenate crystallizes rapidly during the rapid freezing process, the crystallization process is relatively fast, and the crystal growth process is destroyed, forming small-sized ammonium rhenate crystals. Among them, if the concentration, temperature, etc. are not within the range, the particle size will be coarse.

[0091] B. The sulfur content of the second ammonium rhenate crystals is less than 2 ppm.

[0092] Optionally, the sulfur content of the second ammonium rhenate crystals may be 0.01 ppm, 0.1 ppm, 1 ppm, or any value less than 2 ppm.

[0093] It should be noted that when the second ammonium rhenate solution is cooled by liquid nitrogen, by controlling the concentration of ammonium rhenate within the range of 5g / L-20g / L and the initial temperature within the range of 5℃-10℃, and lowering the temperature to -5℃-0℃ within 5min-20min, the solubility of ammonium rhenate can be further reduced under the conditions of extreme freezing, and the difference with the solubility of sulfate is greater, and ammonium rhenate rapidly nucleates and precipitates, reducing surface adsorption, and the S content is <2ppm; among them, if the concentration of ammonium rhenate, initial temperature, mixing cooling time and temperature reached are too low or too high, the S content will be >2ppm.

[0094] A second aspect of the present application provides a rhenium powder, which is prepared by reduction roasting of the first ammonium rhenate crystals and the second ammonium rhenate crystals prepared by the method for preparing ammonium rhenate with controllable sulfur content and dual particle size.

[0095] It should be noted that the particle size of the rhenium powder prepared from the first ammonium rhenate crystal is 40 μm-50 μm, and the particle size of the rhenium powder prepared from the second ammonium rhenate crystal is 15 μm-25 μm.

[0096] In some embodiments, the reduction roasting is performed at a temperature of 300° C. to 750° C. for a time of 2 h to 6 h.

[0097] Optionally, the temperature of the reduction roasting can be 300℃, 350℃, 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃ or any value between 300℃-750℃, and the time can be 2h, 3h, 4h, 5h, 6h or any value between 2h-6h.

[0098] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0099] Example 1

[0100] This embodiment provides a method for preparing ammonium rhenate with controllable sulfur content and double particle size, comprising:

[0101] Mixing ammonium rhenate and water to obtain a 50 g / L ammonium rhenate solution, wherein the temperature of the ammonium rhenate solution is 35° C.;

[0102] The ammonium rhenate solution is placed in a double-layer freezing kettle at -10°C, the volume ratio of the double-layer freezing kettle to the ammonium rhenate solution in the kettle is 4:1, the ammonium rhenate solution is frozen and crystallized by a stirring freezing method, the stirring time is 0.5h, the rotation speed is 300rpm / min, and the first ammonium rhenate crystals and the filtered solution are obtained by filtration;

[0103] The first ammonium rhenate crystal has a particle size of 60 μm and a sulfur content of 4.5 ppm;

[0104] The scanning electron microscope image of the first ammonium rhenate crystal is as follows Figure 1 As shown;

[0105] The concentration of ammonium rhenate in the filtered solution is 15 g / L, and the temperature of the solution is 8° C. The filtered solution is poured into liquid nitrogen in batches for mixing. The total time for pouring liquid nitrogen in batches is 10 minutes. When the temperature of the solution is minus 2° C., the addition of liquid nitrogen is stopped, and solid-liquid separation is performed to obtain a second ammonium rhenate crystal;

[0106] The second ammonium rhenate crystal has a particle size of 23 μm and a sulfur content of less than 2 ppm;

[0107] The scanning electron microscope image of the second ammonium rhenate crystal is as follows Figure 2 shown.

[0108] This embodiment also provides a rhenium powder, including: a first rhenium powder prepared by reduction roasting of the first ammonium rhenate crystal, the reduction roasting temperature is 450° C., and the time is 4 hours;

[0109] The particle size of the first rhenium powder is 40 μm;

[0110] The scanning electron microscope image of the first rhenium powder is as follows Figure 3 shown.

[0111] This embodiment also provides a rhenium powder, comprising: preparing a second rhenium powder by reduction roasting the second ammonium rhenate crystal, wherein the temperature of the reduction roasting is 550° C. and the time is 5 hours;

[0112] The particle size of the second rhenium powder is 20 μm;

[0113] The scanning electron microscope image of the second rhenium powder is as follows Figure 4 shown.

[0114] Example 2

[0115] This embodiment provides a method for preparing ammonium rhenate with controllable sulfur content and double particle size, comprising:

[0116] Mixing ammonium rhenate and water to obtain a 30 g / L ammonium rhenate solution, wherein the temperature of the ammonium rhenate solution is 20° C.;

[0117] The ammonium rhenate solution is placed in a double-layer freezing kettle at minus 4°C, the volume ratio of the double-layer freezing kettle to the ammonium rhenate solution in the kettle is 3:1, the ammonium rhenate solution is frozen and crystallized by a stirring freezing method, the stirring time is 0.7h, the rotation speed is 200rpm / min, and the first ammonium rhenate crystals and the filtered solution are obtained by filtration;

[0118] The first ammonium rhenate crystal has a particle size of 70 μm and a sulfur content of 4 ppm;

[0119] The concentration of ammonium rhenate in the filtered solution is 20 g / L, and the temperature of the solution is 5° C. The filtered solution is poured into liquid nitrogen in batches for mixing. The total time for pouring liquid nitrogen in batches is 8 minutes. When the temperature of the solution is minus 4° C., the addition of liquid nitrogen is stopped, and solid-liquid separation is performed to obtain a second ammonium rhenate crystal;

[0120] The second ammonium rhenate crystal has a particle size of 15 μm and a sulfur content of less than 2 ppm.

[0121] This embodiment also provides a rhenium powder, including: a first rhenium powder prepared by reduction roasting of the first ammonium rhenate crystal, the reduction roasting temperature is 400° C., and the time is 2 hours;

[0122] The particle size of the first rhenium powder is 45 μm.

[0123] This embodiment also provides a rhenium powder, comprising: preparing a second rhenium powder by reduction roasting the second ammonium rhenate crystal, the reduction roasting temperature is 650° C., and the time is 3 hours;

[0124] The particle size of the second rhenium powder is 18 μm.

[0125] Example 3

[0126] This embodiment provides a method for preparing ammonium rhenate with controllable sulfur content and double particle size, comprising:

[0127] Mixing ammonium rhenate and water to obtain a 40 g / L ammonium rhenate solution, wherein the temperature of the ammonium rhenate solution is 28° C.;

[0128] The ammonium rhenate solution is placed in a double-layer freezing kettle at minus 7°C, the volume ratio of the double-layer freezing kettle to the ammonium rhenate solution in the kettle is 4.5:1, the ammonium rhenate solution is frozen and crystallized by a stirring freezing method, the stirring time is 1 hour, the rotation speed is 400 rpm / min, and the first ammonium rhenate crystals and the filtered solution are obtained by filtration;

[0129] The first ammonium rhenate crystal has a particle size of 75 μm and a sulfur content of 4.8 ppm;

[0130] The concentration of ammonium rhenate in the filtered solution is 5 g / L, and the temperature of the solution is 8° C. The filtered solution is poured into liquid nitrogen in batches for mixing. The total time for pouring liquid nitrogen in batches is 15 minutes. When the temperature of the solution is 0° C., the addition of liquid nitrogen is stopped, and solid-liquid separation is performed to obtain a second ammonium rhenate crystal.

[0131] The second ammonium rhenate crystal has a particle size of 28 μm and a sulfur content of less than 2 ppm.

[0132] This embodiment also provides a rhenium powder, including: a first rhenium powder prepared by reduction roasting of the first ammonium rhenate crystal, the reduction roasting temperature is 500° C., and the time is 4.5 hours;

[0133] The particle size of the first rhenium powder is 48 μm.

[0134] This embodiment also provides a rhenium powder, comprising: preparing a second rhenium powder by reduction roasting the second ammonium rhenate crystal, wherein the temperature of the reduction roasting is 700° C. and the time is 6 hours;

[0135] The particle size of the second rhenium powder is 24 μm.

[0136] Comparative Example 1

[0137] This comparative example provides a method for preparing ammonium rhenate, comprising:

[0138] A 50 g / L ammonium rhenate aqueous solution was placed in a -10°C freezer and frozen to 0°C for 6 hours, and after solid-liquid separation, dried to obtain ammonium rhenate crystals;

[0139] The ammonium rhenate crystal was ground and then tested by scanning electron microscopy. The specific test results are as follows: Figure 5 shown.

[0140] The ammonium rhenate crystals have a particle size of 250 μm and a sulfur content of 30 ppm.

[0141] Comparative Example 2

[0142] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that the concentration of the ammonium rhenate solution in this comparative example is 20 g / L, and other conditions are consistent with those in Example 1;

[0143] The obtained first ammonium rhenate crystals have a particle size of 90 μm and a sulfur content of 15 ppm;

[0144] The obtained second ammonium rhenate crystals had a particle size of 40 μm and a sulfur content of 5 ppm.

[0145] Comparative Example 3

[0146] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that the concentration of the ammonium rhenate solution in this comparative example is 100 g / L, and other conditions are consistent with those in Example 1;

[0147] The obtained first ammonium rhenate crystals have a particle size of 120 μm and a sulfur content of 30 ppm;

[0148] The obtained second ammonium rhenate crystals had a particle size of 80 μm and a sulfur content of 10 ppm.

[0149] Comparative Example 4

[0150] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that the temperature of the ammonium rhenate solution in this comparative example is 60° C., and other conditions are consistent with those in Example 1;

[0151] The obtained first ammonium rhenate crystals had a particle size of 105 μm and a sulfur content of 24 ppm;

[0152] The obtained second ammonium rhenate crystals had a particle size of 65 μm and a sulfur content of 8 ppm.

[0153] Comparative Example 5

[0154] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that the temperature of the ammonium rhenate solution in this comparative example is 15° C., and other conditions are consistent with those in Example 1;

[0155] The obtained first ammonium rhenate crystals had a particle size of 170 μm and a sulfur content of 18 ppm;

[0156] The obtained second ammonium rhenate crystals had a particle size of 45 μm and a sulfur content of 9 ppm.

[0157] Comparative Example 6

[0158] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that: the ammonium rhenate solution in this comparative example is placed in a double-layer freezing kettle, the volume ratio of the double-layer freezing kettle to the ammonium rhenate solution is 8:1, and other conditions are consistent with Example 1;

[0159] The obtained first ammonium rhenate crystals had a particle size of 88 μm and a sulfur content of 10 ppm;

[0160] The obtained second ammonium rhenate crystals had a particle size of 35 μm and a sulfur content of 3 ppm.

[0161] Comparative Example 7

[0162] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that: the ammonium rhenate solution in this comparative example is placed in a double-layer freezing kettle, the volume ratio of the double-layer freezing kettle to the ammonium rhenate solution is 1:1, and other conditions are consistent with Example 1;

[0163] The obtained first ammonium rhenate crystals had a particle size of 130 μm and a sulfur content of 35 ppm;

[0164] The obtained second ammonium rhenate crystals had a particle size of 60 μm and a sulfur content of 12 ppm.

[0165] Comparative Example 8

[0166] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that the temperature of the filtered solution in this comparative example is 20° C., and other conditions are consistent with those in Example 1;

[0167] The obtained first ammonium rhenate crystals had a particle size of 80 μm and a sulfur content of 4.9 ppm;

[0168] The obtained second ammonium rhenate crystals had a particle size of 55 μm and a sulfur content of 6.5 ppm.

[0169] Comparative Example 9

[0170] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that the temperature of the filtered solution in this comparative example is 3° C., and other conditions are consistent with those in Example 1;

[0171] The obtained first ammonium rhenate crystals had a particle size of 78 μm and a sulfur content of 4.5 ppm;

[0172] The obtained second ammonium rhenate crystals had a particle size of 43 μm and a sulfur content of 2.8 ppm.

[0173] Comparative Example 10

[0174] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that: in this comparative example, liquid nitrogen is directly mixed with the filtered solution, and other conditions are consistent with Example 1;

[0175] The obtained first ammonium rhenate crystals have a particle size of 80 μm and a sulfur content of 5 ppm;

[0176] The obtained second ammonium rhenate crystals had a particle size of 58 μm and a sulfur content of 4.8 ppm.

[0177] Comparative Example 11

[0178] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that: in this comparative example, liquid nitrogen is directly mixed with the filtered solution, the solution temperature is 2° C., and other conditions are consistent with Example 1;

[0179] The obtained first ammonium rhenate crystals had a particle size of 79 μm and a sulfur content of 4.8 ppm;

[0180] The obtained second ammonium rhenate crystals had a particle size of 49 μm and a sulfur content of 6.2 ppm.

[0181] Comparative Example 12

[0182] This comparative example provides a method for preparing ammonium rhenate, which is different from Example 1 in that: in this comparative example, liquid nitrogen is directly mixed with the filtered solution, and the solution temperature is minus 10° C., and other conditions are consistent with Example 1;

[0183] The obtained first ammonium rhenate crystals had a particle size of 78 μm and a sulfur content of 4.5 ppm;

[0184] The obtained second ammonium rhenate crystals had a particle size of 39 μm and a sulfur content of 4.2 ppm.

[0185] The present application conducted a scanning electron microscope test on the ammonium rhenate used in the above examples and comparative examples. The specific test results are as follows: Figure 6 shown.

[0186] It can be seen from the above embodiments and comparative examples that comparative example 1 is an ammonium rhenate crystal prepared by direct freezing, and the crystal morphology is mostly irregular blocks, and a larger block structure appears. This shows that the ammonium rhenate prepared by direct freezing is not stirred in the liquid, and the ammonium rhenate crystals crystallize at the bottom, forming crystal nuclei and growing continuously, and the ammonium rhenate in the adsorption solution forms crystals on its surface.

[0187] It can be seen from Comparative Examples 2-3 that when the concentration of the ammonium rhenate solution is not within the range specified in the present application, the particle size of the first ammonium rhenate crystal and the second ammonium rhenate crystal is larger and the sulfur content is higher. This is because when the concentration of ammonium rhenate is too high, the ammonium rhenate molecules contact each other and grow continuously, resulting in larger particles of ammonium rhenate. When the concentration of ammonium rhenate is too low, liquid nitrogen is added during rapid cooling, the crystallization is slow, and it is not easy to form a supersaturated solution to precipitate, thereby prolonging the freezing time and making the grains larger.

[0188] It can be seen from Comparative Examples 4-5 that when the temperature of the ammonium rhenate solution is not within the range specified in the present application, the particle size of the first ammonium rhenate crystal and the second ammonium rhenate crystal is larger and the sulfur content is higher. This is because when the initial temperature is too high, the overall time of the ammonium rhenate freezing crystallization process is prolonged, resulting in coarse particles in the ammonium rhenate crystals; when the initial temperature is too low, coarse particles of ammonium rhenate crystals appear before stirring and freezing are fully mixed.

[0189] It can be seen from Comparative Examples 6-7 that when the volume ratio of the double-layer freezing kettle and the ammonium rhenate solution is not within the range of (3-5):1, during the rotary freezing process, the ammonium rhenate solution may not fully exchange heat in the freezing kettle, and the crystal growth is uneven, resulting in a larger particle size. The adsorbed sulfate ions desorb slowly under the action of stirring, resulting in the first ammonium rhenate crystals and the second ammonium rhenate crystals having a larger particle size and a higher sulfur content.

[0190] It can be seen from Comparative Examples 8-9 that when the temperature of the filtered solution is not 5°C-10°C, when the temperature of the second ammonium rhenate solution is too high, the quenching time is prolonged and the ammonium rhenate grain size increases; when the temperature of the second ammonium rhenate solution is too low, ammonium rhenate crystals will precipitate without quenching, resulting in a larger particle size of the second ammonium rhenate crystals and a higher sulfur content.

[0191] It can be seen from Comparative Example 10 that when liquid nitrogen is directly mixed with the filtered solution, part of the solution is rapidly crystallized during the rapid freezing process, resulting in a larger particle size of the second ammonium rhenate crystals and a higher sulfur content.

[0192] It can be seen from Comparative Examples 11-12 that when the temperature of the mixture obtained by mixing liquid nitrogen with the filtered solution is not within the range of -5°C-0°C, the temperature is higher than zero, and the crystallization time of the ammonium rhenate solution is prolonged during the extreme freezing process, resulting in a larger particle size of the second ammonium rhenate crystals and a higher sulfur content; when the temperature is too low, the liquid nitrogen causes the ammonium rhenate solution to form ice cubes, which need to be filtered only when the ice cubes are dissolved into a solid-liquid mixture. The ammonium rhenate crystals stay in the solution for a longer time, resulting in a larger particle size of the second ammonium rhenate crystals and a higher sulfur content.

[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0194] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing ammonium rhenate with controllable sulfur content and double particle size, characterized in that: include: first mixing ammonium rhenate and water to obtain a first ammonium rhenate solution; The first ammonium rhenate solution is subjected to a first freezing crystallization and a first solid-liquid separation to obtain first ammonium rhenate crystals and a second ammonium rhenate solution; The second ammonium rhenate solution and liquid nitrogen are mixed for a second time to perform a second freezing crystallization, and a second solid-liquid separation is performed to obtain second ammonium rhenate crystals; the concentration of the first ammonium rhenate solution is 30 g / L-50 g / L; The temperature of the first ammonium rhenate solution is 20°C-40°C; The temperature of the first freezing crystallization is minus 10°C to minus 4°C; The concentration of ammonium rhenate in the second ammonium rhenate solution is 5 g / L-20 g / L; The temperature of the second ammonium rhenate solution is 5°C-10°C; The temperature of the mixture obtained by the second mixing is -5°C to 0°C; stirring is performed during the first freezing crystallization process, the stirring speed is 200rpm / min to 400rpm / min, and the time is 0.5h to 1h; The first freezing crystallization is carried out in a double-layer freezing kettle, and the volume ratio of the double-layer freezing kettle to the first ammonium rhenate solution in the double-layer freezing kettle is 3-5:

1.

2. The method for preparing ammonium rhenate with controllable sulfur content and double particle size according to claim 1, characterized in that: At least one of the following conditions is met: A. the particle size of the first ammonium rhenate crystal is 50 μm-80 μm; B. The sulfur content of the first ammonium rhenate crystals is 2ppm-5ppm.

3. The method for preparing ammonium rhenate with controllable sulfur content and double particle size according to claim 1, characterized in that: The second mixing time is 5 min-20 min.

4. The method for preparing ammonium rhenate with controllable sulfur content and double particle size according to any one of claims 1 to 3, characterized in that: At least one of the following conditions is met: A. the particle size of the second ammonium rhenate crystal is 10 μm-30 μm; B. The sulfur content of the second ammonium rhenate crystals is less than 2 ppm.

Citation Information

Patent Citations

  • A high-purity ammonium perrylate and its preparation method

    CN115611325B

  • Method for preparing fine-particle crystal ammonium rhenate

    CN116282185A

  • Modification method of ammonium rhenate and nearly spherical rhenium powder

    CN117105278A