Application of red mud as raw material for preparing porcelain clay
By mixing red mud with an acid solution and performing multi-step treatment, including filtration, air drying and iron removal, the problem of insufficient material utilization in red mud is solved, and porcelain clay with excellent performance is produced, which reduces waste slag and wastewater. Improve the utilization efficiency of red mud.
Patent Information
- Application Number
- CN202410706666.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-03
AI Technical Summary
The prior art is difficult to effectively utilize most of the substances in red mud, which makes it difficult to solve the problems of waste slag and wastewater.
The red mud is mixed with the acid solution, and after reaction, the filter is pressed, air is pressed, filtered again, and dried and burned again. Finally, the iron removal treatment is carried out to produce porcelain clay with excellent performance, reducing waste slag and wastewater.
The utilization of most substances in red mud has been achieved, and porcelain clay with excellent performance has been produced, with very little waste residue and wastewater, which meets the requirements of porcelain clay and improves the utilization efficiency of red mud.
Smart Images

Figure BDA0004872775260000051 
Figure BDA0004872775260000061 
Figure BDA0004872775260000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste utilization, and in particular to the application of red mud as a raw material for preparing porcelain clay. Background Art
[0002] The production of alumina produces a large amount of waste slag, with more than 100 million tons produced each year nationwide. The waste slag has a high iron content and is red in color, so it is called red mud. The main components of red mud are aluminum oxide, silicon oxide, iron oxide, titanium oxide, calcium oxide, sodium oxide, potassium oxide, etc. It is imperative to make use of red mud and turn waste into treasure. There are roughly two methods for utilizing red mud. One is to extract substances with higher value, such as titanium dioxide, or certain rare metals, to achieve economic profits. But the problem is that this method still produces a lot of waste and is difficult to implement in practice. The second is to utilize most of the substances in the red mud, producing very little waste slag and wastewater. This is a more ideal way. But how to utilize it is still a topic that has been studied in this field. Summary of the invention
[0003] In view of this, the technical problem to be solved by the present invention is to provide an application of red mud as a raw material for preparing porcelain clay. The present invention can utilize most of the substances in the red mud to produce porcelain clay with better performance, and produces very little waste residue and wastewater.
[0004] The invention provides an application of red mud as a raw material for preparing porcelain clay.
[0005] The present invention also provides a method for preparing porcelain clay, comprising the following steps:
[0006] A) mixing red mud and an acid solution, reacting to obtain a salt solution with a pH value of 4 to 6.8;
[0007] B) filtering the solution obtained in step A) to control the water content to be no more than 50% by weight; then introducing compressed air to dry the solution;
[0008] C) Mixing the air-dried solid with water and filtering again;
[0009] D) drying and burning the solid obtained after the filter pressing in step C);
[0010] E) removing iron from the material calcined in step D) to obtain porcelain clay.
[0011] Preferably, in step A), in the red mud, the mass content of Na2O is 6% to 10%, the mass content of Al2O3 is 22% to 27%, the mass content of SiO2 is 20% to 25%, the mass content of Fe2O3 is 7% to 12%, the mass content of TiO2 is 2% to 7%, the mass content of CaO is 11% to 16%, and the mass content of K2O is 1% to 2%; the Ca / S of the red mud is 0.3 to 0.8:1; and the N / S of the red mud is 0.1 to 0.6:1.
[0012] Preferably, in step A), the acid in the acid solution comprises at least one of hydrochloric acid, oxalic acid, phosphoric acid and sulfuric acid;
[0013] The mass concentration of the acid solution is 2% to 12%.
[0014] Preferably, in step A), the mass ratio of the acid solution to the red mud is 6 to 12:1;
[0015] The mass concentration of soluble salt in the salt solution is 0.5% to 1.2%.
[0016] Preferably, in step B), the amount of compressed air is 4-30 kg / cm 2 ;
[0017] The mass content of soluble salt in the filtrate after the filter pressing is 0.5% to 1.2%.
[0018] Preferably, in step C), the mass ratio of the air-dried solid to water is 1:5-10;
[0019] In the mixed solution, the mass content of soluble salt is 0.065% to 0.14%.
[0020] Preferably, in step C), the mass content of water in the solid after the second filter pressing is ≤50%;
[0021] The mass content of soluble salt in the filtrate after the second filtration is 0.07% to 0.15%.
[0022] Preferably, in step D), the drying temperature is 120-150° C.; the moisture content of the solid after drying is 1%-10%.
[0023] Preferably, in step D), the calcination temperature is 600-1200° C. and the calcination time is 2 min-2 h.
[0024] Preferably, in step E), after iron removal, the iron content of the obtained porcelain clay is 2.5% to 3.5%.
[0025] The present invention provides an application of red mud as a raw material for preparing porcelain clay. Specifically, the preparation method of porcelain clay includes the following steps: A) mixing red mud and an acid solution, reacting to obtain a salt solution with a pH value of 4 to 6.8; B) filtering the solution obtained in step A) to control the mass content of water to be no more than 50%; then introducing compressed air to air dry; C) mixing the solid after air drying with water and filtering again; D) drying and calcining the solid after filtration in step C); E) removing iron from the material after calcination in step D) to obtain porcelain clay. The applicant has found through research that by treating red mud according to the above steps, most of the substances in the red mud can be utilized to obtain porcelain clay with better performance, and very little waste residue and wastewater are generated. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The particle size distribution diagram of the porcelain clay obtained in Example 1 of the present invention;
[0027] Figure 2 This is the particle size distribution diagram of the porcelain clay obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The invention provides an application of red mud as a raw material for preparing porcelain clay.
[0030] The present invention also provides a method for preparing porcelain clay, comprising the following steps:
[0031] A) mixing red mud and an acid solution, reacting to obtain a salt solution with a pH value of 4 to 6.8;
[0032] B) filtering the solution obtained in step A) to control the water content to be no more than 50% by weight; then introducing compressed air to dry the solution;
[0033] C) Mixing the air-dried solid with water and filtering again;
[0034] D) drying and burning the solid obtained after the filter pressing in step C);
[0035] E) removing iron from the material calcined in step D) to obtain porcelain clay.
[0036] In step A):
[0037] The red mud and the acid solution are mixed and reacted to obtain a salt solution with a pH value of 4 to 6.8.
[0038] In certain embodiments of the present invention, in the red mud, the mass content of Na2O is 6% to 10%, the mass content of Al2O3 is 22% to 27%, the mass content of SiO2 is 20% to 25%, the mass content of Fe2O3 is 7% to 12%, the mass content of TiO2 is 2% to 7%, the mass content of CaO is 11% to 16%, and the mass content of K2O is 1% to 2%. The Ca / S (mass ratio) of the red mud is 0.3 to 0.8:1. The N / S (mass ratio) of the red mud is 0.1 to 0.6:1. The water content of the red mud is 10% to 60%, for example, 39.9%.
[0039] In certain embodiments of the present invention, the acid in the acid solution includes at least one of hydrochloric acid, oxalic acid, phosphoric acid and sulfuric acid. The mass concentration of the acid solution is 2% to 12%, such as 2%.
[0040] The mass ratio of the acid solution to the red mud is 6 to 12:1, such as 8:1 or 6:1.
[0041] After mixing water, red mud and acid solution, the sodium oxide in the red mud reacts with the acid to generate soluble salt. At this time, the red mud is completely dispersed in the solution and is in a slurry state. The mass concentration of soluble salt in the obtained salt solution is 0.5% to 1.2%, such as 0.8% or 0.79%. Specifically, the pH value of the salt solution is 5.
[0042] The reaction temperature is 2-40°C, such as 35°C, 20°C; the reaction time is 0.5-5h, such as 1h, 3h.
[0043] In step B):
[0044] The solution obtained in step A) is filtered to control the mass content of water in the filter cake to be no higher than 50%; and then compressed air is introduced to perform air drying.
[0045] The filtration is carried out in a plate and frame filter press. In certain embodiments of the present invention, the mass content of water is controlled to be less than 40%.
[0046] In some embodiments of the present invention, the amount of compressed air is 4-30 kg / cm 2 , for example 20kg / cm 2 , 10kg / cm 2 .
[0047] In certain embodiments of the present invention, the mass content of soluble salt in the filtrate after the filter press is 0.5% to 1.2%, such as 1.02% or 0.99%. The mass content of calcium chloride in the filtrate after the filter press is 0.01% to 0.12%, such as 0.01% or 0.096%.
[0048] In certain embodiments of the present invention, after the filter pressing, the method further comprises: removing calcium chloride in the filtrate and then performing reverse osmosis treatment.
[0049] Methods for removing calcium chloride from the filtrate include:
[0050] The calcium chloride content in the filtrate is determined by a calcium ion detector, and sodium carbonate is added to generate calcium carbonate precipitate and sodium chloride. The upper clear water is subjected to reverse osmosis treatment.
[0051] The molar ratio of the added sodium carbonate to the calcium chloride in the filtrate is 1:1.
[0052] After removing the calcium chloride in the filtrate, the mass content of calcium chloride in the filtrate is ≤400ppm, for example, 20ppm.
[0053] After the reverse osmosis treatment, the mass content of soluble salts in the produced water is ≤150ppm, such as 100ppm, 150ppm. The produced water after reverse osmosis can be reused in step C) and mixed with the solids after air drying. The mass content of soluble salts in the concentrated water after reverse osmosis is 5% to 12%, which can be used for other purposes.
[0054] In step C):
[0055] The air-dried solid is mixed with water and filtered again.
[0056] In certain embodiments of the present invention, the mass ratio of the air-dried solid to water is 1:5-10, such as 1:6. The mass content of soluble salt in the mixed solution is 0.065%-0.14%, such as 0.09% or 0.11%.
[0057] The present invention mixes the air-dried solid with water to further remove soluble salts.
[0058] In certain embodiments of the present invention, the mass content of water in the solid after the second filter pressing is ≤50%.
[0059] In certain embodiments of the present invention, the mass content of soluble salt in the filtrate after the second filter pressing is 0.07% to 0.15%, such as 0.15% or 0.14%. The filtrate after the second filter pressing can be reused in step A).
[0060] In step D):
[0061] The solid after the filter pressing in step C) is dried and calcined.
[0062] In some embodiments of the present invention, the drying temperature is 120-150° C., such as 130° C. The moisture content of the solid after drying is 1%-10%, such as 5.2%.
[0063] After the drying, the method further comprises: crushing, wherein the particle size of the crushed particles does not exceed 100 μm.
[0064] In certain embodiments of the present invention, the burning temperature is 600-1200° C., such as 1000° C., and the burning time is 2 min-2 h, such as 1 h.
[0065] In step E):
[0066] The material after calcination in step D) is subjected to iron removal to obtain porcelain clay.
[0067] The present invention has no particular limitation on the method for removing iron. In certain embodiments of the present invention, the method for removing iron comprises:
[0068] The material is blown into a space between several cylindrical magnetic bars by air flow to remove iron.
[0069] The material is blown into a plurality of cylindrical magnetic bars by air flow, and the material with strong magnetism is attracted by the magnetic bars, while the material with no magnetism or weak magnetism is blown away by the air flow, thereby separating the two.
[0070] After iron removal, the iron content of the obtained porcelain clay is 2.5% to 3.5%, for example 2.9%.
[0071] In certain embodiments of the present invention, in the porcelain clay, the mass content of Al2O3 is 33% to 34%, the mass content of SiO2 is 29% to 32%, the mass content of Fe2O3 is 9% to 11%, the mass content of TiO2 is 6% to 7%, the mass content of CaO is 6% to 8%, and the mass content of Na2O is 0.6% to 0.7%.
[0072] In order to further illustrate the present invention, the application of red mud provided by the present invention as a raw material for preparing porcelain clay is described in detail below in combination with the examples, but it should not be construed as limiting the scope of protection of the present invention.
[0073] The raw materials used in the following examples are all commercially available products.
[0074] Example 1
[0075] Red mud was taken from a place in Shanxi, and its water content was 39.9%.
[0076] Some components in the red mud are shown in Table 1.
[0077] Table 1 Some components in red mud
[0078]
[0079]
[0080] Preparation of porcelain clay:
[0081] 1) In a circular storage tank, add 96 tons of an acid solution with a mass concentration of 2% (a mixed solution of hydrochloric acid and phosphoric acid) and 12 tons of red mud, and react at 35° C. for 1 hour to obtain a salt solution with a pH value of 5; the mass concentration of soluble salt in the salt solution is 0.8%;
[0082] 2) The salt solution is sent to a plate-frame filter press for filtration, and the moisture content of the filter cake is controlled to be 50% by mass; after the filtration is completed, compressed air is introduced to dry the filter cake; the amount of compressed air used is 20 kg / cm 2 The mass content of soluble salt in the filtrate after the filtration is 1.02%, and the mass content of calcium chloride in the filtrate after the filtration is 0.01%;
[0083] After the filtration, the calcium chloride content in the filtrate is measured by a calcium ion detector, an equimolar amount of sodium carbonate is added to generate calcium carbonate precipitate and sodium chloride, the mass content of calcium chloride in the upper clear water is 20ppm, and reverse osmosis treatment is performed; after the reverse osmosis treatment, the mass content of soluble salts in the produced water is 100ppm, and the produced water is reused in step 3); the mass content of soluble salts in the concentrated water after reverse osmosis is 8%;
[0084] 3) Mix the air-dried solid and water, and filter again with a plate and frame filter press; the mass ratio of the air-dried solid to water is 1:6; the mass content of soluble salt in the mixed solution is 0.09%; the mass content of water in the solid after the second filter press is 49.7%; the mass content of soluble salt in the filtrate after the second filter press is 0.15%, and the filtrate is reused in step 1);
[0085] 4) The solid after the filter pressing in step 3) is dried at 130° C., with a weight of 8.71 kg and a water content of 5.2%; the solid is crushed to a particle size of no more than 100 μm; and then, the solid is calcined at 1000° C. for 1 hour.
[0086] 5) The material burned in step 4) is blown into a plurality of cylindrical magnetic bars by air flow to remove iron, thereby obtaining porcelain clay. The iron content of the porcelain clay is 2.9%.
[0087] After testing, the waste residue was 0.61 kg, the porcelain clay yield was 84.2%, the solid conversion rate was 89.9%, and 62 L of water was used.
[0088] Some components of the porcelain clay are shown in Table 2.
[0089] Table 2 Some components of porcelain clay
[0090]
[0091]
[0092] As shown in Tables 1 and 2, after the red mud is treated by the present invention, most of the sodium is removed and the rest is retained. The main components of the finished product are similar to those of porcelain clay, and the titanium oxide content is relatively high, which has the effect of optimizing porcelain. From the perspective of various test indicators, it meets the requirements of porcelain clay.
[0093] Testing the finished porcelain clay revealed that:
[0094] The mass content of soluble salt is 0.32% (the detection instrument is a conductivity meter);
[0095] Loss on ignition: 1.8% (detection instrument is muffle furnace);
[0096] The bulk density of the finished porcelain clay is: 0.445 g / mL (the testing instrument is a bulk density tester).
[0097] The average particle size of the finished porcelain clay is 8.08 μm, equivalent to 1700 mesh. See the particle size distribution chart for details. Figure 1 This is the particle size distribution diagram of the porcelain clay obtained in Example 1 of the present invention.
[0098] The porcelain factory conducted application tests on this sample and the results were good.
[0099] Example 2
[0100] The composition of the red mud is the same as that of Example 1.
[0101] Preparation of porcelain clay:
[0102] 1) In a circular storage tank, add 80 tons of an acid solution (a mixed solution of sulfuric acid and oxalic acid) with a mass concentration of 0.2%, and then add 13 tons of red mud, and react at 20° C. for 3 hours to obtain a salt solution with a pH value of 6; the mass concentration of soluble salt in the salt solution is 0.79%;
[0103] 2) The salt solution is sent to a plate-frame filter press for filtration, and the moisture content of the filter cake is controlled to be 49.3% by mass; after the filtration is completed, compressed air is introduced to dry the filter cake; the amount of compressed air used is 10 kg / cm 2 ; The mass content of soluble salt in the filtrate after the filter press is 0.99%, and the mass content of calcium chloride in the filtrate after the filter press is 0.096%;
[0104] After the filtration, the calcium chloride content in the filtrate is determined by a calcium ion detector, and an equimolar amount of sodium carbonate is added to generate calcium carbonate precipitate and sodium chloride. The mass content of calcium chloride in the upper clear water is 20 ppm, and reverse osmosis treatment is performed; after the reverse osmosis treatment, the mass content of soluble salts in the produced water is 150 ppm, and the produced water is reused in step 3);
[0105] 3) Mix the air-dried solid and water, and filter again with a plate and frame filter press; the mass ratio of the air-dried solid to water is 1:9; the mass content of soluble salt in the mixed solution is 0.11%; the mass content of water in the solid after the second filter press is 49.3%; the mass content of soluble salt in the filtrate after the second filter press is 0.14%, and the filtrate is reused in step 1);
[0106] 4) The solid after the filter pressing in step 3) is dried at 120° C., with a weight of 9.63 kg and a water content of 4.8%; the solid is crushed to a particle size of no more than 100 μm; and then, the solid is calcined at 1200° C. for 30 min.
[0107] 5) The material burned in step 4) was blown into a plurality of cylindrical magnetic bars by air flow to remove iron, thereby obtaining 9.37 kg of porcelain clay, wherein the iron content of the porcelain clay was 3.0%.
[0108] After testing, the waste residue was 0.56kg, the porcelain clay yield was 85.2%, the solid conversion rate was 89.7%, and 68L of water was used.
[0109] Some components of the porcelain clay are shown in Table 3.
[0110] Table 3 Some components of porcelain clay
[0111]
[0112] As can be seen from Table 1 and Table 3, after the red mud is treated by the present invention, most of the sodium is removed and the rest is retained. The main components of the finished product are similar to those of porcelain clay, and the titanium oxide content is relatively high, which has the effect of optimizing porcelain. From the perspective of various test indicators, it meets the requirements of porcelain clay.
[0113] Testing the finished porcelain clay revealed that:
[0114] The mass content of soluble salt is 0.34% (detection method is conductivity meter);
[0115] Loss on ignition: 2.0% (detection instrument is muffle furnace);
[0116] The bulk density of the finished porcelain clay is: 0.451 g / mL (the testing instrument is a bulk density tester).
[0117] The average particle size of the finished porcelain clay is 10μm, equivalent to 1600 mesh. See the particle size distribution chart for details. Figure 2 This is the particle size distribution diagram of the porcelain clay obtained in Example 2 of the present invention.
[0118] The porcelain factory conducted application tests on this sample and the results were good.
[0119] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing porcelain clay, comprising the following steps: A) mixing red mud and an acid solution, reacting to obtain a salt solution with a pH value of 4 to 6.8; The red mud has a mass content of Na2O of 6% to 10%, a mass content of Al2O3 of 22% to 27%, a mass content of SiO2 of 20% to 25%, a mass content of Fe2O3 of 7% to 12%, a mass content of TiO2 of 2% to 7%, a mass content of CaO of 11% to 16%, and a mass content of K2O of 1% to 2%; B) filtering the solution obtained in step A) to control the mass content of water to be no more than 50%, and the mass content of soluble salt in the filtrate after filtering is 0.5% to 1.2%; then introducing compressed air to dry the solution; The amount of compressed air is 4-30 kg / cm 2 ; After the filtration, the method further includes: removing calcium chloride from the filtrate; the method for removing calcium chloride from the filtrate includes: measuring the calcium chloride content in the filtrate according to a calcium ion detector, adding sodium carbonate to generate calcium carbonate precipitation and sodium chloride, and performing reverse osmosis treatment on the upper layer of clear water; After the calcium chloride in the filtrate is removed, the mass content of calcium chloride in the filtrate is ≤400ppm; after the reverse osmosis treatment, the mass content of soluble salts in the produced water is ≤150ppm; C) mixing the air-dried solid with water and filtering again; The water includes the produced water after the reverse osmosis treatment in step B); The filtrate after the second filtration is reused in step A); D) drying and calcining the solid after the filter press in step C); the calcination temperature is 600 to 1200° C. and the time is 2 minutes to 2 hours; E) removing iron from the material burned in step D) to obtain porcelain clay; The iron removal method comprises: blowing the material into a plurality of cylindrical magnetic bars by air flow to remove iron; after the iron removal, the iron content of the obtained porcelain clay is 2.5% to 3.5%.
2. The preparation method according to claim 1, characterized in that: In step A), the Ca / S of the red mud is 0.3-0.8:1; the N / S of the red mud is 0.1-0.6:
1.
3. The preparation method according to claim 1, characterized in that: In step A), the acid in the acid solution includes at least one of hydrochloric acid, oxalic acid, phosphoric acid and sulfuric acid; The mass concentration of the acid solution is 2% to 12%.
4. The preparation method according to claim 1, characterized in that: In step A), the mass ratio of the acid solution to the red mud is 6 to 12:1; The mass concentration of soluble salt in the salt solution is 0.5% to 1.2%.
5. The preparation method according to claim 1, characterized in that: In step C), the mass ratio of the solid to water after air drying is 1:5-10; In the mixed solution, the mass content of soluble salt is 0.065% to 0.14%.
6. The preparation method according to claim 1, characterized in that: In step C), the mass content of water in the solid after the second filter pressing is ≤50%; The mass content of soluble salt in the filtrate after the second filtration is 0.07% to 0.15%.
7. The preparation method according to claim 1, characterized in that: In step D), the drying temperature is 120-150° C.; the moisture content of the solid after drying is 1%-10%.
Citation Information
Patent Citations
Method for gradient recovery of iron and sodium resources in red mud and full-quantitative utilization of tailings
CN113562770A