A kind of concrete anticorrosion silane impregnating agent and preparation method thereof

By using composite emulsifiers and silane components to prepare paste impregnation agents, the problem of insufficient binding strength of concrete preservatives in the prior art is solved, and better anticorrosion and durability are achieved, and by forming a stable emulsified structure and hydrophobic protection are achieved. The film significantly improves the waterproof and corrosion resistance of concrete.

CN118495989BActive Publication Date: 2024-11-22SHANDONG VOSGES XUANWEI NEW MATERIAL TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410968533.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing concrete anti-corrosion silane impregnant has weak bonding power with the concrete matrix, resulting in poor corrosion resistance and poor durability.

Method used

The paste-like impregnating agent is prepared by using composite emulsifier and silane components. Through the synergy of non-ionic emulsifier and coconut oil fatty acid diethanolamide, a stable emulsification structure is formed, which improves the wetting and permeability of the impregnating agent, and passes through silane. The hydrolysis and condensation reaction forms a hydrophobic protective film, enhancing the bonding force with concrete.

Benefits of technology

It significantly improves the bonding force between the impregnating agent and the concrete matrix, enhances corrosion resistance and durability, ensures uniform coverage and deep penetration of the impregnating agent, effectively blocks corrosive substances such as moisture, oxygen and CO2, and extends the service life of the concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of concrete surface treatment, and more particularly to a concrete anticorrosive silane impregnating agent and a preparation method thereof, comprising the following steps: S1, adding a composite emulsifier to water, stirring and mixing, and obtaining a mixed solution A, wherein the composite emulsifier at least comprises a nonionic emulsifier and coconut oil fatty acid diethanolamide; S2, slowly adding the mixed silane to the mixed solution A under stirring, stirring for 2-3 hours, then adding an auxiliary agent, emulsifying at a rotation speed of 2000-4000rpm, and the emulsification time is 0.5-2 hours, and obtaining an anticorrosive silane impregnating agent, wherein the anticorrosive silane impregnating agent is in a paste state. The paste impregnating agent is prepared by mixing silane and a composite emulsifier, and the paste formulation has high viscosity and fluidity, and can be better attached to the concrete surface; at the same time, each component acts synergistically, thereby improving the bonding force between the impregnating agent and the concrete matrix, and improving the corrosion resistance and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete surface treatment, and in particular to a concrete anticorrosive silane impregnating agent and a preparation method thereof. Background Art

[0002] Concrete is one of the most widely used building materials in modern architecture. However, due to its porosity and surface hydrophilicity, concrete is easily corroded by water and harmful substances, which leads to a decrease in the durability of concrete structures and shortens their service life. In order to extend the service life of concrete structures and improve their durability, concrete surface treatment technology has emerged. At present, common methods for concrete surface treatment include cement-based penetrating crystalline waterproof coating brushing, silane impregnation material treatment and concrete surface coating treatment. Cement-based penetrating crystalline waterproof coating is mainly based on silicate treatment agent, which penetrates into the pores of the concrete surface, improves the surface density and durability of the concrete material, but has limited sealing effect on the porous structure of concrete. Concrete surface coating treatment mainly adopts epoxy, polyurethane and other polymer compounds to form a dense protective film on the concrete surface to block the erosion of harmful substances, but there are problems such as interface adhesion attenuation and poor recoating performance.

[0003] In contrast, silane impregnated materials have unique advantages. Its main component, alkyl alkoxysilane, hydrolyzes in the alkaline environment of concrete to form silanol, which reacts chemically with the concrete surface to form a -Si-O-Si- structure. At the same time, the alkyl group, as a hydrophobic group, gives the concrete surface excellent hydrophobicity. Silane impregnants can form a hydrophobic layer 3-10mm on the surface of concrete, effectively blocking the invasion of harmful substances such as water and chloride ions, and greatly improving the durability indicators of concrete such as freeze-thaw resistance and chloride ion salt resistance. In addition, by reducing water absorption, silane impregnation can also alleviate the problem of concrete carbonization caused by carbon dioxide. Therefore, using silane impregnants to treat the concrete surface is an effective way to improve the durability of concrete.

[0004] The existing patent CN108101582A discloses an organic-inorganic hybrid concrete impregnating agent and a preparation method, comprising tetraethyl orthosilicate, anhydrous ethanol, tartaric acid, terminal hydroxyl silicone oil, water and nano-silica sol, wherein the molar ratio of tetraethyl orthosilicate, anhydrous ethanol and tartaric acid is 1:(1-2):(0.025-0.030), the content of terminal hydroxyl silicone oil is 30%-35% of the mass of tetraethyl orthosilicate, the molar ratio of water to tetraethyl orthosilicate is 2:1, and the content of nano-silica sol is 10%-15% of the mass of tetraethyl orthosilicate. The hydrophobicity of the concrete surface is improved by optimizing and complementing the performance of organic materials and inorganic materials. However, the above scheme has the following problems: on the one hand, the organic-inorganic hybrid network structure is not perfect enough, which easily leads to weak bonding between the coating and the concrete matrix. Under the long-term effects of external factors such as wind, rain, and temperature changes, the coating is prone to cracking, peeling, and falling off. On the other hand, the organic components in the impregnating agent, such as end-hydroxy silicone oil, are prone to chemical bond breaking under long-term ultraviolet radiation and humid and hot environments, resulting in a decrease in the mechanical properties of the coating, the shedding of hydrophobic groups, and a significant reduction in the waterproof and anti-corrosion effect, resulting in poor corrosion resistance and durability. Summary of the invention

[0005] In view of this, the present invention proposes a concrete anti-corrosion silane impregnating agent and a preparation method thereof, so as to solve the problems that the existing anti-corrosion impregnating agent has weak bonding force with the concrete matrix, poor anti-corrosion performance and poor durability.

[0006] The technical solution of the present invention is achieved in this way:

[0007] In a first aspect, the present invention provides a method for preparing a concrete anti-corrosion silane impregnating agent, comprising the following steps:

[0008] S1, adding a composite emulsifier to water, stirring and mixing, to obtain a mixed solution A, wherein the composite emulsifier comprises at least a nonionic emulsifier and coconut oil fatty acid diethanolamide;

[0009] S2. Slowly add the mixed silane to the mixed solution A under stirring, stir for 2-3 hours, then add the auxiliary agent, emulsify at a rotation speed of 2000-4000 rpm, and the emulsification time is 0.5-2 hours to obtain an anti-corrosion silane impregnating agent, which is a paste.

[0010] In the present invention, a paste impregnating agent is prepared with silane and an emulsifier. The paste formulation has high viscosity and fluidity, can be better attached to the concrete surface, and is not easy to lose. Compared with a liquid formulation, the paste impregnating agent is less likely to overflow and leak, which is conducive to ensuring that the impregnating agent can evenly cover the entire concrete surface and exert the best anti-corrosion effect. Among them, the silane component will undergo a hydrolysis and condensation reaction in the concrete to form a hydrophobic siloxane polymer film. This hydrophobic protective film can effectively block corrosive substances such as moisture, oxygen, and CO2 from entering the interior of the concrete, and play a good anti-corrosion role; a non-ionic emulsifier and coconut oil fatty acid diethanolamide are compounded to form a composite emulsifier, which can improve the wettability and permeability of the impregnating agent to the concrete, promote its penetration into the internal pores, and uniform coverage and deep penetration help to form a continuous and uniform protective film, effectively protecting the internal structure of the concrete.

[0011] On the basis of the above technical solution, preferably, in step S1, the method for preparing the composite emulsifier comprises the following steps:

[0012] S11, adding a nonionic emulsifier to deionized water, and then adding coconut oil fatty acid diethanolamide, stirring evenly to obtain a mixed solution B;

[0013] S12, adding MgCl2 to the mixed solution B, and then adding perfluoro-2,5-dimethyl-3,6-dioxononyl alkyl ester, stirring evenly to obtain the composite emulsifier.

[0014] On the basis of the above technical solution, preferably, the nonionic emulsifier is any one of a span series emulsifier, a tween series emulsifier and an op series emulsifier.

[0015] Furthermore, nonionic emulsifiers can change the properties of the water-oil interface, reduce interfacial tension, and enhance emulsification ability; at the same time, they can stabilize small particle emulsions and improve the emulsification stability of the system. Coconut oil fatty acid diethanolamide is a nonionic surfactant, and its structure can be adsorbed on the oil-water interface to form a stable emulsion film, enhancing the stability of the emulsification system; it also has good wettability and permeability. Compared with a single nonionic emulsifier, a composite emulsifier formed by a nonionic emulsifier and coconut oil fatty acid diethanolamide, the synergistic effect of the two further improves the emulsification performance of the composite emulsifier through the synergistic effect of interfacial activity and wettability; significantly reduces the contact angle and interfacial tension of the impregnating agent on the concrete surface, and greatly improves the wettability and permeability of the impregnating agent.

[0016] As an inorganic salt, MgCl2 can increase the ionic strength of the emulsified system and further improve the emulsified stability; perfluoro-2,5-dimethyl-3,6-dioxononyl alkyl ester has extremely strong hydrophobicity and can be better compatible with hydrophobic substances such as silane. In the emulsified system, it can be synergistically adsorbed on the surface of silane particles with emulsifier molecules to form a stable interface, thereby improving the stability of the emulsion. The addition of MgCl2 and perfluoroalkyl ester can enhance the stability of the emulsifier micelles, avoid phase separation, and ensure the stability of the impregnant quality; the stable emulsified structure is conducive to better dispersion of silane in the water phase, improving the penetration and adhesion of the impregnant to concrete; the addition of hydrophobic perfluoroalkyl ester can enhance the hydrophobic protection of the impregnant on concrete and improve the anti-corrosion performance.

[0017] On the basis of the above technical scheme, preferably, by weight, the amount of the nonionic emulsifier added is 30-40 parts, the amount of coconut oil fatty acid diethanolamide added is 20-30 parts, the amount of MgCl2 added is 5-10 parts, and the amount of perfluoro-2,5-dimethyl-3,6-dioxononyl alkyl ester added is 10-20 parts.

[0018] On the basis of the above technical solution, preferably, in step S2, the mixed silane includes a silane monomer and a methyltrimethoxysilane prepolymer, and the mass ratio of the silane monomer to the methyltrimethoxysilane prepolymer is 3-5:5-7.

[0019] On the basis of the above technical solution, preferably, in step S2, the method for preparing the methyltrimethoxysilane prepolymer comprises the following steps:

[0020] Add methyltrimethoxysilane and ethyl silicate to an organic solvent, then add a catalyst, stir evenly, control the solution pH to 2-5, heat in a water bath to 70-80°C, react for 5-10 hours, filter to remove the catalyst, and remove the organic solvent by reduced pressure distillation to obtain a methyltrimethoxysilane prepolymer.

[0021] On the basis of the above technical scheme, preferably, the mass ratio of methyltrimethoxysilane to ethyl silicate is 1:1.3-1.5, the organic solvent is any one of ethanol and propanol, the catalyst is hydrochloric acid or sulfuric acid, and the amount of the catalyst added is 0.3-0.5% of the mass of methyltrimethoxysilane.

[0022] Specifically, silane monomers have a small molecular weight and strong reactivity, can penetrate deep into the concrete, and react chemically with components in the concrete (such as calcium, silicon, etc.) to form a strong chemical bond; methyltrimethoxysilane prepolymers have a large molecular weight and low reactivity, forming a stable hydrophobic film at the interface. Mixing silane monomers and methyltrimethoxysilane prepolymers and using them in synergy can achieve a synergistic anti-corrosion mechanism of surface hydrophobic protection and internal chemical bonding.

[0023] On the basis of the above technical solution, preferably, the silane monomer includes one or more of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-aminopropyltriethoxysilane, dimethyldimethoxysilane, and dodecyltrimethoxysilane.

[0024] On the basis of the above technical solution, preferably, the anti-corrosion silane impregnating agent comprises, by weight, 20-30 parts of silane, 8-12 parts of composite emulsifier, 30-40 parts of water, and 3-5 parts of auxiliary agent.

[0025] Based on the above technical solution, preferably, in step S2, the auxiliary agent includes glycerol or ethylene glycol. Auxiliary agents such as glycerol or ethylene glycol can improve the viscosity and ductility of the impregnating agent, facilitate the formation of a uniform and stable protective film layer, and also improve the flexibility and weather resistance of the film layer.

[0026] In a second aspect, the present invention provides a concrete anti-corrosion silane impregnating agent, wherein the concrete anti-corrosion silane impregnating agent is prepared by a preparation method as described in any one of the above items.

[0027] The concrete anticorrosion silane impregnating agent and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:

[0028] (1) A paste impregnating agent is prepared by using silane and emulsifier. The silane component penetrates into the concrete matrix and forms Si-O-Si bonds through condensation reaction, firmly bonding with the concrete surface, effectively blocking corrosive substances such as moisture, oxygen, and CO2 from entering the interior of the concrete, thus playing a good anti-corrosion role. The emulsifier can form a stable micelle structure, effectively disperse and suspend the hydrophobic silane monomer or prepolymer, improve the wettability and permeability of the impregnating agent, and promote the silane to penetrate deeper into the concrete matrix, ensuring that the silane not only forms a hydrophobic film on the surface, but also penetrates into the interior, thus playing a comprehensive protective role.

[0029] (2) A composite emulsifier is formed by a non-ionic emulsifier and coconut oil fatty acid diethanolamide. The synergistic effect of the two further improves the emulsification performance of the composite emulsifier through the synergistic effect of interfacial activity and wettability, significantly reduces the contact angle and interfacial tension of the impregnant on the concrete surface, and greatly improves the wettability and permeability of the impregnant. The addition of MgCl2 and perfluoroalkyl ester can enhance the stability of the emulsifier, avoid phase separation, and ensure the stability of the impregnant quality. The stable emulsified structure is conducive to better dispersion of silane in the water phase, thereby improving the penetration and adhesion of the impregnant to concrete. The synergistic effect of each component improves the bonding strength between the impregnant and the concrete matrix, and improves the corrosion resistance and durability.

[0030] (3) A paste impregnating agent is prepared by mixing silane and composite emulsifier. The paste formulation has higher viscosity and fluidity, can better adhere to the concrete surface, and is not easy to flow. Compared with liquid formulations, the paste impregnating agent is less likely to overflow and leak, which helps to ensure that the impregnating agent can evenly cover the entire concrete surface and exert the best anti-corrosion effect. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] This embodiment provides a concrete anti-corrosion silane impregnating agent and a preparation method thereof, which specifically comprises the following steps:

[0034] (1) Add 35 g of tween 80 to deionized water, then add 25 g of coconut oil fatty acid diethanolamide, stir evenly, and heat to 50°C to make the solute better dissolved and evenly dispersed to obtain a composite emulsifier; add 10 g of the composite emulsifier to 35 g of water, stir and mix, and obtain a mixed solution A;

[0035] (2) Add 10 g of methyltrimethoxysilane and 14 g of ethyl silicate to 25 g of ethanol, then add hydrochloric acid (1 mol / L), stir evenly, then slowly add 5 g of water, control the pH of the solution to 3.5, heat to 75°C in a water bath, react for 8 h, filter to remove the catalyst, and remove the organic solvent by vacuum distillation to obtain a methyltrimethoxysilane prepolymer;

[0036] (3) γ-aminopropyltriethoxysilane and methyltrimethoxysilane prepolymer are mixed in a mass ratio of 2:3 to obtain a mixed silane. 25 g of the mixed silane is slowly added to the mixed solution A while stirring for 2.5 hours. Then, 4 g of ethylene glycol is added and emulsified at a rotation speed of 3000 rpm for 1.5 hours to obtain an anti-corrosion silane impregnating agent, which is in a paste state.

[0037] Example 2

[0038] This embodiment provides a concrete anticorrosive silane impregnating agent and a preparation method thereof. The specific preparation method is the same as that of Embodiment 1, except that:

[0039] (1) Add 35g of tween 80 to deionized water, then add 25g of coconut oil fatty acid diethanolamide, stir evenly, then add 8g of MgCl2, continue to stir evenly, and heat to 50°C to make the solute better dissolved and evenly dispersed to obtain a composite emulsifier; add 10g of the composite emulsifier to 35g of water, stir and mix, and obtain a mixed solution A.

[0040] Example 3

[0041] This embodiment provides a concrete anticorrosive silane impregnating agent and a preparation method thereof. The specific preparation method is the same as that of Embodiment 1, except that:

[0042] (1) Add 35g of tween 80 to deionized water, then add 25g of coconut oil fatty acid diethanolamide, stir evenly, then add 8g of MgCl2 and 15g of perfluoro-2,5-dimethyl-3,6-dioxonyl alkyl ester in sequence, continue to stir evenly, and heat to 50°C to make the solute better dissolved and evenly dispersed to obtain a composite emulsifier; add 10g of the composite emulsifier to 35g of water, stir and mix, and obtain a mixed solution A.

[0043] Example 4

[0044] This embodiment provides a concrete anti-corrosion silane impregnating agent and a preparation method thereof, which specifically comprises the following steps:

[0045] (1) Add 30g of tween 80 to deionized water, then add 20g of coconut oil fatty acid diethanolamide, stir evenly, then add 5g of MgCl2 and 10g of perfluoro-2,5-dimethyl-3,6-dioxonyl alkyl ester in sequence, continue to stir evenly, and heat to 50°C to make the solute better dissolved and evenly dispersed to obtain a composite emulsifier; add 8g of the composite emulsifier to 30g of water, stir and mix, and obtain a mixed solution A;

[0046] (2) Add 10 g of methyltrimethoxysilane and 13 g of ethyl silicate to 20 g of ethanol, then add 30 mg of hydrochloric acid (1 mol / L), stir evenly, then slowly add 4 g of water, control the pH of the solution to 2, heat to 70°C in a water bath, react for 5 h, filter to remove the catalyst, and remove the organic solvent by vacuum distillation to obtain a methyltrimethoxysilane prepolymer;

[0047] (3) Dimethyldimethoxysilane and methyltrimethoxysilane prepolymers are mixed in a mass ratio of 3:5 to obtain a mixed silane. 20 g of the mixed silane is slowly added to the mixed solution A while stirring for 2 h. Then, 3 g of ethylene glycol is added and emulsified at a rotation speed of 2000 rpm for 0.5 h to obtain an anti-corrosion silane impregnating agent, which is in a paste state.

[0048] Example 5

[0049] This embodiment provides a concrete anti-corrosion silane impregnating agent and a preparation method thereof, which specifically comprises the following steps:

[0050] (1) Add 40g of tween 80 to deionized water, then add 30g of coconut oil fatty acid diethanolamide, stir evenly, then add 10g of MgCl2 and 20g of perfluoro-2,5-dimethyl-3,6-dioxonyl alkyl ester in sequence, continue to stir evenly, and heat to 50°C to make the solute better dissolved and evenly dispersed to obtain a composite emulsifier; add 12g of the composite emulsifier to 40g of water, stir and mix, and obtain a mixed solution A;

[0051] (2) Add 10 g of methyltrimethoxysilane and 15 g of ethyl silicate to 30 g of ethanol, then add 50 mg of hydrochloric acid (1 mol / L), stir evenly, then slowly add 7 g of water, control the pH of the solution to 5, heat to 80°C in a water bath, react for 10 h, filter to remove the catalyst, and remove the organic solvent by vacuum distillation to obtain a methyltrimethoxysilane prepolymer;

[0052] (3) γ-aminopropyltriethoxysilane and methyltrimethoxysilane prepolymer are mixed in a mass ratio of 5:7 to obtain a mixed silane. 30 g of the mixed silane is slowly added to the mixed solution A while stirring for 3 h. Then, 5 g of glycerol is added and emulsified at a rotation speed of 4000 rpm for 2 h to obtain an anti-corrosion silane impregnating agent, which is in a paste state.

[0053] Example 6

[0054] This embodiment provides a concrete anticorrosive silane impregnating agent and a preparation method thereof. The specific preparation method is the same as that of Embodiment 3, except that:

[0055] (3) γ-aminopropyltriethoxysilane and methyltrimethoxysilane prepolymer are mixed in a mass ratio of 2:3 to obtain a mixed silane. 25 g of the mixed silane is slowly added to the mixed solution A while stirring for 2.5 hours. Emulsification is performed at a rotation speed of 3000 rpm for 1.5 hours to obtain an anti-corrosion silane impregnating agent, which is in a paste state.

[0056] Example 7

[0057] The present embodiment provides a concrete anti-corrosion silane impregnating agent and a preparation method thereof. The specific preparation method is the same as that of Example 3, except that: in step (1), the amount of tween 80 added is 25 g, the amount of coconut oil fatty acid diethanolamide added is 15 g, the amount of MgCl2 added is 8 g, and the amount of perfluoro-2,5-dimethyl-3,6-dioxononyl alkyl ester added is 15 g.

[0058] Comparative Example 1

[0059] This embodiment provides a concrete anti-corrosion silane impregnating agent and a preparation method thereof, and the specific preparation method is as follows:

[0060] (1) Add 35g of tween 80 to deionized water, stir evenly, and heat to 50°C to make the solute dissolve better and disperse evenly to obtain an emulsifier; add 10g of the emulsifier to 35g of water, stir and mix to obtain a mixed solution A;

[0061] (2) Slowly add 25 g of γ-aminopropyltriethoxysilane to the mixed solution A while stirring for 2.5 h, and emulsify at a rotation speed of 3000 rpm for 1.5 h to obtain an anti-corrosion silane impregnating agent, which is in the form of a paste.

[0062] Comparative Example 2

[0063] This embodiment provides a concrete anticorrosive silane impregnating agent and a preparation method thereof. The specific preparation method is the same as that of Comparative Example 1, except that:

[0064] (1) Add 35 g of tween 80 to deionized water, then add 25 g of coconut oil fatty acid diethanolamide, stir evenly, and heat to 50 ° C to make the solute better dissolved and evenly dispersed to obtain a composite emulsifier; add 10 g of the composite emulsifier to 35 g of water, stir and mix, and obtain a mixed solution A.

[0065] Comparative Example 3

[0066] This embodiment provides a concrete anticorrosive silane impregnating agent and a preparation method thereof. The specific preparation method is the same as that of Comparative Example 1, except that:

[0067] 35g of tween 80 was added to deionized water, followed by 25g of coconut oil fatty acid diethanolamide, stirred evenly, and then 8g of MgCl2 and 15g of perfluoro-2,5-dimethyl-3,6-dioxonyl alkyl ester were added in sequence, and stirring was continued evenly. The mixture was heated to 50°C to make the solutes better dissolved and evenly dispersed to obtain a composite emulsifier; 10g of the composite emulsifier was added to 35g of water, stirred and mixed to obtain a mixed solution A.

[0068] Performance Testing

[0069] The silane impregnating agents prepared in Examples 1-7 and Comparative Examples 1-3 were applied to impregnated concrete, and performance tests were performed, including water absorption, penetration depth, carbonization depth, and freeze-thaw cycle performance. After the impregnated concrete specimens with strength grade C30 were cured for 28 days, they were dried at 80°C for 8 hours to obtain the dried concrete specimens to be impregnated. The concrete specimens were impregnated with silane according to the industry standard "Corrosion Protection Construction Code for Water Transport Engineering Structures" (JTS / T 209-2020), and the impregnation was performed 3 times, with an amount of 300 ml / m 2 , measure the penetration depth and water absorption rate, and measure the carbonization depth according to GB / T 50082. The specific test results are shown in Table 1.

[0070] Table 1

[0071]

[0072] As can be seen from Table 1, by comparing Examples 1-3, it can be seen that the synergistic effect of the components in the composite emulsifier can improve the waterproof and anti-corrosion properties of the impregnating agent. Comparison of Examples 3-5 shows that the silane impregnating agent prepared by the present invention has good waterproof and anti-corrosion properties. Comparing Example 3 with Example 6, it can be seen that the addition of the auxiliary agent is conducive to the formation of a uniform and stable protective film layer of the impregnating agent, thereby improving the anti-corrosion performance. Comparing Example 3 with Example 7, it can be seen that the ratio of the components in the composite emulsifier may have an impact on the performance of the impregnating agent. Comparing Example 3 with Comparative Examples 1-3, it is shown that the composite emulsifier obtained by compounding a non-ionic emulsifier, coconut oil fatty acid diethanolamide, MgCl2 and perfluoro-2,5-dimethyl-3,6-dioxononyl alkyl ester, and the silane monomer and silane prepolymer form a mixed silane, the synergistic effect of the composite emulsifier and the mixed silane can improve the waterproof and anti-corrosion properties of the silane impregnating agent.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a concrete anticorrosive silane impregnating agent, characterized in that: The following steps are involved: S1, adding a composite emulsifier to water, stirring and mixing, to obtain a mixed solution A, wherein the composite emulsifier comprises at least a nonionic emulsifier and coconut oil fatty acid diethanolamide; S2. Slowly add the mixed silane to the mixed solution A under stirring, stir for 2-3 hours, then add the auxiliary agent, emulsify at a rotation speed of 2000-4000rpm, and the emulsification time is 0.5-2h to obtain an anti-corrosion silane impregnating agent, wherein the anti-corrosion silane impregnating agent is in a paste state, and the mixed silane includes a silane monomer and a methyltrimethoxysilane prepolymer; In step S1, the preparation method of the composite emulsifier comprises the following steps: S11, adding a nonionic emulsifier to deionized water, and then adding coconut oil fatty acid diethanolamide, stirring evenly to obtain a mixed solution B; S12, adding MgCl2 to the mixed solution B, and then adding perfluoro-2,5-dimethyl-3,6-dioxonyl alkyl ester, stirring evenly to obtain the composite emulsifier; The nonionic emulsifier is any one of the span series emulsifiers, tween series emulsifiers and op series emulsifiers; In step S2, the mass ratio of the silane monomer to the methyltrimethoxysilane prepolymer is 3-5:5-7; the silane monomer includes one or more of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-aminopropyltriethoxysilane, dimethyldimethoxysilane, and dodecyltrimethoxysilane.

2. The method for preparing a concrete anticorrosive silane impregnating agent according to claim 1, characterized in that: In parts by weight, the amount of the nonionic emulsifier added is 30-40 parts, the amount of coconut oil fatty acid diethanolamide added is 20-30 parts, the amount of MgCl2 added is 5-10 parts, and the amount of perfluoro-2,5-dimethyl-3,6-dioxononyl alkyl ester added is 10-20 parts.

3. The method for preparing a concrete anticorrosive silane impregnating agent according to claim 1, characterized in that: In step S2, the method for preparing the methyltrimethoxysilane prepolymer comprises the following steps: Add methyltrimethoxysilane and ethyl silicate to an organic solvent, then add a catalyst, stir evenly, control the solution pH to 2-5, heat in a water bath to 70-80°C, react for 5-10 hours, filter to remove the catalyst, and remove the organic solvent by reduced pressure distillation to obtain a methyltrimethoxysilane prepolymer.

4. The method for preparing a concrete anticorrosive silane impregnating agent according to claim 1, characterized in that: The anticorrosive silane impregnating agent comprises, by weight, 20-30 parts of silane, 8-12 parts of composite emulsifier, 30-40 parts of water and 3-5 parts of auxiliary agent.

5. The method for preparing a concrete anticorrosive silane impregnating agent according to claim 1, characterized in that: In step S2, the auxiliary agent includes glycerol or ethylene glycol.

6. A concrete anticorrosive silane impregnating agent, characterized in that: The concrete anti-corrosion silane impregnating agent is prepared by a preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Organic-inorganic hybrid concrete impregnant and preparation method thereof

    CN108101582A

  • Special silane paste protective agent for concrete and preparation method thereof

    CN101746988A

  • Preparation method of high-permeability concrete surface silicate-silane protective agent

    CN103588502A

  • Organosilicon concrete protective agent and preparation method

    CN103923561A

  • Environment-friendly hydrophobic corrosion-resistant silane paste impregnant for concrete and preparation method of environment-friendly hydrophobic corrosion-resistant silane paste impregnant

    CN114989648A