Preparation method and application of phosphate modified cellulose
By introducing phosphate and imide structures into nanocellulose, phosphate-modified cellulose with bicyclic structures, the problems of low mechanical strength, poor thermal stability and high flammability of nanocellulose aerogel materials are solved. , achieving higher thermal stability and flame retardant performance, improving its application performance in building fireproof partitions and thermal insulation layers.
Patent Information
- Application Number
- CN202410958842.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Due to its low mechanical strength, poor thermal stability and high flammability, nanocellulose aerogel materials have unstable performance and insufficient safety in actual applications, making it difficult to meet the needs of thermal insulation and fire protection.
By introducing phosphate and imide structures, polymers are introduced into nanocellulose through ring-opening metathesis polymerization and epoxidation reactions, forming phosphate-modified cellulose with bicyclic structures, enhancing its mechanical properties and flame retardant performance.
It significantly improves the thermal stability and flame retardant properties of the material, enhances the mechanical properties, delays the combustion process, and improves the safety and practical effects of the material.
Smart Images

Figure CN118496385B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cellulose materials, and in particular to a preparation method and application of phosphate-modified cellulose. Background Art
[0002] As a green and environmentally friendly biomass material, the nanocellulose obtained from wood has a high aspect ratio and a mesh-like winding structure. Its suspension can form a stable three-dimensional network structure through hydrogen bonding and mutual entanglement between fibers. By removing the solvent in it through a certain drying method, it can be converted into an ultra-light, high-porosity, low-thermal conductivity porous solid material - aerogel. As one of the lightest solid materials in the world, aerogel has a porosity of more than 90% and a density as low as 1 kg / m 3 .
[0003] The low thermal conductivity of nanocellulose aerogels gives them great potential for application in thermal insulation materials. However, natural nanocellulose aerogel materials still face many challenges in practical use. The internal structure of nanocellulose aerogels is mainly connected by hydrogen bonds and physical entanglements between cellulose fibers. The overall mechanical strength is low, especially the resilience is poor. It will inevitably be squeezed to a certain extent during storage and use. If the internal structure changes significantly after the external force is removed, its physical properties such as porosity, specific surface area, and thermal conductivity will change significantly, and its performance will inevitably be affected. Secondly, nanocellulose aerogels have a large specific surface area and an active surface chemical environment. Compared with other biomass materials, they are more flammable. The inherent low mechanical strength, poor thermal stability, and high flammability of nanocellulose aerogel materials significantly reduce their practical effects and safety of use. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a method for preparing phosphate-modified cellulose, phosphate-modified cellulose prepared by the method for preparing phosphate-modified cellulose, phosphate-modified cellulose aerogel prepared by the phosphate-modified cellulose, and application of the phosphate-modified cellulose aerogel in building fireproof partitions and thermal insulation layers. The present invention modifies phosphate by norbornene imide, and introduces a polymer containing a bicyclic, imide, and phosphate structure into nanocellulose through ring-opening metathesis polymerization and epoxidation. The rigid imide and bicyclic structures improve the thermal stability of phosphate and enhance the mechanical properties of nanocellulose. The combined effect of the introduced phosphate, bicyclic and imide structures effectively improves the flame retardant properties of nanocellulose.
[0005] The object of the present invention is to provide a method for preparing phosphate-modified cellulose, which is achieved by the following scheme:
[0006] A method for preparing phosphate-modified cellulose comprises the following steps:
[0007] S1. Synthesis of phosphate monomer: dissolve 5-norbornene-2,3-dicarboximide, halogenating agent and activating agent in a solvent, stir for 1 to 5 min at 0 to 25 °C, slowly add phosphate, continue stirring for 2 to 30 min, filter to obtain solid and filtrate, wash the solid three times with solvent during the filtration process, then spin-dry the filtrate to remove the solvent to obtain a solid product, dissolve the product in dichloromethane, wash three times with sodium hydroxide aqueous solution and hydrochloric acid aqueous solution in sequence, collect the organic phase, and spin-dry again to obtain the phosphate monomer;
[0008] S2. Synthesis of polyphosphate: Under nitrogen atmosphere, 1 eq of the phosphate monomer obtained in step S1 and 1 / 200~1 / 50 eq of the catalyst were dissolved in toluene to carry out ring-opening metathesis polymerization. After heating to 50~100 °C for 1~5 h, vinyl ethyl ether was added to quench the reaction, the solvent was removed, and polyphosphate was obtained by recrystallization through acetone;
[0009] S3. Epoxidation of polyphosphate: Under a nitrogen atmosphere, the polyphosphate obtained in step S2 is dissolved in toluene, m-chloroperbenzoic acid is added and stirred at 10-25 °C for 2-5 h, and excess methanol is added to precipitate the epoxidized polyphosphate;
[0010] S4. Cellulose modification: dilute the nanocellulose aqueous suspension to a solution with a solid content of 0.4~0.8 wt.%, add 0.16~0.4 weight parts of epoxidized polyphosphate, the mass ratio of nanocellulose solid content to epoxidized polyphosphate is (5:1)~(2:1), stir at 600~800 rpm at 25~40 ℃ for 8~12 h, continue ultrasonic dispersion for 10~30 min, let stand at room temperature to remove bubbles, and freeze in liquid nitrogen for 5~10 min. Place the frozen sample in a freeze dryer at a temperature of -60~-50 ℃ and a pressure of 1~20 Pa for freeze drying for 60~72 h to obtain a gel-like solid. Place the obtained gel in a vacuum drying oven at a temperature of 140~160 ℃ for 5~10 min to obtain phosphate-modified cellulose.
[0011] Preferably, the concentration of the nanocellulose aqueous suspension is 1-3 wt.%, and the diameter of the nanocellulose is 15-25 nm.
[0012] The present invention uses a rigid norbornene structure as the main chain and simultaneously introduces imide and phosphate groups, thereby improving polymer performance while increasing flame retardancy.
[0013] It should be noted that:
[0014] In the washing steps involved in the present invention, the volume ratio of the washing solvent to the washing liquid is 1:5.
[0015] The concentrations of the sodium hydroxide aqueous solution and the hydrochloric acid aqueous solution used in step S1 are 1-2 mol / L.
[0016] The reaction mechanism in step S1 of the present invention is that the imide first generates the halogenated amide, and then reacts with the phosphate to generate the phosphate monomer.
[0017] Preferably, the halogenating agent is one or more of N-chlorosuccinimide, N-bromosuccinimide, N-iodosuccinimide and dibromohydantoin.
[0018] More preferably, the halogenating agent is N-bromosuccinimide.
[0019] Preferably, the activator is one or more of 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, triethylenediamine, triethylamine, triphenylphosphine and 1,8-diazabicyclo[5.4.0]undec-7-ene.
[0020] More preferably, the activating agent is 1,8-diazabicyclo[5.4.0]undec-7-ene.
[0021] Preferably, the phosphate ester is one or more of dibenzyl phosphite, diphenyl phosphite, diphenyl chlorophosphate and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0022] More preferably, the phosphate ester is 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0023] Preferably, the solvent in step S1 is one or more of N,N-dimethylformamide, tetrahydrofuran, toluene, dichloromethane and acetonitrile.
[0024] More preferably, the solvent in step S1 is acetonitrile.
[0025] By adopting ring-opening metathesis polymerization, polyphosphates with different molecular weights can be simply and efficiently obtained by changing the ratio of phosphate monomer to catalyst. The catalyst is one or more of Grubbs first-generation catalyst, Grubbs second-generation catalyst, and Grubbs third-generation catalyst. The molar ratio of phosphate monomer to catalyst is (50-200):1.
[0026] Preferably, the catalyst is a Grubbs II catalyst.
[0027] Preferably, the molar ratio of 5-norbornene-2,3-dicarboximide, halogenating agent, activating agent and phosphate in step S1 is (1.2-1.8):(1.1-1.3):(1.1-1.3):1.
[0028] More preferably, the molar ratio of 5-norbornene-2,3-dicarboximide, halogenating agent, activating agent and phosphate in step S1 is 1.5:1.2:1.2:1.
[0029] The present invention peroxidizes the double bonds on the main chain by peroxide to obtain a polyphosphate with an epoxy group as the main chain. The epoxy group can efficiently react with the hydroxyl group in the nanocellulose to cross-link the nanocellulose by covalent bonds.
[0030] Preferably, the mass ratio of the polyphosphate to m-chloroperbenzoic acid in step S3 is 1:(10-15)
[0031] More preferably, the mass ratio of the polyphosphate to m-chloroperbenzoic acid is 1:12.
[0032] Another object of the present invention is to provide a phosphate-modified cellulose prepared by the phosphate-modified cellulose preparation method.
[0033] Another object of the present invention is to provide a phosphate-modified cellulose aerogel, which is prepared by the following steps: placing an aqueous solution of phosphate-modified cellulose in liquid nitrogen and freezing it for 5 to 10 minutes, placing the frozen sample in a freeze dryer at a temperature of -60 to -50 ° C and a pressure of 1 to 20 Pa for freeze drying for 60 to 72 hours to obtain a gel-like solid, and placing the obtained gel in a vacuum drying oven at a temperature of 140 to 160 ° C for 5 to 10 minutes to obtain a phosphate-modified cellulose aerogel.
[0034] Another object of the present invention is to protect the application of phosphate modified cellulose aerogel in building fireproof partitions and thermal insulation layers.
[0035] Beneficial Effects
[0036] The present invention has the following beneficial effects:
[0037] 1) The imide structure itself has excellent thermal stability. Introducing it into the cellulose structure can significantly improve the thermal stability of the material.
[0038] 2) Ring-opening metathesis polymerization is used to efficiently and conveniently prepare polyphosphates of different molecular weights. By adjusting the molecular weight and dosage of the polyphosphates, the performance of the final product can be flexibly controlled.
[0039] 3) The oxidized epoxy structure of the double bond in the main chain can efficiently chemically bond to cellulose and produce a stable COC structure.
[0040] 4) The main chain of the double-ring structure has good rigidity, which not only retains the low density and high porosity characteristics of the nanocellulose aerogel itself, but also improves its mechanical properties; the double-ring structure requires higher energy to decompose, so it has better stability at high temperatures; the double-ring structure can form more carbon layers during the combustion process, which helps to prevent the further transfer of heat and oxygen, thereby improving the flame retardant properties.
[0041] 5) Phosphate esters, imides and bicyclic structures can work together to achieve a flame retardant effect of 1+1+1>3. Phosphoric acid produced by the decomposition of phosphate esters at high temperatures reacts with imides to form ammonium phosphate-like substances, which more effectively promotes the carbonization of the bicyclic structure and cellulose. The generated ammonium phosphate further decomposes and releases ammonia as the temperature rises, converting the carbon layer into an expanded carbon layer, further significantly improving the flame retardant properties of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The synthetic route of the phosphate-modified cellulose of the present invention;
[0043] Figure 2 is the hydrogen nuclear magnetic spectrum of the phosphate monomer of the present invention;
[0044] Figure 3 Comparative H NMR spectra of the phosphate monomer, polyphosphate and epoxidized polyphosphate of the present invention;
[0045] Figure 4 The thermogravimetric curves of Examples 2, 5-7 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0046] The following is a more detailed description of the specific implementation method of the present invention, the purpose of which is to explain the concept and characteristics of the present invention, and it cannot be used to limit the scope of protection of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the scope of protection of the present invention.
[0047] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0048] The raw materials used in the embodiments and comparative examples are described as follows:
[0049] Norbornene-2,3-dicarboximide: Shanghai Haohong Biopharmaceutical Technology Co., Ltd., product number 1136952;
[0050] N-Bromosuccinimide: Shanghai MacLean Biochemical Technology Co., Ltd., product number N802275;
[0051] 1,8-diazabicyclo[5.4.0]undec-7-ene: Shanghai MacLean Biochemical Technology Co., Ltd., product number D807027;
[0052] 9,10-Dihydro-9-oxa-10-phosphaphenanthrene-10-oxide: Shanghai MacLean Biochemical Technology Co., Ltd., product number D806521;
[0053] Grubbs II catalyst: Shanghai MacLean Biochemical Technology Co., Ltd., product number G810692;
[0054] Metachloroperbenzoic acid: content 85%, Shanghai Myril Biochemical Technology Co., Ltd.;
[0055] Nanocellulose aqueous suspension: Nanocellulose solution, concentration: 1wt%, diameter: 15-25 nm, Jingkang Biological, product number JK-R0757.
[0056] Preparation of phosphate monomers:
[0057] In a 100 ml round-bottom flask, add 1.5 mol of 5-norbornene-2,3-dicarboximide, 1.2 mol of N-bromosuccinimide and 1.2 mol of 1,8-diazabicyclo[5.4.0]undec-7-ene, dissolve them in acetonitrile, stir for 5 min at 0 °C, then slowly add 1.0 mol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, continue stirring for 10 min. After the reaction is completed, filter out the solid, wash the solid three times with acetonitrile, and spin dry to remove the solvent. The product is dissolved in dichloromethane, washed three times with sodium hydroxide aqueous solution and hydrochloric acid aqueous solution, respectively, and the organic phase is collected and spin dried to obtain the phosphate monomer.
[0058] The polyphosphate ester and phosphate-modified cellulose solution of the present invention are prepared by the following method:
[0059] Polyphosphate 1
[0060] Under nitrogen atmosphere, 1 mol of the obtained phosphate monomer and solvent were added to a 100 ml three-necked flask, and then 1 / 50 mol of Grubbs II catalyst was dissolved in toluene and slowly added dropwise to the three-necked flask for ring-opening metathesis polymerization. After the temperature was raised to 100 °C and the reaction was carried out for 3 h, vinyl ethyl ether was added to quench the reaction, the solvent was removed, and polyphosphate was obtained by recrystallization through acetone.
[0061] Polyphosphate 2
[0062] Compared with polyphosphate 1, the difference is that 1 / 100 mol of Grubbs II catalyst is dissolved in toluene.
[0063] Polyphosphate 3
[0064] Compared with polyphosphate 1, the difference is that 1 / 150 mol of Grubbs II catalyst is dissolved in toluene.
[0065] Polyphosphate 4
[0066] Compared with polyphosphate 1, the difference is that 1 / 200 mol of Grubbs II catalyst is dissolved in toluene.
[0067] Polyphosphate 5
[0068] Compared with polyphosphate 1, the difference is that 1 / 20 mol of Grubbs II catalyst is dissolved in toluene.
[0069] Polyphosphate 6
[0070] Compared with polyphosphate 1, the difference is that 1 / 250 mol of Grubbs II catalyst is dissolved in toluene.
[0071] Phosphate modified cellulose 1
[0072] Under nitrogen atmosphere, 1 g of the obtained polyphosphate ester 1 was dissolved in toluene in a 100 ml flask. 12 g of m-chloroperbenzoic acid was added at 25 °C and stirred for 5 h. Excess methanol was added to precipitate the epoxidized polyphosphate ester.
[0073] In a 500 mL beaker, the nanocellulose aqueous suspension was diluted to 100 ml of a solution with a solid content of 0.8 wt.%, and 0.16 g of epoxidized polyphosphate was added. After stirring at 800 rpm at 30 °C for 10 h, ultrasonic dispersion was continued for 30 min. After standing at room temperature to remove bubbles, phosphate-modified cellulose was obtained for use.
[0074] Phosphate modified cellulose 2
[0075] Compared with phosphate-modified cellulose 1, the difference lies in that polyphosphate ester 1 is replaced by polyphosphate ester 2.
[0076] Phosphate modified cellulose 3
[0077] Compared with phosphate-modified cellulose 1, the difference lies in that polyphosphate ester 1 is replaced by polyphosphate ester 3.
[0078] Phosphate modified cellulose 4
[0079] Compared with phosphate-modified cellulose 1, the difference lies in that polyphosphate ester 1 is replaced by polyphosphate ester 4.
[0080] Phosphate modified cellulose 5
[0081] Compared with phosphate-modified cellulose 2, the difference is that 0.20 g of epoxidized polyphosphate is added during fiber modification.
[0082] Phosphate modified cellulose 6
[0083] Compared with phosphate-modified cellulose 2, the difference is that 0.27 g of epoxidized polyphosphate is added during fiber modification.
[0084] Phosphate modified cellulose 7
[0085] Compared with phosphate-modified cellulose 2, the difference is that 0.40 g of epoxidized polyphosphate is added during fiber modification.
[0086] Phosphate modified cellulose 8
[0087] Compared with phosphate-modified cellulose 1, the difference lies in that polyphosphate ester 1 is replaced by polyphosphate ester 5.
[0088] Phosphate modified cellulose 9
[0089] Compared with phosphate-modified cellulose 1, the difference lies in that polyphosphate ester 1 is replaced by polyphosphate ester 6.
[0090] Phosphate modified cellulose 10
[0091] Compared with phosphate-modified cellulose 2, the difference is that 0.08 g of epoxidized polyphosphate is added during fiber modification.
[0092] Phosphate modified cellulose 11
[0093] Compared with phosphate-modified cellulose 2, the difference is that 0.60 g of epoxidized polyphosphate is added during fiber modification.
[0094] Preparation Example 1
[0095] The aqueous solution of phosphate-modified cellulose 1 was frozen in liquid nitrogen for 10 min, and the frozen sample was quickly placed in a freeze dryer at a temperature of -58 °C and a pressure of 10 Pa for freeze drying for 72 h. The resulting gel was placed in a vacuum drying box at a temperature of 150 °C for 10 min to obtain phosphate-modified cellulose aerogel.
[0096] Preparation Examples 2~7
[0097] Compared with Preparation Example 1, the difference is that phosphate-modified cellulose 1 is changed to phosphate-modified cellulose 2-7.
[0098] Comparative Example 1
[0099] In a 500 mL beaker, the nanocellulose aqueous suspension was diluted to 100 ml of a solution with a solid content of 0.8 wt.%, stirred at 800 rpm at 30 °C for 10 h, and then ultrasonically dispersed for 30 min. After standing at room temperature to remove bubbles, an unmodified cellulose solution was obtained, which was frozen in liquid nitrogen for 10 min. The frozen sample was quickly placed in a freeze dryer at a temperature of -58 °C and a pressure of 10 Pa for freeze drying for 72 h. The resulting gel was placed in a vacuum drying box at a temperature of 150 °C for 10 min to obtain a cellulose aerogel.
[0100] Comparative Examples 2 to 5
[0101] Compared with Preparation Example 1, the difference is that phosphate-modified cellulose 1 is changed to phosphate-modified cellulose 8-11.
[0102] The following is the test method of the performance parameters involved in the present invention:
[0103] (1) Relative molecular weight: gel permeation chromatography-differential detector (Waters, USA);
[0104] (2) Molecular weight distribution: gel permeation chromatography-differential detector (Waters, USA);
[0105] (3) NMR spectra: 400 MHz NMR spectrometer (Bruker, Germany);
[0106] (4) Apparent density , m is the mass of the aerogel sample, and V is the macroscopic volume of the aerogel sample.
[0107] (5) Aerogel porosity: , is the skeleton density of the aerogel sample;
[0108] (6) Compression performance test: Tested by referring to GB / T 8813 "Test method for compression performance of rigid foam plastics";
[0109] (7) Pore size analysis: First, the nitrogen adsorption-desorption isotherm of the aerogel was obtained using a fully automatic specific surface area and pore size analyzer, and the BJH method was used to estimate the average pore size of the aerogel from the nitrogen desorption isotherm.
[0110] (8) Thermal stability test: Using a thermogravimetric analyzer, the sample was heated from room temperature to 750 °C at a heating rate of 10 °C / min;
[0111] (9) Micro-combustion calorimetry test: A micro-combustion calorimeter was used according to ASTM D7309-2007. 2-10 mg of aerogel sample was taken and heated at 80 cm 3The aerogel was pyrolyzed by heating from 75 to 750 °C in a nitrogen atmosphere at a rate of 5 °C / s. The pyrolysis products were then mixed with an O2 / N2 mixture to accelerate the combustion. The oxygen concentration and flow rate of the combustion gas were evaluated, and the heat generated by the aerogel was calculated based on the oxygen consumption.
[0112] Depend on Figure 2 The H-NMR spectrum confirmed the synthesis of the phosphate monomer. Figure 3 The figures in the figure are the comparison of H NMR spectra of phosphate monomer, polyphosphate and epoxidized polyphosphate, respectively. The chemical shift of the double bond after polymerization changes from a sharp peak to an irregular peak. The disappearance of the double bond peak after epoxidation indicates that the double bond is successfully oxidized.
[0113] Table 1 Relative molecular weight and molecular weight distribution of polyphosphate
[0114]
[0115] Table 2 Properties of phosphate-modified cellulose aerogels (Preparation Examples 1-7)
[0116]
[0117] Table 3 Cellulose aerogel properties (Comparative Examples 1-5)
[0118]
[0119] It can be seen from the data of the embodiments and comparative examples that the phosphate-modified cellulose aerogel prepared by the present invention has the advantages of good thermal stability, excellent mechanical properties and excellent flame retardant effect. The thermogravimetric mass residual rate at 700°C is as high as 45.6%, and the compressive strength is as high as 85 Kpa. By cross-linking the epoxidized polyphosphate with nanocellulose, the heat release rate during the combustion of the aerogel can be effectively reduced, the heat release mode can be changed, and the combustion can be delayed.
[0120] From the data of Preparation Examples 1 to 4 in Table 2 and Table 3, it can be seen that within a certain range, the larger the molecular weight of the prepared polyphosphate ester, the better the thermal stability, flame retardant properties and mechanical properties of the prepared phosphate-modified cellulose aerogel, but the density increases slowly and the porosity decreases to a certain extent. From the data of Preparation Examples 2, 5 to 7, it can be seen that with the increase in the amount of polyphosphate ester, the mechanical properties of the aerogel gradually increase, and the thermal stability and flame retardant properties first increase and then decrease. From the data of Comparative Example 1, it can be seen that the aerogel obtained by hydrogen bond entanglement inside cellulose has far less thermal stability, excellent mechanical properties and flame retardant effect than the phosphate-modified cellulose aerogel prepared by the present invention.
[0121] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing phosphate-modified cellulose, characterized in that: The following steps are involved: S1. Synthesis of phosphate monomer: dissolve 5-norbornene-2,3-dicarboximide, halogenating agent and activating agent in a solvent, stir for 1 to 5 min at 0 to 25 °C, slowly add phosphate, continue stirring for 2 to 30 min, filter to obtain solid and filtrate, wash the solid three times with solvent during the filtration process, then spin-dry the filtrate to remove the solvent to obtain a solid product, dissolve the product in dichloromethane, wash three times with sodium hydroxide aqueous solution and hydrochloric acid aqueous solution in sequence, collect the organic phase, and spin-dry again to obtain the phosphate monomer; S2. Synthesis of polyphosphate: Under nitrogen atmosphere, 1 eq of the obtained phosphate monomer and 1 / 200~1 / 50 eq of the catalyst were dissolved in toluene to carry out ring-opening metathesis polymerization. After heating to 50~100 °C for 1~5 h, vinyl ethyl ether was added to quench the reaction, the solvent was removed, and polyphosphate was obtained by recrystallization through acetone; S3. Epoxidation of polyphosphate: Under nitrogen atmosphere, the obtained polyphosphate was dissolved in toluene, m-chloroperbenzoic acid was added and stirred at 10-25 °C for 2-5 h, and excess methanol was added to precipitate the epoxidized polyphosphate; S4. Cellulose modification: Dilute the nanocellulose aqueous suspension to a solution with a solid content of 0.4~0.8 wt.%, add 0.16~0.4 weight parts of epoxidized polyphosphate, the mass ratio of nanocellulose solid content to epoxidized polyphosphate is (5:1)~(2:1), stir at 600~800 rpm at 25~40 ℃ for 8~12 h, continue ultrasonic dispersion for 10~30 min, stand at room temperature to remove bubbles, and obtain phosphate-modified cellulose.
2. The method for preparing phosphate-modified cellulose according to claim 1, characterized in that: The halogenating agent is one or more of N-chlorosuccinimide, N-bromosuccinimide, N-iodosuccinimide and dibromohydantoin.
3. The method for preparing phosphate-modified cellulose according to claim 1, characterized in that: The activator is one or more of 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, triethylenediamine, triethylamine, triphenylphosphine and 1,8-diazabicyclo[5.4.0]undec-7-ene.
4. The method for preparing phosphate-modified cellulose according to claim 1, characterized in that: The solvent in step S1 is one or more of N,N-dimethylformamide, tetrahydrofuran, toluene, dichloromethane and acetonitrile.
5. The method for preparing phosphate-modified cellulose according to claim 1, characterized in that: The phosphate ester is one or more of dibenzyl phosphite, diphenyl phosphite, diphenyl chlorophosphate and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
6. The method for preparing phosphate-modified cellulose according to claim 1, characterized in that: The catalyst is one or more of Grubbs first generation catalyst, Grubbs second generation catalyst and Grubbs third generation catalyst.
7. The method for preparing phosphate-modified cellulose according to claim 1, characterized in that: The molar ratio of 5-norbornene-2,3-dicarboximide, halogenating agent, activating agent and phosphate in step S1 is (1.2-1.8): (1.1-1.3): (1.1-1.3): 1; the mass ratio of polyphosphate to m-chloroperbenzoic acid in step S3 is 1: (10-15).
8. A phosphate-modified cellulose, characterized in that: The cellulose is prepared by the method for preparing phosphate-modified cellulose according to any one of claims 1 to 7.
9. A phosphate-modified cellulose aerogel, characterized in that: The phosphate-modified cellulose aerogel is prepared by the following steps: placing the aqueous solution of the phosphate-modified cellulose of claim 8 in liquid nitrogen for freezing for 5 to 10 minutes, placing the frozen sample in a freeze dryer at a temperature of -60 to -50 ° C and a pressure of 1 to 20 Pa for freeze drying for 60 to 72 hours to obtain a gel-like solid, and placing the obtained gel in a vacuum drying oven at a temperature of 140 to 160 ° C for 5 to 10 minutes to obtain a phosphate-modified cellulose aerogel.
10. Use of the phosphate-modified cellulose aerogel as claimed in claim 9 in fireproof partitions and thermal insulation layers of buildings.