A method for preparing a friction nanogenerator enhanced by a combined crystallization diffusion method
The double-layer triboelectric electronegative dielectric layer MxP/Ag@MxPC film prepared by combined crystal diffusion method solves the problem that the existing PVDF-based TENG cannot simultaneously have high electrical output, breathability, hydrophobicity, hydrophilicity and antibacterial properties. , realizes a high-performance wearable friction nanogenerator, suitable for human motion monitoring.
Patent Information
- Application Number
- CN202410568531.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing PVDF-based TENG cannot simultaneously have high electrical output performance, breathability, external surface hydrophobicity, internal surface hydrophilicity and antibacterial activity, which limits its application.
The double-layer triboelectric electronegative dielectric layer MxP/Ag@MxPC film was prepared by combining crystallization diffusion method (CCD). The ultrasonic dispersion and heating homogenization of Ag@MXene, PVDF and cellulose acetate in dimethyl sulfoxide were used to form Porous, breathable, antibacterial, Janus-infiltrating membrane structure.
Achieve high output, breathable, antibacterial and biocompatible W-TENG, with a water vapor transmission rate of 6779.39g/m2·24h, and the water contact angles of the top and bottom surfaces are 142.65° and 69.27° respectively, with a maximum peak power The density can reach 29W/m2, which is suitable for human movement monitoring.
Smart Images

Figure CN118496539B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of friction nanogenerators. Background Art
[0002] With the continuous development of smart devices and Internet of Things technology, the demand for smart control and biosensing systems has also increased dramatically. Although traditional smart control and biosensing systems have made significant progress and are widely used, they are not suitable for portable devices due to their large size and heavy weight. In addition, the dependence on external power sources and the need for periodic battery replacement will interrupt continuous monitoring and affect system reliability. For this reason, researchers have turned to the development of smaller, lighter, and self-powered smart control and biosensing systems.
[0003] Wearable triboelectric nanogenerators (W-TENGs) can convert low-frequency kinetic energy of human motion into electrical energy, providing a sustainable solution to energy dependence for the miniaturization of intelligent control and biosensing systems. The breathability of W-TENG is one of its important characteristics, which helps prevent skin allergies or itching. In addition, the surface of W-TENG in contact with the human body should be hydrophilic and antibacterial to absorb sweat and accelerate perspiration to prevent bacterial infection, while the outer surface should be hydrophobic to improve self-cleaning ability and extend the use time. Therefore, a practical W-TENG should have breathability, hydrophobic outer surface, hydrophilic inner surface and antibacterial activity.
[0004] Among many materials, polyvinylidene fluoride (PVDF) is regarded as an ideal material for manufacturing W-TENG due to its excellent non-reactivity, electronegativity, dielectric properties, and remarkable flexibility and mechanical strength. At present, PVDF-based TENG technology mainly focuses on the optimization of electrical output performance, but the considerations of safety and physical comfort are still insufficient, which greatly limits its application. The manufacture of PVDF membranes mainly relies on phase inversion technology, solvent evaporation technology, and electrospinning technology, which have manufacturing limitations, such as the challenges of phase inversion technology in air permeability and surface roughness, solvent evaporation technology may cause uneven film shrinkage, and electrospinning is not suitable for large-scale production due to low productivity and high cost. Therefore, there is an urgent need to develop a simple and low-cost new method to prepare high electrical output TENG with ideal characteristics. Summary of the invention
[0005] The present invention aims to solve the problem that the existing PVDF-based TENG cannot simultaneously have high electrical output performance, air permeability, outer surface hydrophobicity, inner surface hydrophilicity and antibacterial activity, and further provide a preparation method of a friction nanogenerator enhanced by a combined crystallization diffusion method.
[0006] A method for preparing a triboelectric nanogenerator enhanced by a combined crystal diffusion method is carried out according to the following steps:
[0007] 1. Synthesis of Ag@MXene:
[0008] The MXene nanosheets are uniformly dispersed in deionized water to obtain a MXene solution, and then an AgNO3 aqueous solution is added to the MXene solution and ultrasonically treated, and finally centrifuged, ultrasonically dispersed in deionized water, and freeze-dried in sequence to obtain Ag@MXene;
[0009] 2. Preparation of MxP / Ag@MxPC membrane:
[0010] ① Add Ag@MXene to dimethyl sulfoxide for ultrasonic dispersion, then add PVDF powder and cellulose acetate powder, and finally heat and homogenize under sealed conditions to obtain the bottom casting solution;
[0011] ② Add MXene nanosheets to dimethyl sulfoxide for ultrasonic dispersion, then add PVDF powder, and finally heat and homogenize under sealed conditions to obtain the top layer casting solution;
[0012] ③ Coat the bottom casting solution and the top casting solution on the surface of the substrate in sequence, then cool for 30s to 60s at a temperature of -20℃ to -40℃, immerse in ice water at a temperature of 0℃ to 4℃ for 4h to 12h after cooling, finally take out, vacuum dry and remove the substrate to obtain the MxP / Ag@MxPC film.
[0013] The beneficial effects of the present invention are:
[0014] This paper proposes and implements for the first time a combined crystal diffusion method (CCD) for the preparation of high-performance wearable triboelectric nanogenerators (W-TENGs). A porous, breathable, antibacterial, Janus wettable, high-output and biocompatible double-layer triboelectric negative dielectric layer (MxP / Ag@MxPC) can be prepared in a one-step, low-cost method. The water vapor permeability can reach 6779.39 g / m 2 After 24 hours, the water contact angles of the top and bottom surfaces can reach 142.65° and 69.27°. The maximum peak power density of the MxP / Ag@MxPC TENG under 8MΩ load can reach 29W / m 2 Based on the excellent performance of the obtained composite material, it can be applied to human motion monitoring.
[0015] Instruction Manual
[0016] Figure 1 A schematic diagram of the preparation of a triboelectric nanogenerator enhanced by a combined crystal diffusion method of the present invention;
[0017] Figure 2The morphology and element distribution of Ag@MXene prepared in step 1 of Example 1, a is a scanning electron microscope image of Ag@MXene, b is a HAADF-STEM image of Ag@MXene, and c is an elemental spectrum;
[0018] Figure 3 The SEM images of the 2_MxP / 2_Ag@MxPC film prepared in Example 2, i is the overall cross-sectional view, ii is the enlarged cross-sectional view of the top layer, iii is the enlarged cross-sectional view of the bottom layer, iv is the surface view of the top layer, and v is the surface view of the bottom layer;
[0019] Figure 4 This is the internal pore size distribution diagram of the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2;
[0020] Figure 5 The scanning electron microscope images of the MXene embedded in the top layer and the Ag@MXene embedded in the bottom layer in the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2, a is the top layer, b is the bottom layer;
[0021] Figure 6 : This is a comparison chart of the water vapor permeability of the x_MxP / y_Ag@MxPC film as a function of the MXene content in the top layer and the Ag@MXene content in the bottom layer, 0 is the 0_MxP / 0_Ag@MxPC film prepared in the comparative experiment 1, 1 is the 1_MxP / 1_Ag@MxPC film prepared in Example 1, 2 is the 2_MxP / 2_Ag@MxP film C prepared in Example 2, 3 is the 3_MxP / 3_Ag@MxPC film prepared in Example 3, and 4 is the 4_MxP / 4_Ag@MxPC film prepared in Example 4;
[0022] Figure 7 : It is a comparison diagram of water contact angle test, i is the top surface of the PVDF membrane (NIPS) prepared in comparative experiment three, ii is the top surface of the PVDF membrane (CCD) prepared in comparative experiment two, ii is the top surface of the 1_MxP / 1_Ag@MxPC membrane prepared in Example one, iv is the bottom surface of the 1_MxP / 1_Ag@MxPC membrane prepared in Example one, v is the top surface of the 2_MxP / 2_Ag@MxPC membrane prepared in Example two, vi is the bottom surface of the 2_MxP / 2_Ag@MxPC membrane prepared in Example two, ⅶ is the top surface of the 3_MxP / 3_Ag@MxPC membrane prepared in Example three, and ⅷ is the bottom surface of the 3_MxP / 3_Ag@MxPC membrane prepared in Example three;
[0023] Figure 8 Comparison of water contact angles of the bottom surface of the PVDF membrane (CCD) prepared in comparative experiment 2 and the bottom surface of the PVDF / CA membrane (CCD) prepared in comparative experiment 4;
[0024] Fig. 9This is the performance test of the TENG prepared using the 2_MxP / 2_Ag@MxPC film of Example 2, i, ii and ii are the response characteristics of voltage, current and charge to frequency, and iv is the relationship between voltage output and power density and resistive load at a frequency of 4 Hz;
[0025] Fig.10 The antibacterial and biocompatibility tests of the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2, i is the colony diagram of Escherichia coli and Staphylococcus aureus retained on the agar plate after being treated with the 2_MxP / 2_Ag@MxPC membrane, ii is the bactericidal efficiency of the 2_MxP / 2_Ag@MxPC membrane at different times, iii is the biocompatibility diagram of the 2_MxP / 2_Ag@MxPC membrane;
[0026] Fig.11 Figure 2 is a detection diagram of TENG prepared by using 2_MxP / 2_Ag@MxPC film in human body motion, i is the response voltage signal diagram of TENG to finger tapping, fist hammering and palm slapping, ii is the voltage signal diagram of TENG when the finger is bent at 30°, 45°, 60° and 90°, iii is the response voltage signal diagram of TENG to wrist bending, iv is the response voltage signal of TENG to elbow bending;
[0027] Fig.12 This is the uniaxial tensile stress-strain behavior of the 2_MxP / 2_Ag@MxPC film prepared in Example 2. DETAILED DESCRIPTION
[0028] Specific implementation method 1: This implementation method is a method for preparing a friction nanogenerator enhanced by a combined crystal diffusion method, which is carried out according to the following steps:
[0029] 1. Synthesis of Ag@MXene:
[0030] The MXene nanosheets are uniformly dispersed in deionized water to obtain a MXene solution, and then an AgNO3 aqueous solution is added to the MXene solution and ultrasonically treated, and finally centrifuged, ultrasonically dispersed in deionized water, and freeze-dried in sequence to obtain Ag@MXene;
[0031] 2. Preparation of MxP / Ag@MxPC membrane:
[0032] ① Add Ag@MXene to dimethyl sulfoxide for ultrasonic dispersion, then add PVDF powder and cellulose acetate powder, and finally heat and homogenize under sealed conditions to obtain the bottom casting solution;
[0033] ② Add MXene nanosheets to dimethyl sulfoxide for ultrasonic dispersion, then add PVDF powder, and finally heat and homogenize under sealed conditions to obtain the top layer casting solution;
[0034] ③ Coat the bottom casting solution and the top casting solution on the surface of the substrate in sequence, then cool for 30s to 60s at a temperature of -20℃ to -40℃, immerse in ice water at a temperature of 0℃ to 4℃ for 4h to 12h after cooling, finally take out, vacuum dry and remove the substrate to obtain the MxP / Ag@MxPC film.
[0035] Figure 1 This is a schematic diagram of the preparation of the friction nanogenerator enhanced by the combined crystallization diffusion method of the present invention; as shown in the figure, the bottom layer is formed by dissolving Ag@MXene (MXene nanosheets loaded with silver nanoparticles), polyvinylidene fluoride (PVDF) and cellulose acetate (CA) in dimethyl sulfoxide (DMSO), while the top layer is made by dissolving MXene nanosheets and PVDF in DMSO. After cooling treatment, DMSO solidifies into crystals and is leached in an ice water bath to eventually form a microporous template for the membrane. The double-layer friction layer has three-dimensional micro-nano pores that enable the skin to exchange with external gases. The surface layer has good hydrophobicity and enhances the self-cleaning function; the bottom layer exhibits good hydrophilicity, which helps to absorb sweat in time and maintain skin health. In addition, the silver nanoparticles of Ag@MXene also show significant antibacterial activity against Escherichia coli and Staphylococcus aureus, effectively inhibiting bacterial growth and preventing infection. In human applications, the maximum power density of W-TENG is 29W / m 2 , can effectively monitor the movement status of the human body.
[0036] This embodiment combines the crystallization diffusion method (CCD method) with DMSO with a higher freezing point as a solvent to dissolve the polymer and form ice crystals under unidirectional cooling conditions. After the ice crystals are dissolved in ice water, micropores are formed, thereby improving the air permeability of the membrane. In addition, this process can also generate micro-nano structures on the surface, thereby improving the hydrophobicity and contact area during the operation of W-TENG. The higher crystallinity in the β phase of PVDF increases the dipole arrangement and surface potential, thereby increasing the triboelectric properties of TENG, and the CCD method can convert the α phase of PVDF into the β phase during the crystallization process. Therefore, the CCD method is very suitable for the production of high-performance W-TENG.
[0037] The beneficial effects of this embodiment are:
[0038] This embodiment proposes and implements a combined crystal diffusion method (CCD) for the preparation of high-performance wearable triboelectric nanogenerators (W-TENG) for the first time. It can prepare a porous, breathable, antibacterial, Janus wettable, high-output and biocompatible double-layer triboelectric negative dielectric layer (MxP / Ag@MxPC) in a one-step, low-cost method. The water vapor permeability can reach 6779.39g / m 2 After 24 hours, the water contact angles of the top and bottom surfaces can reach 142.65° and 69.27°. The maximum peak power density of the MxP / Ag@MxPC TENG under 8MΩ load can reach 29W / m 2 Based on the excellent performance of the obtained composite material, it can be applied to human motion monitoring.
[0039] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the volume ratio of the mass of the MXene nanosheets described in step 1 to deionized water is 1 mg: (1-5) mL; the concentration of the AgNO3 aqueous solution described in step 1 is 1 mg / mL-4 mg / mL; the volume ratio of the MXene solution described in step 1 to the AgNO3 aqueous solution is (8-12): 1. The rest is the same as specific embodiment 1.
[0040] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the ultrasonic treatment in step 1 is carried out for 5 to 15 minutes at a power of 20 to 180 W. The rest is the same as specific implementation method 1 or 2.
[0041] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the centrifugation described in step 1 is carried out at a speed of 8000 r / min to 12000 r / min for 10 to 30 min, and the centrifugation is repeated 3 to 5 times to obtain a centrifugal precipitate. The rest is the same as specific embodiments 1 to 3.
[0042] Specific embodiment 5: This embodiment is different from specific embodiments 1 to 4 in that the ultrasonic dispersion in deionized water and freeze drying described in step 1 are specifically carried out according to the following steps: adding the centrifugal precipitate to deionized water, then ultrasonically treating it for 30s to 60s at a power of 20w to 180w, and finally freeze drying it for 12h to 24h at a temperature of -60°C; the mass ratio of the centrifugal precipitate to the volume of deionized water is 1mg:(1-4)mL. The rest is the same as specific embodiments 1 to 4.
[0043] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the MXene nanosheets in step 1 and step 2② are titanium carbide nanosheets with a size of 5 μm to 20 μm. Other aspects are the same as specific embodiments 1 to 5.
[0044] Specific embodiment 7: This embodiment is different from specific embodiments 1 to 6 in that: the mass ratio of Ag@MXene in step 2① to dimethyl sulfoxide is (1 to 50) mg: 1 mL; the mass ratio of Ag@MXene in step 2① to PVDF powder is 1: (10 to 20); the mass ratio of Ag@MXene in step 2① to cellulose acetate powder is (0.2 to 1): 1. Others are the same as specific embodiments 1 to 6.
[0045] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: the mass ratio of the MXene nanosheets in step 2② to the volume ratio of dimethyl sulfoxide is (8 to 50) mg:1 mL; the mass ratio of the MXene nanosheets in step 2① to the PVDF powder is 1:(3 to 15). Others are the same as specific embodiments 1 to 7.
[0046] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that: the ultrasonic dispersion described in step 2 ① and ② is specifically carried out under the condition of 20w to 180w power, and the ultrasonic treatment is carried out for 30s to 60s; the heating homogenization under sealed conditions described in step 2 ① and ② is specifically carried out under the condition of sealing, temperature of 60℃ to 80℃ and stirring speed of 50r / min to 120r / min, and the heating homogenization treatment is carried out for 10min to 20min. The rest is the same as specific embodiments 1 to 8.
[0047] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: the substrate described in step 2 ③ is an aluminum plate; the coating thickness of the bottom casting solution described in step 2 ③ is 50 μm to 100 μm; the coating thickness of the top casting solution described in step 2 ③ is 50 μm to 100 μm; the vacuum drying described in step 2 ③ is specifically under the condition of a vacuum degree of 2Pa to 1kPa, and the vacuum drying is performed for 12h to 24h. The rest is the same as specific embodiments 1 to 9.
[0048] The following examples are used to verify the beneficial effects of the present invention:
[0049] Embodiment 1:
[0050] A method for preparing a triboelectric nanogenerator enhanced by a combined crystal diffusion method is carried out according to the following steps:
[0051] 1. Synthesis of Ag@MXene:
[0052] 20 mg of MXene nanosheets were evenly dispersed in 20 mL of deionized water to obtain a MXene solution, and then 2 mL of AgNO3 aqueous solution (4 mg / mL) was added to the MXene solution, and ultrasonic treatment was performed for 12 min at a power of 35 W, and then centrifuged for 15 min at a speed of 12000 r / min, and the centrifugation was repeated 3 times to obtain a centrifugal precipitate, which was added to deionized water, and then ultrasonic treatment was performed for 60 s at a power of 35 W, and finally freeze-dried at a temperature of -60 ° C for 12 h to obtain Ag@MXene;
[0053] The mass ratio of the centrifugal precipitate to the volume of deionized water is 1 mg:4 mL;
[0054] 2. Preparation of MxP / Ag@MxPC membrane:
[0055] ① Add 100 mg of Ag@MXene to 10 mL of dimethyl sulfoxide, ultrasonically treat for 1 min at a power of 35 W, then add 1.5 g of PVDF powder and 0.5 g of cellulose acetate powder, and finally heat and homogenize for 10 min under the conditions of sealing, temperature of 80 ° C and stirring speed of 60 r / min to obtain the bottom casting solution;
[0056] ② Add 100 mg of MXene nanosheets to 10 mL of dimethyl sulfoxide, ultrasonically treat for 1 min at a power of 35 W, then add 1.5 g of PVDF powder, and finally heat and homogenize for 10 min under the conditions of sealing, temperature of 80 ° C and stirring speed of 60 r / min to obtain the top layer casting solution;
[0057] ③ Coat the bottom casting solution and the top casting solution on the surface of the aluminum plate in turn, then cool it at -30°C for 30 seconds, immerse it in ice water at 0°C for 6 hours, take it out, vacuum dry it at room temperature and a vacuum degree of 2Pa for 12 hours, and remove the substrate to obtain the MxP / Ag@MxPC film.
[0058] The MXene nanosheets described in step 1 and step 2② are titanium carbide nanosheets with a size of 5 to 20 microns.
[0059] The coating thickness of the bottom casting solution described in step 2 (3) is 100 μm; the coating thickness of the top casting solution described in step 2 (3) is 50 μm.
[0060] Example 2: This example is different from Example 1 in that: Step 2① adds 200 mg of Ag@MXene to 10 mL of dimethyl sulfoxide; Step 2② adds 200 mg of MXene nanosheets to 10 mL of dimethyl sulfoxide. The rest is the same as Example 1.
[0061] Example 3: This example is different from Example 1 in that: Step 2① adds 300 mg of Ag@MXene to 10 mL of dimethyl sulfoxide; Step 2② adds 300 mg of MXene nanosheets to 10 mL of dimethyl sulfoxide. The rest is the same as Example 1.
[0062] Example 4: This example is different from Example 1 in that: Step 2① adds 400 mg of Ag@MXene to 10 mL of dimethyl sulfoxide; Step 2② adds 400 mg of MXene nanosheets to 10 mL of dimethyl sulfoxide. The rest is the same as Example 1.
[0063] Comparative Experiment 1: The difference between this comparative experiment and Example 1 is that: in step 2①, the addition of Ag@MXene is cancelled; in step 2②, the addition of MXene nanosheets is cancelled. The rest is the same as Example 1.
[0064] Comparative Experiment 2: This comparative experiment is different from Example 1 in that 1.5 grams of PVDF powder is added to 10 mL of dimethyl sulfoxide, and then heated and homogenized for 10 minutes under the conditions of sealing, temperature of 80°C and stirring speed of 60 r / min to obtain a PVDF polymer solution, 150 microns of the PVDF polymer solution is coated on the surface of the aluminum plate, and then cooled for 30 seconds at a temperature of -30°C, immersed in ice water at a temperature of 0°C for 6 hours after cooling, and finally taken out and vacuum dried for 12 hours at room temperature and a vacuum degree of 2 Pa to obtain a PVDF membrane (CCD). Others are the same as Example 1.
[0065] Comparative Experiment 3: This comparative experiment is different from Example 1 in that 1.5 g of PVDF powder is added to 10 mL of dimethyl sulfoxide, and then heated and homogenized for 10 min under the conditions of sealing, temperature of 80°C and stirring speed of 60 r / min to obtain a PVDF polymer solution, 150 microns of PVDF polymer solution is coated on the surface of the aluminum plate, and then immersed in ice water at a temperature of 0°C for 6 h, and finally taken out and vacuum dried for 12 h at room temperature and a vacuum degree of 2 Pa to obtain a PVDF membrane (NIPS), i.e., non-solvent induced phase separation method (NIPS). The rest is the same as Example 1.
[0066] Comparative Experiment 4: This comparative experiment is different from Example 1 in that 1.5 g of PVDF powder and 0.5 g of cellulose acetate powder are added to 10 mL of dimethyl sulfoxide, and then heated and homogenized for 10 min under the conditions of sealing, temperature of 80°C and stirring speed of 60 r / min to obtain a PVDF polymer solution, 150 μm of PVDF polymer solution is coated on the surface of the aluminum plate, and then cooled for 30 s at a temperature of -30°C, immersed in ice water at a temperature of 0°C for 6 h after cooling, and finally taken out and vacuum dried for 12 h at room temperature and vacuum degree of 2 Pa to obtain a PVDF / CA membrane (CCD). The rest is the same as Example 1.
[0067] The MxP / Ag@MxPC prepared in Examples 1 to 4 and Comparative Experiment 1 were named in sequence with x_MxP / y_Ag@MxPC, where x represents the content of MXene in the top casting solution, and y represents the content of Ag@MXene in the bottom casting solution. The product of Example 1 was named 1_MxP / 1_Ag@MxPC film, the product of Example 2 was named 2_MxP / 2_Ag@MxPC film, the product of Example 3 was named 3_MxP / 3_Ag@MxPC film, the product of Example 4 was named 4_MxP / 4_Ag@MxPC film, and the product of Comparative Experiment 1 was named 0_MxP / 0_Ag@MxPC film,
[0068] Figure 2 The morphology and element distribution of Ag@MXene prepared in step 1 of Example 1, a is a scanning electron microscope image of Ag@MXene, b is a HAADF-STEM image of Ag@MXene, and c is an elemental map. As can be seen from the figure, Ag@MXene presents a typical flake structure. And the silver nanoparticles are evenly distributed on the surface of MXene, and the particle size is approximately between 20 nanometers and 60 nanometers. It is confirmed that the silver nanoparticles are successfully attached to the MXene nanosheets, indicating the successful synthesis of Ag@MXene.
[0069] Figure 3 The SEM images of the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2, i is the overall cross-sectional view, ii is the enlarged cross-sectional view of the top layer, iii is the enlarged cross-sectional view of the bottom layer, iv is the surface view of the top layer, and v is the surface view of the bottom layer. As can be seen from the figure, there is a clear boundary between the top layer and the bottom layer. Compared with the bottom layer, the microporous structure of the top layer is looser, and there is a wide distribution of pores on the surfaces of the top layer and the bottom layer.
[0070] Figure 4 This is a diagram of the internal pore size distribution of the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2. As can be seen from the figure, the pore size range of 2_MxP / 2_Ag@MxPC is from 10 nanometers to 2 micrometers, and its peak pore size is about 200 nanometers.
[0071] Figure 5 Scanning electron microscope images of MXene embedded in the top layer and Ag@MXene embedded in the bottom layer in the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2, a is the top layer and b is the bottom layer. It can be seen from the figure that both MXene and Ag@MXene nanosheets are properly embedded in the polymer matrix.
[0072] Figure 6 The water vapor transmission rate of x_MxP / y_Ag@MxPC film is compared with the change of MXene content in the top layer and Ag@MXene content in the bottom layer. 0 is the 0_MxP / 0_Ag@MxPC film prepared in comparative experiment 1, 1 is the 1_MxP / 1_Ag@MxPC film prepared in Example 1, 2 is the 2_MxP / 2_Ag@MxP film C prepared in Example 2, 3 is the 3_MxP / 3_Ag@MxPC film prepared in Example 3, and 4 is the 4_MxP / 4_Ag@MxPC film prepared in Example 4. It can be seen from the figure that the water vapor transmission rate (WVTR) of 2_MxP / 2_Ag@MxPC is 6779.39 g / m 2 ·24h. Increasing the content of MXene-based fillers will lead to a significant decrease in WVTR, and the WVTR of 4_MxP / 4_Ag@MxPC film is reduced to 4761.13g / m 2 ·24 h, which is attributed to the reduced pore size and the layered structure of MXene and Ag@MXene hindering the passage of gas molecules.
[0073] Figure 7 : It is a comparison diagram of water contact angle test, i is the top surface of the PVDF membrane (NIPS) prepared in comparative experiment three, ii is the top surface of the PVDF membrane (CCD) prepared in comparative experiment two, ii is the top surface of the 1_MxP / 1_Ag@MxPC membrane prepared in Example one, iv is the bottom surface of the 1_MxP / 1_Ag@MxPC membrane prepared in Example one, v is the top surface of the 2_MxP / 2_Ag@MxPC membrane prepared in Example two, vi is the bottom surface of the 2_MxP / 2_Ag@MxPC membrane prepared in Example two, ⅶ is the top surface of the 3_MxP / 3_Ag@MxPC membrane prepared in Example three, and ⅷ is the bottom surface of the 3_MxP / 3_Ag@MxPC membrane prepared in Example three; Figure 8The water contact angle comparison diagram of the bottom surface of the PVDF membrane (CCD) prepared in the comparative experiment 2 and the bottom surface of the PVDF / CA membrane (CCD) in the comparative experiment 4; the preparation method of the PVDF membrane in the comparative experiment 3 is to immerse the polymer solution directly in water without the need for a low-temperature crystallization step. This method is called non-solvent induced phase separation (NIPS). The CCD method used in Examples 1 to 4 plays an important role in the microstructure of the top surface and has a great influence on the surface wettability. Without the addition of Mxene-based fillers, the single-layer PVDF membrane prepared by the NIPS method in the comparative experiment 3 has a relatively smooth top surface, while the single-layer PVDF membrane prepared by the CCD method in the comparative experiment 2 has a micro-nano structure, and the water contact angles are 85.35° (NIPS method) and 151.53° (CCD method). The bottom surface of the membrane prepared by the CCD method in the comparative experiment 2 is relatively flat, so the water contact angle is 85.64°. In order to further improve the hydrophilicity, the comparative experiment 4 adds hydrophilic cellulose acetate to the bottom surface to reduce the water contact angle to 73.21°. Similarly, due to the hydrophilicity of MXene-based fillers, the water contact angle also decreases with the increase of its content. In 2_MxP / 2_Ag@MxPC, the contact angles of the top and bottom surfaces decrease to 142.65° and 69.27°, respectively; in 3_MxP / 3_Ag@MxPC, the contact angles of the top and bottom surfaces decrease to 125.47° and 62.31°, respectively.
[0074] The 2_MxP / 2_Ag@MxPC membrane prepared in Example 2 was used to assemble the TENG, as follows: the 2_MxP / 2_Ag@MxPC membrane and the conductive silver fiber were integrated into a conductor using a porous conductive tape. When the conductive silver fiber was connected to the ground through an external resistor, the 2_MxP / 2_Ag@MxPC-based TENG would work in a single-electrode mode, and the electrical output came from the combined effects of contact charging and electrostatic induction. Fig. 9 For the performance test of TENG prepared by using the 2_MxP / 2_Ag@MxPC film of Example 2, i, ii and ii are the response characteristics of voltage, current and charge to frequency, and iv is the relationship between voltage output and power density and resistive load at a frequency of 4Hz; the output performance of TENG prepared by using the 2_MxP / 2_Ag@MxPC film of Example 2 is affected by the contact frequency. Specifically, when the contact frequency changes from 1Hz to 4Hz, the voltage output increases significantly from 850V to 1236V, the current output increases from 20μA to 70μA, and the charge output increases from about 122nC to 203n. This phenomenon can be attributed to the momentum enhancement at higher frequencies, which causes the deformation of the triboelectric layer. This deformation may expand the effective contact area of the triboelectric material, thereby improving the output performance. Fig. 9Figure iv shows the output performance of TENG at 4 Hz using various external load resistances. The voltage output increases with the increase of load resistance, while the energy density increases first and then decreases, reaching a peak of about 29 W / m at 8 MΩ load. 2 .
[0075] The bactericidal efficiency of MxP / Ag@MxPC membranes was studied over time to further explore their antibacterial activity. Fig.10 The antibacterial and biocompatibility tests of the 2_MxP / 2_Ag@MxPC membrane prepared in Example 2, i is the colony diagram of Escherichia coli and Staphylococcus aureus retained on the agar plate after being treated with the 2_MxP / 2_Ag@MxPC membrane, ii is the bactericidal efficiency of the 2_MxP / 2_Ag@MxPC membrane at different times, iii is the biocompatibility diagram of the 2_MxP / 2_Ag@MxPC membrane; Fig.10 Figures i and ii show that the number of E. coli and Staphylococcus aureus colonies remaining on the agar plate decreased dramatically over time, and by the 8th hour, both bacteria could not be detected, and the bacterial activity was about 0%. In addition, after the 2_MxP / 2_Ag@MxPC membrane was attached to the back skin of mice for 24 hours, it was found that the skin was still healthy, indicating that the MxP / Ag@MxPC membrane has high biocompatibility and safety ( Fig.10 (iii).
[0076] The 2_MxP / 2_Ag@MxPC membrane prepared in Example 2 was used to assemble TENG, specifically as follows: the MxP / Ag@MxPC membrane and conductive silver fibers were integrated into a conductor using a porous conductive tape, which was then fixed to the human joints using medical tape so that its bottom layer was in contact with human skin to generate electrical signals. Fig.11 Figure 2 is a detection diagram of TENG prepared by using 2_MxP / 2_Ag@MxPC film in human body motion, i is the response voltage signal diagram of TENG to finger tapping, fist hammering and palm slapping, ii is the voltage signal diagram of TENG when the finger is bent at 30°, 45°, 60° and 90°, iii is the response voltage signal diagram of TENG to wrist bending, iv is the response voltage signal of TENG to elbow bending; Fig.11 As shown in Figure 1, the sensor is extremely sensitive to hand movements and can distinguish between finger taps (about 200V), fist hammers (about 250V), and palm slaps (about 600V) through different voltage amplitudes. It is worth noting that palm slaps can generate voltages as high as 600V, reflecting the sensor's excellent electrical responsiveness. In addition, the electrical signal increases with the increase in the finger bending angle (from about 25V to about 80V), demonstrating the sensor's ability to dynamically track movement ( Fig.11ii). The MxP / Ag@MxPC film can also distinguish between full bending and half bending of the wrist and elbow joints based on signal changes. The maximum output voltage of the half-bending wrist joint is about 75V, and the voltage of the full bending is about 125V. Since the elbow joint has a larger range of motion, its voltage output is higher than that of the wrist joint. Its half-bending output voltage is about 100V, and the voltage of the full bending is about 250V. This improves its practicality in monitoring applications ( Fig.11 iii and iv). Therefore, the MxP / Ag@MxPC membrane has great value in daily health and sports tracking.
[0077] In order to directly apply the MxP / Ag@MxPC film as a self-powered biosensor to detect motion signals in the human body, its stretchability was evaluated by uniaxial tensile test. Fig.12 The uniaxial tensile stress-strain behavior of the 2_MxP / 2_Ag@MxPC film prepared in Example 2; as shown in the figure, the tensile stress is about 0.85MPa, and the strain at the maximum load is about 35.8%. Considering that the maximum elongation of human arm skin is about 27%, the MxP / Ag@MxPC film can meet the requirements of practical applications.
Claims
1. A method for preparing a triboelectric nanogenerator enhanced by a combined crystal diffusion method, characterized in that It is carried out in the following steps:
1. Synthesis of Ag@MXene: The MXene nanosheets are uniformly dispersed in deionized water to obtain a MXene solution, and then an AgNO3 aqueous solution is added to the MXene solution and ultrasonically treated, and finally centrifuged, ultrasonically dispersed in deionized water, and freeze-dried in sequence to obtain Ag@MXene; 2. Preparation of MxP / Ag@MxPC membrane: ① Add Ag@MXene to dimethyl sulfoxide for ultrasonic dispersion, then add PVDF powder and cellulose acetate powder, and finally heat and homogenize under sealed conditions to obtain the bottom casting solution; ② Add MXene nanosheets to dimethyl sulfoxide for ultrasonic dispersion, then add PVDF powder, and finally heat and homogenize under sealed conditions to obtain the top layer casting solution; ③ Coat the bottom casting solution and the top casting solution on the surface of the substrate in sequence, then cool for 30s to 60s at a temperature of -20℃ to -40℃, immerse in ice water at a temperature of 0℃ to 4℃ for 4h to 12h after cooling, finally take out, vacuum dry and remove the substrate to obtain the MxP / Ag@MxPC film.
2. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The mass ratio of the MXene nanosheets described in step one to the volume ratio of deionized water is 1 mg: (1 to 5) mL; the concentration of the AgNO3 aqueous solution described in step one is 1 mg / mL to 4 mg / mL; the volume ratio of the MXene solution described in step one to the AgNO3 aqueous solution is (8 to 12):
1.
3. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The ultrasonic treatment described in step 1 is specifically carried out at a power of 20w to 180w for 5min to 15min.
4. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The centrifugation described in step 1 is specifically carried out at a rotation speed of 8000 r / min to 12000 r / min for 10 min to 30 min, and the centrifugation is repeated 3 to 5 times to obtain a centrifugal precipitate.
5. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 4, characterized in that The ultrasonic dispersion in deionized water and freeze drying described in step 1 are specifically carried out according to the following steps: adding the centrifugal precipitate to deionized water, then ultrasonically treating it for 30s to 60s at a power of 20w to 180w, and finally freeze drying it for 12h to 24h at a temperature of -60°C; the mass ratio of the centrifugal precipitate to the volume of deionized water is 1mg:(1~4)mL.
6. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The MXene nanosheets described in step 1 and step 2② are titanium carbide nanosheets with a size of 5 μm to 20 μm.
7. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The mass ratio of the Ag@MXene described in step 2① to the volume ratio of dimethyl sulfoxide is (1-50) mg:1 mL; the mass ratio of the Ag@MXene described in step 2① to the PVDF powder is 1:(10-20); the mass ratio of the Ag@MXene described in step 2① to the cellulose acetate powder is (0.2-1):
1.
8. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The mass ratio of the MXene nanosheets described in step 2② to the volume ratio of dimethyl sulfoxide is (8-50) mg:1 mL; the mass ratio of the MXene nanosheets described in step 2① to the PVDF powder is 1:(3-15).
9. The method for preparing a triboelectric nanogenerator enhanced by a combined crystal diffusion method according to claim 1, characterized in that The ultrasonic dispersion described in step 2① and ② is specifically carried out under the condition of 20w~180w power and ultrasonic treatment for 30s~60s; the heating homogenization under sealed conditions described in step 2① and ② is specifically carried out under the conditions of sealing, temperature of 60℃~80℃ and stirring speed of 50r / min~120r / min, and heating homogenization treatment is carried out for 10min~20min.
10. The method for preparing a triboelectric nanogenerator enhanced by a combined crystallization diffusion method according to claim 1, characterized in that The substrate described in step 2③ is an aluminum plate; the coating thickness of the bottom casting solution described in step 2③ is 50μm~100μm; the coating thickness of the top casting solution described in step 2③ is 50μm~100μm; the vacuum drying described in step 2③ is specifically vacuum drying for 12h~24h under the condition of vacuum degree of 2Pa~1kPa.