One-component high temperature resistant water repellent polyurethane potting glue and preparation method thereof
By designing the molecular structure of single-component polyurethane potting glue and introducing temperature resistance and hydrophobic groups, the problems of insufficient temperature resistance, weather resistance and water repellency of polyurethane potting glue are solved, the production process is simplified and the cost is reduced. , and improves environmental friendliness and is suitable for industrial production.
Patent Information
- Application Number
- CN202410970762.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing polyurethane potting adhesives have deficiencies in temperature resistance, weather resistance and water repellency, and the production process is complex and costly. They also contain additives that are difficult to degrade, affecting environmental friendliness.
Using a single-component preparation method, using raw materials such as silicone-modified castor oil polyols, fluorine-containing modified polyols, chain extenders and catalysts, through chemical polymerization and thiol-ene click reactions, the molecular structure is designed and temperature resistance is introduced and hydrophobic groups, simplifying the production process and reducing dependence on external additives.
It significantly improves the temperature resistance, weather resistance and water repellency of the potting glue, simplifies the production process, reduces costs, enhances environmental friendliness, improves the stability and service life of the product, and is suitable for industrial mass production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane adhesives, and in particular relates to a single-component high-temperature resistant and water-repellent polyurethane potting adhesive and a preparation method thereof. Background Art
[0002] There are three main types of potting glue available on the market: epoxy resin potting glue, polyurethane potting glue and silicone potting glue. Among them, epoxy resin potting glue has good light transmittance, but its toughness and yellowing resistance are poor. The hardness of silicone potting glue can be adjusted after curing, and it has excellent temperature resistance, but the adhesion of silicone resin potting glue is poor and the cost is high. Polyurethane potting glue has many advantages such as a wide hardness range, easy availability of raw materials, good bonding performance, and strong resistance to water vapor penetration, but it has poor weather resistance.
[0003] Traditional polyurethane potting glue mostly achieves the temperature resistance of the material by adding thermal conductive fillers. For example, Chinese patent CN116376505A discloses a high thermal conductivity delayed curing two-component polyurethane potting glue, which uses modified thermal conductive powder and performs surface modification on it to enhance the wettability of the powder to the resin and improve the thermal conductivity efficiency; Chinese patent CN116376502A discloses a silicone resin modified polyurethane potting glue and its preparation method, which uses thermal conductive fillers and silicone resin to improve the thermal conductivity of the material. However, its stability is poor and there is a risk of thermal conductive powder precipitation. Chinese patent CN117343276A discloses a method for preparing a flame-retardant two-component polyurethane potting adhesive. Component A is prepared using polypropylene oxide glycol, polypropylene oxide glycol, and toluene diisocyanate as raw materials, and component B is prepared using castor oil, cardanol-containing silicon-containing bis(bisphenol A) phosphate chain extender, and dibutyltin dilaurate as raw materials. The prepared two-component polyurethane potting adhesive has excellent flame retardant properties, mechanical properties, and heat resistance, but the preparation process of its chain extender is cumbersome and not suitable for industrial production. Summary of the invention
[0004] In view of the shortcomings of the prior art, the object of the present invention is to provide a one-component high temperature resistant and water repellent polyurethane potting glue, which not only significantly improves the temperature resistance, weather resistance and water repellency of the potting glue through molecular structure design, but also simplifies the production process, reduces costs, enhances environmental friendliness, and has broad application prospects;
[0005] Another object of the present invention is to provide a method for preparing a one-component high temperature resistant and water repellent polyurethane potting adhesive, which has a simple process and is easy to mass produce.
[0006] The technical solution adopted by the present invention is as follows:
[0007] The one-component high temperature resistant and water repellent polyurethane potting glue is composed of the following raw materials in parts by mass:
[0008] Silicone modified castor oil polyol: 50-70 parts;
[0009] Fluorine-modified polyol: 30-50 parts;
[0010] Chain extender: 5~7 parts;
[0011] Isocyanate: 8-12 parts;
[0012] Catalyst: 0.2~0.7 parts;
[0013] Silane coupling agent: 1~2 parts;
[0014] The silicone-modified castor oil polyol uses castor oil as an initiator and propylene oxide and octamethylcyclotetrasiloxane as polymerization monomers;
[0015] The fluorine-containing modified polyol is prepared by using a terminal hydroxyl prepolymer containing a mercapto group and a benzene ring structure and a fluorine-containing acrylate as raw materials through a mercapto-ene click reaction under the action of an initiator;
[0016] The molecular structure of the chain extender contains a benzene ring structure.
[0017] The number average molecular weight of the siloxane-modified castor oil polyol is 2700-8100, and the average hydroxyl functionality is 2.7; the preparation method of the siloxane-modified castor oil polyol is: castor oil is used as an initiator, and under the catalytic action of a phosphazene catalyst or phosphotungstic acid, catalyzes propylene oxide and octamethylcyclotetrasiloxane to carry out a ring-opening polymerization reaction to prepare the siloxane-modified castor oil polyol, wherein the amount of octamethylcyclotetrasiloxane used is 15-23wt.% of the total amount of polymerization monomers.
[0018] The chain extender is NORYL SA90, which is a double-terminal hydroxyl-containing benzene ring structure, has a functionality of 2, and a number average molecular weight of 1600, and is purchased from Saudi Basic Industries (China) Investment Co., Ltd.
[0019] The isocyanate is toluene diisocyanate or diphenylmethane diisocyanate.
[0020] The catalyst is bismorpholinyl diethyl ether.
[0021] The silane coupling agent is ALINK-25 or ALINK-35, purchased from Momentive Silicone Materials (Shanghai) Co., Ltd.
[0022] The preparation method of the fluorine-containing modified polyol is:
[0023] 1) Add polyether polyol and dithiol with a number average molecular weight of 3000-6000 and a functionality of 3-6 into a reaction kettle, vacuum dehydrate at 98-102°C until the moisture content is less than 500ppm, then cool to 78-82°C, add toluene diisocyanate or diphenylmethane diisocyanate to carry out polymerization reaction, the reaction time is 2-3h, until the -NCO% content is 0, and obtain a hydroxyl-terminated prepolymer;
[0024] 2) Add N,N-dimethylformamide to the hydroxyl-terminated prepolymer, then add fluorinated acrylate and initiator, irradiate at room temperature and UV light for 5-6 hours to carry out mercapto-ene click reaction to introduce fluorine structure, remove N,N-dimethylformamide in vacuum after the reaction is completed, and obtain fluorinated modified polyol; wherein the UV light irradiance is 25mW / cm 2 .
[0025] In the step 1), the molar ratio of dithiol to toluene diisocyanate or diphenylmethane diisocyanate is (0.9-1.1):1; in the step 2), the amount of N,N-dimethylformamide added is 10-20wt.% of the total amount of the terminal hydroxyl prepolymer.
[0026] The dithiol is 4,4'-thiobisthiophenol or biphenyl-4,4'-dithiol, and the molar ratio of the dithiol to the polyether polyol is (0.9-4.1):1.
[0027] The fluorine-containing acrylate is one of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluorobutyl acrylate or octafluoropentyl acrylate, preferably octafluoropentyl acrylate; the molar ratio of dithiol to fluorine-containing acrylate is 1:(0.9~1).
[0028] The initiator is benzoin dimethyl ether, and the amount of the initiator is 0.2-0.3wt.% of the total amount of the terminal hydroxyl prepolymer and the fluorine-containing acrylate.
[0029] The preparation method of the one-component high temperature resistant and water repellent polyurethane potting glue comprises the following steps:
[0030] Add siloxane-modified castor oil polyol, fluorine-modified polyol and chain extender into the reaction kettle, dehydrate at 98-102°C for 2-3h, cool to 78-82°C, add isocyanate, react until -NCO% is 1-1.5wt.%, cool to below 60°C, add catalyst and silane coupling agent, stir evenly, seal with nitrogen, and obtain a one-component high temperature resistant and water-repellent polyurethane potting adhesive.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention directly introduces groups with good heat resistance and weather resistance (such as siloxane segments, benzene rings, etc.) and hydrophobic groups (such as fluorine-containing groups, siloxane segments, etc.) into the molecular structure of the raw materials by chemical polymerization, which gives the potting compound inherent heat resistance and water repellency. There is no need to add a large amount of flame retardants or waterproofing agents, which reduces the compatibility problems and precipitation risks that may be caused by additives, and improves the stability and service life of the product. By selecting a diol containing a benzene ring as a chain extender, the content of soft and hard segments in the potting compound is adjusted, which can not only increase the hardness of the potting compound, but also further improve its temperature resistance.
[0033] (2) The present invention reduces dependence on external additives and reduces raw material costs by optimizing the molecular structure design. At the same time, the simplified production process also improves production efficiency and further reduces overall costs. In addition, since the potting glue itself has stable performance and does not contain a large amount of difficult-to-degrade additives, it is green and environmentally friendly and can reduce the pressure of waste on the environment.
[0034] (3) The preparation method of the present invention adopts mild and safe reaction conditions (normal pressure, low temperature <100°C). Compared with the complicated preparation process in the traditional method, it greatly simplifies the production process, reduces energy consumption and safety hazards, and is more suitable for industrial large-scale production. DETAILED DESCRIPTION
[0035] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.
[0036] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.
[0037] Some of the raw materials used in the examples and comparative examples are described as follows:
[0038] Phosphazene catalyst was purchased from Shanghai Qike Fluorosilicon Materials Co., Ltd.;
[0039] Polyether polyol INOVOL C3050A (number average molecular weight of 3000, functionality of 3) was purchased from Shandong INOVOL New Materials Co., Ltd.;
[0040] Polyether polyol INOVOL C216 (functionality 2, number average molecular weight 1600) was purchased from Shandong INOVOL New Materials Co., Ltd.
[0041] Example 1
[0042] The one-component high temperature resistant and water repellent polyurethane potting glue is composed of the following raw materials in parts by mass:
[0043] Silicone modified castor oil polyol: 50 parts;
[0044] Fluorine-modified polyol: 50 parts;
[0045] NORYL SA90: 5 parts;
[0046] Diphenylmethane diisocyanate: 12 parts;
[0047] Bismorpholinyl diethyl ether: 0.7 parts;
[0048] ALINK-25: 2 copies.
[0049] The number average molecular weight of the siloxane-modified castor oil polyol is 2700, and the average functionality of the hydroxyl group is 2.7. The preparation method of the siloxane-modified castor oil polyol is as follows: 1000g of castor oil with a number average molecular weight of 1000 is taken as an initiator, 1.8g of a phosphazene catalyst is added, 300g of octamethylcyclotetrasiloxane and 1700g of propylene oxide are catalyzed to carry out a ring-opening polymerization reaction, and the siloxane-modified castor oil polyol is obtained after acid neutralization, adsorption, drying, and filtering to remove the catalyst.
[0050] The preparation method of the fluorine-containing modified polyol is:
[0051] 1) 6000g of a polyether polyol having a number average molecular weight of 6000 and a functionality of 6 (prepared by ring-opening polymerization of 6484g of propylene oxide using 182g of sorbitol as an initiator and 20g of potassium hydroxide as a catalyst, followed by neutralization, adsorption, drying and filtration to remove the catalyst) and 1020g of 4,4'-thiobisthiophenol were added to a reactor, vacuum-dehydrated to a moisture content of 258ppm at 100±2°C, then cooled to 82°C, and 1000g of diphenylmethane diisocyanate was added to carry out polymerization reaction for 3h until the -NCO% content was 0, thereby obtaining a hydroxyl-terminated prepolymer;
[0052] 2) Add 802g of N,N-dimethylformamide to the hydroxyl-terminated prepolymer, then add 1168g of octafluoropentyl acrylate and 27.56g of benzoin dimethyl ether, and irradiate for 6h at room temperature and UV irradiation to carry out mercapto-ene click reaction. After the reaction is completed, remove N,N-dimethylformamide in vacuum to obtain fluorine-modified polyol; wherein the UV irradiance is 25mW / cm 2 .
[0053] The preparation method of the one-component high temperature resistant and water repellent polyurethane potting glue comprises the following steps:
[0054] Add siloxane-modified castor oil polyol, fluorine-modified polyol and NORYL SA90 into the reactor, vacuum dehydrate at 100±2°C for 2h, cool to 80±2°C, add diphenylmethane diisocyanate, react until -NCO% is 1.04wt.%, cool to 40°C, add bismorpholinyl diethyl ether and ALINK-25, stir evenly, seal with nitrogen, and obtain a one-component high temperature resistant and water-repellent polyurethane potting adhesive.
[0055] Example 2
[0056] The one-component high temperature resistant and water repellent polyurethane potting glue is composed of the following raw materials in parts by mass:
[0057] Silicone modified castor oil polyol: 60 parts;
[0058] Fluorine-modified polyol: 40 parts;
[0059] NORYL SA90: 7 parts;
[0060] Toluene diisocyanate: 8 parts;
[0061] Bismorpholinyl diethyl ether: 0.6 parts;
[0062] ALINK-25: 1.5 parts.
[0063] The number average molecular weight of the siloxane-modified castor oil polyol is 5400, and the average hydroxyl functionality is 2.7; the preparation method of the siloxane-modified castor oil polyol is: take 1000g of castor oil with a number average molecular weight of 1000 as an initiator, add 2.7g of phosphotungstic acid, catalyze 900g of octamethylcyclotetrasiloxane and 4100g of propylene oxide to carry out a ring-opening polymerization reaction, and obtain the siloxane-modified castor oil polyol.
[0064] The preparation method of the fluorine-containing modified polyol is:
[0065] 1) Add 5000g of a polyether polyol having a number average molecular weight of 5000 and a functionality of 5 (prepared by using 152g of xylitol as an initiator and 14g of potassium hydroxide as a catalyst to catalyze 5400g of propylene oxide for ring-opening polymerization, and then neutralize, adsorb, dry and filter to remove the catalyst) and 750g of 4,4'-thiobisthiophenol into a reactor, vacuum dehydrate to a moisture content of 260ppm at 100±2°C, then cool to 78°C, add 522g of toluene diisocyanate to carry out polymerization reaction, and react for 2h until the -NCO% content is 0 to obtain a hydroxyl-terminated prepolymer;
[0066] 2) Add 940g of N,N-dimethylformamide to the hydroxyl-terminated prepolymer, then add 858g of octafluoropentyl acrylate and 17.4g of benzoin dimethyl ether, and irradiate for 5h at room temperature and UV irradiation to carry out mercapto-ene click reaction. After the reaction is completed, remove N,N-dimethylformamide in vacuum to obtain fluorine-modified polyol; wherein the UV irradiance is 25mW / cm 2 .
[0067] The preparation method of the one-component high temperature resistant and water repellent polyurethane potting glue comprises the following steps:
[0068] Add siloxane-modified castor oil polyol, fluorine-modified polyol and NORYL SA90 into the reactor, vacuum dehydrate at 100±2°C for 2h, cool to 80±2°C, add toluene diisocyanate, react until -NCO% reaches 1.5wt.%, cool to 30°C, add bismorpholinyl diethyl ether and ALINK-25, stir evenly, seal with nitrogen, and obtain a one-component high-temperature resistant and water-repellent polyurethane potting adhesive.
[0069] Example 3
[0070] The one-component high temperature resistant and water repellent polyurethane potting glue is composed of the following raw materials in parts by mass:
[0071] Silicone modified castor oil polyol: 70 parts;
[0072] Fluorine-modified polyol: 30 parts;
[0073] NORYL SA90: 6 parts;
[0074] Diphenylmethane diisocyanate: 10 parts;
[0075] Bismorpholinyl diethyl ether: 0.2 parts;
[0076] ALINK-35: 2 copies.
[0077] The number average molecular weight of the siloxane-modified castor oil polyol is 8100, and the average functionality of the hydroxyl group is 2.7. The preparation method of the siloxane-modified castor oil polyol is as follows: 1000g of castor oil with a number average molecular weight of 1000 is taken as an initiator, 7.2g of a phosphazene catalyst is added, 1800g of octamethylcyclotetrasiloxane and 6200g of propylene oxide are catalyzed to carry out a ring-opening polymerization reaction, and the siloxane-modified castor oil polyol is obtained after acid neutralization, adsorption, drying, and filtering to remove the catalyst.
[0078] The preparation method of the fluorine-containing modified polyol is:
[0079] 1) Add 3000g of INOVOL C3050A and 218g of biphenyl-4,4'-dithiol into a reactor, vacuum dehydrate to a moisture content of 200ppm at 100±2℃, then cool to 80℃, add 250g of diphenylmethane diisocyanate to carry out polymerization reaction for 2h until the -NCO% content is 0, and obtain a hydroxyl-terminated prepolymer;
[0080] 2) Add 693g of N,N-dimethylformamide to the hydroxyl-terminated prepolymer, then add 236g of hexafluorobutyl acrylate and 7.4g of benzoin dimethyl ether, and irradiate for 5h at room temperature and UV irradiation to carry out mercapto-ene click reaction to introduce fluorine structure. After the reaction is completed, remove N,N-dimethylformamide in vacuum to obtain fluorine-containing modified polyol; wherein the UV irradiance is 25mW / cm 2 .
[0081] The preparation method of the one-component high temperature resistant and water repellent polyurethane potting glue comprises the following steps:
[0082] Add siloxane-modified castor oil polyol, fluorine-modified polyol and NORYL SA90 into the reactor, vacuum dehydrate at 100±2°C for 2h, cool to 80±2°C, add diphenylmethane diisocyanate, react until -NCO% is 1.19wt.%, cool to 35°C, add bismorpholinyl diethyl ether and ALINK-35, stir evenly, seal with nitrogen, and obtain a one-component high temperature resistant and water-repellent polyurethane potting adhesive.
[0083] Comparative Example 1
[0084] The difference from Example 1 is that the octamethylcyclotetrasiloxane in the siloxane-modified castor oil polyol is replaced with propylene oxide to obtain a modified castor oil polyol without siloxane segments, with a number average molecular weight of 2700 and an average hydroxyl functionality of 2.7. The rest is the same as Example 1.
[0085] Comparative Example 2
[0086] The difference from Example 1 is that in the preparation process of the fluorine-containing modified polyol, n-pentyl acrylate is used instead of octafluoropentyl acrylate to prepare the fluorine-free modified polyol, and the rest is the same as Example 1.
[0087] Comparative Example 3
[0088] The difference from Example 1 is that INOVOL C216 is used to replace the chain extender in Example 1, and the rest is the same as Example 1.
[0089] Comparative Example 4
[0090] The difference from Example 1 is that in the preparation process of the fluorine-containing modified polyol, 1,16-hexadecanethiol is used to replace 4,4'-thiobisthiophenol to obtain a modified polyol without a benzene ring. The rest is the same as Example 1.
[0091] Comparative Example 5
[0092] The difference from Example 1 is:
[0093] The octamethylcyclotetrasiloxane in the siloxane-modified castor oil polyol was replaced with propylene oxide to obtain a modified castor oil polyol without a siloxane segment having a number average molecular weight of 2700 and an average hydroxyl functionality of 2.7;
[0094] A propylene glycol initiator polyether polyol (propylene glycol is used as an initiator to catalyze the polymerization of propylene oxide, and the catalyst is DMC) with a functionality of 2 and a number average molecular weight of 9188 is used to replace the fluorine-containing modified polyol in Example 1;
[0095] INOVOL C216 was used to replace the chain extender in Example 1;
[0096] The rest is the same as in Example 1.
[0097] The performance tests were performed on the MS glues prepared in Examples 1 to 3 and Comparative Examples 1 to 5, respectively, and the test methods were as follows:
[0098] Refer to GB / T531.1-2008 to test the hardness (Shore A);
[0099] Refer to GB / T19250-2013 and test the water absorption rate (%) after 30 days;
[0100] Refer to GB / T42694-2023 to test the rolling angle (°);
[0101] Refer to GB / T30693-2014 to test the water contact angle (°);
[0102] The onset thermal decomposition temperature (°C) was tested using a differential scanning calorimeter;
[0103] The test results are shown in Table 1.
[0104] Table 1 Performance test results
[0105]
[0106] From the test data in Table 1, it can be seen that the introduction of low surface energy fluorine and siloxane into the molecular structure of the potting compound can significantly improve the water repellency and temperature resistance of the material. In addition, the introduction of the benzene ring structure can improve the hardness and temperature resistance of the material to a certain extent. The improvement of the above properties can greatly enrich the application scenarios of the potting compound in outdoor or harsh environmental conditions.
Claims
1. A one-component high temperature resistant and water repellent polyurethane potting adhesive, characterized in that: It is composed of the following raw materials in parts by weight: Silicone modified castor oil polyol: 50-70 parts; Fluorine-modified polyol: 30-50 parts; Chain extender: 5~7 parts; Isocyanate: 8-12 parts; Catalyst: 0.2~0.7 parts; Silane coupling agent: 1~2 parts; The silicone-modified castor oil polyol uses castor oil as an initiator and propylene oxide and octamethylcyclotetrasiloxane as polymerization monomers; The preparation method of the fluorine-containing modified polyol is: 1) Add polyether polyol and dithiol with a number average molecular weight of 3000-6000 and a functionality of 3-6 into a reaction kettle, vacuum dehydrate until the moisture content is less than 500ppm, then cool to 78-82°C, add toluene diisocyanate or diphenylmethane diisocyanate to carry out polymerization reaction until the -NCO% content is 0, and obtain a hydroxyl-terminated prepolymer; 2) Add N,N-dimethylformamide to the hydroxyl-terminated prepolymer, then add fluorinated acrylate and initiator, and carry out mercapto-ene click reaction at room temperature and under ultraviolet irradiation conditions. After the reaction, remove N,N-dimethylformamide in vacuum to obtain fluorinated modified polyol; The dithiol is 4,4'-thiobisthiophenol or biphenyl-4,4'-dithiol; The chain extender is NORYL SA90.
2. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: The number average molecular weight of the siloxane-modified castor oil polyol is 2700-8100, and the average hydroxyl functionality is 2.7; the preparation method of the siloxane-modified castor oil polyol is: castor oil is used as an initiator, and under the catalytic action of a phosphazene catalyst or phosphotungstic acid, catalyzes propylene oxide and octamethylcyclotetrasiloxane to carry out a ring-opening polymerization reaction to prepare the siloxane-modified castor oil polyol, wherein the amount of octamethylcyclotetrasiloxane used is 15-23wt.% of the total amount of polymerization monomers.
3. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: The isocyanate is toluene diisocyanate or diphenylmethane diisocyanate.
4. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: The catalyst is bismorpholinyl diethyl ether; and the silane coupling agent is ALINK-25 or ALINK-35.
5. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: In the step 1), the molar ratio of dithiol to toluene diisocyanate or diphenylmethane diisocyanate is (0.9-1.1):1; in the step 2), the amount of N,N-dimethylformamide added is 10-20wt.% of the total amount of the terminal hydroxyl prepolymer.
6. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: The molar ratio of the dithiol to the polyether polyol is (0.9-4.1):
1.
7. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: The fluorine-containing acrylate is one of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluorobutyl acrylate or octafluoropentyl acrylate, and the molar ratio of dithiol to fluorine-containing acrylate is 1:(0.9-1).
8. The one-component high temperature resistant and water repellent polyurethane potting adhesive according to claim 1, characterized in that: The initiator is benzoin dimethyl ether, and the amount of the initiator is 0.2-0.3wt.% of the total amount of the terminal hydroxyl prepolymer and the fluorine-containing acrylate.
9. A method for preparing the one-component high temperature resistant and water repellent polyurethane potting adhesive according to any one of claims 1 to 8, characterized in that: Here are the steps: Add siloxane-modified castor oil polyol, fluorine-modified polyol and chain extender into a reaction kettle, dehydrate, cool to 78-82°C, add isocyanate, react until -NCO% is 1-1.5wt.%, cool to below 60°C, add catalyst and silane coupling agent, stir evenly, and obtain a one-component high temperature resistant and water-repellent polyurethane potting adhesive.